Preparation method of magnetic powder glue
By forming a double-layer coating on the magnetic powder and adding solvent-free photosensitive adhesive, the problems of magnetic powder leveling and environmental pollution in the silk-printed magnetic ink are solved, achieving better three-dimensional effects and reducing manufacturing costs.
Patent Information
- Application Number
- CN202411140352.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing silk-print magnetic ink process, the magnetic powder leveling is caused by solvent volatility, the pattern has poor three-dimensional effect, high manufacturing cost, and serious environmental pollution.
The suspension is prepared using magnetic materials, silane coupling agents and solvents, and the double-coated magnetic properties are formed by precipitation of silver nitrate solution, washing with deionized water, polydimethyldiallyl ammonium chloride and sodium polystyrene sulfonate. Add powder to solvent-free photosensitive glue to improve the dispersion between the powder and glue and avoid leveling.
The high dispersion between magnetic powder and photosensitive adhesive is achieved, the three-dimensional effect is improved, the manufacturing cost is reduced, and environmental pollution is avoided.
Smart Images

Figure CN118995057A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of electronic equipment, and specifically relates to a method for preparing magnetic powder glue. Background Art
[0002] At present, with the rapid development of electronic devices, users have higher and higher requirements on the appearance of the housing of electronic devices, and housings with three-dimensional effects are gradually coming into the field of vision of users.
[0003] In the related art, the three-dimensional effect of the shell is generally achieved by silk-screening magnetic ink. However, in the process of silk-screening magnetic ink, since the magnetic ink system contains solvents, the shell needs to be baked to evaporate the solvent, which increases the manufacturing cost. At the same time, during the evaporation of the solvent, the magnetic powder will level, thereby weakening the three-dimensional effect of the pattern. Summary of the invention
[0004] The present application aims to provide a method for preparing magnetic powder glue, which at least solves the problem of poor three-dimensional effect of the pattern on the shell in the related art.
[0005] In order to solve the above technical problems, this application is implemented as follows:
[0006] The embodiment of the present application proposes a method for preparing a magnetic powder glue, including: preparing a suspension using a magnetic material, a silane coupling agent and a solvent; adding a first powder to the suspension, and adding a first dispersant to obtain a first solution, adding a silver nitrate solution to the first solution to obtain a first precipitate; washing the first precipitate with deionized water to obtain a second powder; adding the second powder to a polydimethyldiallylammonium chloride solution to obtain a second precipitate, and adding the second precipitate to a sodium polystyrene sulfonate solution to obtain a third precipitate; drying the third precipitate to obtain a magnetic powder; and adding the magnetic powder to a photosensitive glue to obtain a magnetic powder glue.
[0007] In an embodiment of the present application, the preparation method of magnetic powder glue includes: first using magnetic material, silane coupling agent and solvent to prepare suspension, then adding first powder to the suspension, adding first dispersant to obtain first solution, so that magnetic material and first powder fully react, then adding silver nitrate solution to the first melt, so that first precipitate gradually precipitates, then washing the first precipitate with deionized water, removing silver nitrate solution and other substances on the surface of the first precipitate, and then obtaining second powder. In the second powder, the magnetic material wraps the first powder to form a first layer of coating on the first powder. Then the second powder is added to the polydimethyldiallyl ammonium chloride solution, and a second precipitate is obtained after sufficient reaction. Then the second precipitate is added to the sodium polystyrene sulfonate solution to obtain a third precipitate, and then the third precipitate is dried to obtain magnetic powder. In the process of treating the second powder with the polydimethyldiallyl ammonium chloride solution and the sodium polystyrene sulfonate solution, the polydimethyldiallyl ammonium chloride and the sodium polystyrene sulfonate can form an ion complex, which is then wrapped around the outside of the second powder, so that the final magnetic powder has a double-layer wrapping. Then the magnetic powder is added to the photosensitive adhesive to obtain a magnetic powder adhesive, which improves the dispersibility between the magnetic powder and the photosensitive adhesive. At the same time, since the photosensitive adhesive is a solvent-free material, it can avoid the situation of material leveling, improve the three-dimensional effect, and also avoid pollution to the environment and reduce manufacturing costs.
[0008] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0010] Figure 1 is a structural diagram of magnetic powder according to an embodiment of the present application;
[0011] Figure 2 The schematic diagram of the structure of a single-station transfer printing machine is shown;
[0012] Figure 3 A schematic diagram of the material stacking structure at the loading station on a single-station transfer printing machine is shown;
[0013] Figure 4 The schematic diagram of the structure of the four-station transfer printing machine is shown;
[0014] Figure 5 A schematic diagram of the material stacking structure at the loading station on a four-station transfer machine is shown;
[0015] Figure 6A schematic structural diagram of a cover body according to an embodiment of the present application is shown;
[0016] Figure 7 A schematic structural diagram of a cover body according to another embodiment of the present application is shown.
[0017] Reference numerals:
[0018] 1 magnetic powder, 10 first powder, 12 first coating layer, 14 second coating layer, 2 magnetic powder glue, 3 machine table, 30 support table, 31 magnetic template, 32 curing lamp, 33 rubber roller, 34 texture template, 35 roller table, 36 loading table, 37 unloading table, 4 substrate, 5 coating layer, 6 ink layer, 7 paint layer. DETAILED DESCRIPTION
[0019] The embodiments of the present application will be described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be construed as limitations on the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0020] The term "first" or "second" in the specification and claims of this application may include one or more of the features explicitly or implicitly. In the description of this application, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the objects connected before and after are in an "or" relationship.
[0021] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0022] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0023] Combine the following Figure 1-Figure 7 The preparation method of magnetic powder glue according to an embodiment of the present application is described.
[0024] According to some embodiments of the present application, the preparation method of magnetic powder glue includes: preparing a suspension using a magnetic material, a silane coupling agent and a solvent; adding a first powder to the suspension, and adding a first dispersant to obtain a first solution, adding a silver nitrate solution to the first solution to obtain a first precipitate; washing the first precipitate with deionized water to obtain a second powder; adding the second powder to a polydimethyldiallylammonium chloride solution to obtain a second precipitate, and adding the second precipitate to a sodium polystyrene sulfonate solution to obtain a third precipitate; drying the third precipitate to obtain a magnetic powder; adding the magnetic powder to a photosensitive glue to obtain a magnetic powder glue.
[0025] In an embodiment of the present application, a method for preparing a magnetic powder glue includes: first preparing a suspension using a magnetic material, a silane coupling agent and a solvent, then adding a first powder to the suspension, and then adding a first dispersant to obtain a first solution, so that the magnetic material and the first powder fully react, and then adding a silver nitrate solution to the first melt to gradually precipitate a first precipitate, and then washing the first precipitate with deionized water to remove substances such as the silver nitrate solution on the surface of the first precipitate, thereby obtaining a second powder, in which the magnetic material wraps the first powder to form a first layer of coating on the first powder. Then the second powder is added to the polydimethyldiallyl ammonium chloride solution, and a second precipitate is obtained after sufficient reaction. Then the second precipitate is added to the sodium polystyrene sulfonate solution to obtain a third precipitate, and then the third precipitate is dried to obtain magnetic powder. In the process of treating the second powder with the polydimethyldiallyl ammonium chloride solution and the sodium polystyrene sulfonate solution, the polydimethyldiallyl ammonium chloride and the sodium polystyrene sulfonate can form an ion complex, which is then wrapped around the outside of the second powder, so that the final magnetic powder has a double-layer wrapping. Then the magnetic powder is added to the photosensitive adhesive to obtain a magnetic powder adhesive. Since the magnetic powder has a double-layer wrapping structure, the dispersibility between the magnetic powder and the photosensitive adhesive can be improved. At the same time, since the photosensitive adhesive is a solvent-free material, the material leveling can be avoided, the three-dimensional effect can be improved, and the pollution to the environment can be avoided and the manufacturing cost can be reduced.
[0026] Optionally, the first powder includes silver powder and / or pearl powder.
[0027] Optionally, the silver nitrate solution is slowly added to the first solution, so that the first precipitate is slowly precipitated.
[0028] Optionally, 0.1 M silver nitrate solution is slowly added to the first solution, so that the first precipitate is slowly precipitated.
[0029] Optionally, the third precipitate is placed in a vacuum drying oven for drying to prevent oxidation of the third precipitate and remove moisture, thereby obtaining magnetic powder.
[0030] According to some embodiments of the present application, optionally, after the step of adding the first powder to the suspension and adding the first dispersant, the step further includes: ultrasonically treating the suspension to which the first powder and the first dispersant are added; and / or adding dilute sodium hydroxide or dilute hydrochloric acid to the suspension to adjust the pH value of the first solution; wherein the pH value of the first solution is greater than or equal to 7 and less than or equal to 9.
[0031] In this embodiment, the first powder is added to the suspension, and the first dispersant is added, and then ultrasonic treatment is performed, so that the magnetic powder fully wraps the first powder, thereby improving the dispersion uniformity between the magnetic powder and the first powder and improving the wrapping of the first powder by the magnetic powder. Optionally, dilute sodium hydroxide or dilute hydrochloric acid is added to the suspension to adjust the pH value of the first solution so that the pH value of the first melt is between 7 and 9, thereby ensuring the stability of the suspension and improving the wrapping adequacy between the magnetic powder and the first powder.
[0032] Optionally, the power of the ultrasonic treatment is greater than or equal to 200W and less than or equal to 300W.
[0033] According to some embodiments of the present application, optionally, in the first solution, the weight of the first powder is 100 parts, the weight of the suspension is greater than or equal to 10 parts and less than or equal to 30 parts, and the weight of the first dispersant is greater than or equal to 1 part and less than or equal to 2 parts; the first dispersant includes: alkyl ammonium salt.
[0034] In this embodiment, in the first solution, the weight of the first powder is 100 parts, the weight of the suspension is greater than or equal to 10 parts and less than or equal to 30 parts, and the weight of the first dispersant is greater than or equal to 1 part and less than or equal to 2 parts. After a certain proportion of the first powder, the suspension and the first dispersant are mixed, it can be ensured that the magnetic powder fully wraps the first powder. The first dispersant includes an alkyl ammonium salt, which can effectively disperse the first powder, improve the dispersibility of the first powder, and thus improve the wrapping of the first powder by the magnetic material.
[0035] According to some embodiments of the present application, optionally, the weight ratio of the sum of the mass of the polydimethyldiallylammonium chloride solution and the sodium polystyrene sulfonate solution to the magnetic powder is greater than or equal to 0.1% and less than or equal to 1%.
[0036] In this embodiment, optionally, the weight ratio of the sum of the mass of the polydimethyldiallylammonium chloride solution and the sodium polystyrene sulfonate solution to the magnetic powder is greater than or equal to 0.1% and less than or equal to 1%, thereby improving the encapsulation of the first powder by both.
[0037] According to some embodiments of the present application, optionally, after the step of adding the second powder to a polydimethyldiallylammonium chloride solution to obtain a second precipitate, the method further includes: washing the second precipitate with deionized water to remove unabsorbed polydimethyldiallylammonium chloride; and after the step of adding the second precipitate to a sodium polystyrene sulfonate solution to obtain a third precipitate, the method further includes: washing the third precipitate with deionized water to remove unabsorbed sodium polystyrene sulfonate.
[0038] In this embodiment, after the step of adding the second powder to the polydimethyldiallyl ammonium chloride solution to obtain the second precipitate, the method further includes: washing the second precipitate with deionized water to remove the polydimethyldiallyl ammonium chloride that is not adsorbed on the second precipitate, and then adding the sodium polystyrene sulfonate solution so that the sodium polystyrene sulfonate fully covers the second precipitate. Optionally, after the step of adding the second precipitate to the sodium polystyrene sulfonate solution to obtain the third precipitate, the method further includes: washing the third precipitate with deionized water to clean off the sodium polystyrene sulfonate that is not adsorbed on the third precipitate.
[0039] According to some embodiments of the present application, optionally, in the suspension, the weight parts of the magnetic material are 50 parts, the weight parts of the silane coupling agent are 1 part, and the weight parts of the solvent are 100 parts; and / or the magnetic material includes a mixture of at least two of ferrite, neodymium iron boron and cobalt aluminum nickel; and / or the solvent includes at least one of ethanol and water.
[0040] In this embodiment, the magnetic material, the silane coupling agent and the solvent are mixed in a weight ratio of 50 parts to 1 part to 100 parts, so that the magnetic material is fully mixed in the solvent. Optionally, the magnetic material includes a mixture of at least two of ferrite, neodymium iron boron and cobalt aluminum nickel, so as to achieve the effect of silvery white and translucent magnetic powder, and avoid the problem of yellowing, blackening and obvious impurity points of the prepared powder. Optionally, the solvent includes at least one of ethanol and water, which is low in price and can effectively dissolve the magnetic material in the solvent.
[0041] According to some embodiments of the present application, optionally, the step of preparing a suspension using a magnetic material, a silane coupling agent and a solvent includes: mixing the magnetic material, the silane coupling agent and the solvent and stirring them at a first stirring rate for a first time to obtain a suspension.
[0042] In this embodiment, in the step of preparing the suspension, the mixed solution is stirred so that the magnetic material is dispersed in the solvent.
[0043] Optionally, the first stirring rate is greater than or equal to 1000 rpm and less than or equal to 1500 rpm; the first time length is greater than or equal to 15 min and less than or equal to 30 min.
[0044] According to some embodiments of the present application, optionally, the method for preparing magnetic powder glue further includes: stirring the polydimethyldiallylammonium chloride solution to which the second powder is added at a second stirring rate for a second time period.
[0045] In this embodiment, after the second powder is added to the polydimethyldiallylammonium chloride solution, stirring is performed at a second stirring rate for a second time period, so that the second powder is evenly distributed in the polydimethyldiallylammonium chloride solution, thereby improving the dispersibility of the second powder.
[0046] Optionally, the second speed is 1000rpm-1500rpm, the second duration is greater than or equal to 20min and less than or equal to 40min, and optionally, the second duration is 30min.
[0047] According to some embodiments of the present application, optionally, the step of adding magnetic powder to a photosensitive adhesive to obtain a magnetic powder adhesive includes: adding the magnetic powder to a photosensitive resin, and adding a second dispersant for pre-dispersion treatment to obtain a second solution; adding the second solution to the photosensitive adhesive and stirring to obtain a third solution; and degassing the third solution to obtain a magnetic powder adhesive.
[0048] In this embodiment, the preparation method of the magnetic powder glue includes adding the magnetic powder to the photosensitive resin, then adding the second dispersant for pre-dispersion treatment and obtaining the second solution, then adding the second solution to the photosensitive adhesive, stirring, and then obtaining the third solution. The pre-dispersion treatment step can make the dispersibility and compatibility between the magnetic powder and the photosensitive adhesive better, and the photosensitive adhesive can be quickly photocured, and the texture effect formed has a strong three-dimensional sense, which can achieve a richer design effect. In addition, the third solution is degassed to obtain the magnetic powder glue, which can eliminate the bubbles in the photosensitive adhesive and the microbubbles at the interface between the magnetic powder and the photosensitive adhesive, so that the texture formed after curing is clearer and more stable.
[0049] Optionally, during the degassing treatment, the pressure value of the degassing treatment is 0.3 MPa, and the degassing time is between 15 min and 30 min.
[0050] The second solution is added to the photosensitive adhesive and stirred so that the magnetic powder in the second solution is repeatedly dispersed in the photosensitive adhesive, thereby improving the compatibility and dispersibility between the magnetic powder and the photosensitive adhesive. Optionally, in this step, stirring is continued for 30 min-40 min, the stirring rate is 1000 rpm-1500 rpm, and the prepared third solution needs to be filtered using a 100-150 mesh filter.
[0051] According to some embodiments of the present application, optionally, the photosensitive resin includes one or more of the following compounds: functional acrylic monomers hexanediol diacrylate, tetramethylene acrylate, N-vinyl pyrrolidone, N,N-dimethylacrylamide; and / or the second dispersant includes: alkyl ammonium salt; and / or the weight ratio of the magnetic powder, the photosensitive resin and the second dispersant is 5 parts: 100 parts: 1 part.
[0052] In this embodiment, the photosensitive resin includes one or more of the following compounds: functional acrylic monomer hexanediol diacrylate, tetrahydrofuran acrylate, N-vinyl pyrrolidone, N,N-dimethylacrylamide. The magnetic powder is first added to the photosensitive resin, and a second dispersant is added to achieve pre-dispersion of the magnetic powder. The second dispersant includes: an alkyl ammonium salt, which can effectively disperse the magnetic powder and improve the dispersibility of the magnetic powder. The weight ratio of the magnetic powder, the photosensitive resin, and the second dispersant is 5 parts: 100 parts: 1 part, so that the magnetic powder and the photosensitive resin have good compatibility and dispersibility.
[0053] According to some embodiments of the present application, optionally, components of the third solution include a high-functional group resin, a toughening resin, a photosensitive resin, a photoinitiator, a second dispersant and a magnetic powder; wherein the weight of the high-functional group resin is greater than or equal to 40 parts and less than or equal to 50 parts, the weight of the toughening resin is greater than or equal to 20 parts and less than or equal to 30 parts, the weight of the photosensitive resin is greater than or equal to 20 parts and less than or equal to 30 parts, the weight of the photoinitiator is greater than or equal to 3 parts and less than or equal to 4 parts, the weight of the second dispersant is greater than or equal to 1 part and less than or equal to 3 parts, and the weight of the magnetic powder is greater than or equal to 1 part and less than or equal to 5 parts.
[0054] In this embodiment, the components of the third solution include high-functional group resin, toughening resin, photosensitive resin, photoinitiator, second dispersant, and magnetic powder. The photosensitive adhesive cures quickly and can enhance the three-dimensional sense of the formed texture. Among them, the weight of the high-functional group resin is greater than or equal to 40 parts and less than or equal to 50 parts, the weight of the toughening resin is greater than or equal to 20 parts and less than or equal to 30 parts, the weight of the photosensitive resin is greater than or equal to 20 parts and less than or equal to 30 parts, the weight of the photoinitiator is greater than or equal to 3 parts and less than or equal to 4 parts, the weight of the second dispersant is greater than or equal to 1 part and less than or equal to 3 parts, the weight of the magnetic powder is greater than or equal to 1 part and less than or equal to 5 parts, and the magnetic powder has a double-layer package, which ensures the dispersibility of the magnetic powder in the photosensitive adhesive while ensuring the compatibility between the magnetic powder and the photosensitive adhesive, and avoiding the magnetic powder from precipitating quickly.
[0055] According to some embodiments of the present application, optionally, the high-functional group resin is at least one of the following: high-functional polyurethane acrylate 9018E and high-functional polyurethane acrylate 7605B; and / or the toughening resin is at least one of the following: polyol functional acrylate and polyacid functional acrylate; and / or the photoinitiator is at least one of the following: 1-hydroxycyclohexyl phenyl ketone or 2,4,6-trimethylbenzoyl.
[0056] In this embodiment, the high-functional group resin is at least one of the following: high-functional polyurethane acrylate 9018E and high-functional polyurethane acrylate 7605B, and / or the toughening resin is at least one of the following: polyol functional acrylate and polyacid functional acrylate; and / or the photoinitiator is at least one of the following: 1-hydroxycyclohexyl phenyl ketone or 2,4,6-trimethylbenzoyl, which ensures the dispersibility of the magnetic powder in the photosensitive adhesive while ensuring the compatibility between the magnetic powder and the photosensitive adhesive.
[0057] According to some embodiments of the present application, optionally, the viscosity of the magnetic powder glue is greater than or equal to 800 cPs and less than or equal to 1000 cPs.
[0058] In this embodiment, the viscosity of the magnetic powder glue is greater than or equal to 800 cPs and less than or equal to 1000 cPs, and when applied to the cover, the adhesion between the magnetic powder glue and the cover can be ensured. According to some embodiments of the present application, optionally, the pressure value of the degassing treatment is greater than or equal to 0.3 MPa and less than or equal to 0.5 MPa, and the duration of the degassing treatment is greater than or equal to 15 min and less than or equal to 30 min.
[0059] In this embodiment, the pressure value of the degassing treatment is greater than or equal to 0.3 MPa and less than or equal to 0.5 MPa, and the duration of the degassing treatment is greater than or equal to 15 minutes and less than or equal to 30 minutes, so that the bubbles in the photosensitive adhesive and the microbubbles at the interface between the magnetic powder and the photosensitive adhesive are eliminated, making the texture formed after curing clearer and more stable.
[0060] According to some embodiments of the present application, a magnetic powder adhesive is also proposed, which is prepared by any of the above-mentioned methods for preparing magnetic powder adhesives. Therefore, it has all the beneficial effects of any of the above-mentioned magnetic powder adhesives, which will not be described in detail here.
[0061] According to an embodiment of the present application, a cover is also provided, on which magnetic powder glue is provided. Therefore, all the beneficial effects of the magnetic powder glue are not described in detail here.
[0062] According to an embodiment of the present application, an electronic device is also provided, comprising: a cover body as provided in any one of the above items. Therefore, all the beneficial effects of the cover body are not described in detail here.
[0063] In specific applications, such as Figure 1 As shown, the preparation method of the three-dimensional smart powder (such as magnetic powder 1) is mainly as follows:
[0064] ① Preparation of magnetic material suspension (e.g. suspension):
[0065] The magnetic material suspension is composed of a magnetic material (such as the first powder 10), a silane coupling agent, and a solvent, wherein the ratio of magnetic material: silane coupling agent: solvent is 50 parts: 1 part: 100 parts, wherein the magnetic material includes but is not limited to a mixture of at least two of ferrite, neodymium iron boron, and cobalt aluminum nickel, and the solvent includes but is not limited to ethanol, water, etc., the stirring rate is 1000rpm-1500rpm, and the time is 15min-30min.
[0066] ②The first layer of coating 12:
[0067] Silver powder or pearl powder is added to the magnetic material suspension, and then a certain proportion of dispersant is added, and it is fully coated by ultrasonic dispersion. At the same time, the pH of the system is adjusted by dilute sodium hydroxide or dilute hydrochloric acid during the process to ensure the stability of the suspension. The ratio of silver powder or pearl powder: magnetic material suspension: dispersant is 100 parts: 10 parts-30 parts: 1 part-2 parts, the dispersant is BYK-9076 (for example, alkyl ammonium salt), the ultrasonic power is 200W-300W (adjusted according to the sample amount), the ultrasonic frequency is 25kHz-30kHz, the time is 15min-30min, and the pH value is adjusted to between 7-9; after the reaction is completed, 0.1M silver nitrate solution is slowly added to control the slow precipitation of the powder, and the precipitate is washed and filtered with deionized water to obtain a powder with a first layer of coating 12 (for example, a second powder).
[0068] ③The second layer of coating 14:
[0069] The powder with the first layer of coating 12 is added to a polydimethyldiallyl ammonium chloride (PDADMAC) solution, stirred thoroughly to ensure uniform coating, washed and filtered with deionized water to remove unabsorbed PDADMAC, and then the precipitate is transferred to a sodium polystyrene sulfonate (PSS) solution, stirred thoroughly to ensure uniform coating, washed and filtered with deionized water to remove unabsorbed PSS, and finally the coated powder is placed in a low-temperature vacuum drying oven to dry to prevent oxidation of the powder and remove residual moisture to obtain a three-dimensional smart powder. The ratio of PDADMAC and PSS solution is 0.1wt%-1wt%, the stirring time is 30min each time, the stirring rate is 1000rpm-1500rpm, and the particle size of the obtained magnetic powder is between 2μm-20μm. The stacked structure diagram of the prepared double-layer coated three-dimensional smart powder is as shown in the figure. Figure 1 As shown, the first coating 12 is wrapped around the outside of the first powder 10, and the second coating 14 is wrapped around the outside of the first coating 12, thereby finally forming a magnetic powder 1 with double layers of coating.
[0070] In order to realize a composite panel battery cover with a three-dimensional and dynamic 3D effect, this process scheme utilizes the characteristics of ultraviolet rays (UV) glue that can be evenly dispersed, quickly cured, and solvent-free, as well as the advantages of the UV glue transfer process that is easy to operate and automated in one-time operations. Three-dimensional dynamic powder is added to the UV glue to solve the problems of difficult dispersion and poor compatibility, and to ensure the stable mass production of subsequent construction processes. At the same time, double-layer textures and four-layer three-dimensional 3D effects can be superimposed on the outer surface (such as the second side of the cover) and the inner surface (such as the first side of the cover), which greatly enriches the appearance effect and enhances the product's appearance experience and the richness of the design.
[0071] like Figures 2 to 7 As shown, the production and processing of a mobile phone shell made of a composite sheet material with a three-dimensional and dynamic 3D effect includes two processes: (1) the production of a three-dimensional and dynamic UV glue (such as magnetic powder glue 2) and (2) the processing of the mobile phone shell made of the composite sheet material.
[0072] The production and processing process of (1) three-dimensional flexible UV glue includes three processes: ① pre-dispersion of three-dimensional flexible powder, ② preparation of three-dimensional flexible UV glue and ③ degassing treatment of glue.
[0073] ① Add the double-layer coated three-dimensional smart powder to the UV glue monomer resin, add a certain proportion of dispersant, and use ultrasonic dispersion treatment (ultrasonic power 200W-300W, ultrasonic frequency 25kHz-30kHz, 15 minutes-20 minutes) to ensure that the system is evenly dispersed, wherein the UV glue monomer resin is composed of one or more of functional acrylic monomers hexanediol diacrylate (HDDA), tetrahydrofuran acrylate (THFA), N-vinyl pyrrolidone (NVP), N,N-dimethylacrylamide (DMAA), wherein the dispersant type is BYK-9076 (such as alkyl ammonium salt), wherein the ratio of magnetic powder: monomer resin: dispersant is 5 parts: 100 parts: 1 part.
[0074] ② Then slowly add the dispersed solution in ① into the UV glue, and continue stirring for 30 minutes at a stirring rate of 1000rpm-1500rpm. The overall components of the three-dimensional smart UV glue include high-functional group resin, toughening resin, monomer resin, photoinitiator, dispersant, and three-dimensional smart powder in a ratio of 40 parts-50 parts: 20 parts-30 parts: 20 parts-30 parts: 3 parts-4 parts: 1 part-3 parts: 1 part-5 parts, wherein the high-functional group resin is one or both of high-functional polyurethane acrylate 9018E or 7605B, wherein the toughening resin is one or both of polyol functional acrylate or polyacid functional acrylate; wherein the monomer resin It is composed of one or more functional acrylic monomers HDDA, THFA, NVP, and DMAA; wherein the photoinitiator is composed of one or more 1-hydroxycyclohexyl phenyl ketone (such as 184) or 2,4,6-trimethylbenzoyl (TPO); wherein the dispersant is one or two of Solsperse2000 (such as hyperdispersant HY1305), BYK-110 (such as BYK dispersant BYK-110) or BYK-9076 (BYK dispersant BYK-9076), and the viscosity of the prepared glue is 800cPs-1000cPs, and the prepared glue needs to be filtered using a 100-150 mesh filter.
[0075] ③ Degas the stirred 3D flexible UV glue in a vacuum degassing device (0.3MPa, 15-30min) to ensure the dispersion and stability of the system.
[0076] Among them, the specific process flow of (2) the mobile phone shell of the composite sheet material with three-dimensional and flexible 3D effect is as follows:
[0077] Process solution 1 (2D composite sheet battery cover):
[0078] 1) Composite board cutting (e.g. Figure 6 Substrate 4):
[0079] Use CNC cutting to cut large sheets of composite panels into designed sizes.
[0080] 2) Inner surface transfer three-dimensional flexible UV glue:
[0081] A layer of three-dimensional flexible UV glue is printed on the inner surface of the composite board (PC surface, wherein PC is Polycarbonate) by roller transfer, two magnetic plates (such as magnetic template 31) are placed above and below the transfer machine, and a texture sub-mold (such as texture template 34) is superimposed, and the three-dimensional flexible 3D effect and the texture effect are superimposed in one step by LED light curing on the transfer machine, wherein the three-dimensional flexible UV glue used is the material prepared above, wherein the texture sub-mold includes but is not limited to photolithography texture, machined texture and etching texture, etc.; the film thickness of the transfer glue is 18μm-25μm, the roller pressure is 4kg-5kg, the roller speed is 40mm / s-60mm / s, and the LED lamp curing energy is 1000mJ / cm 2 -1800mJ / cm 2 .
[0082] Main functions:
[0083] The same machine can achieve the rich effects of three-dimensional dynamic 3D effect and texture effect superposition in one step. There is no need to repeatedly move the magnetic plate mold, product and texture sub-mold. It is efficient and fast, and the effect is rich.
[0084] 3) Optical coating (forming Figure 6 Coating layer in 5):
[0085] In order to enhance the three-dimensional and dynamic 3D effect of the transfer, an optical coating process is performed on the inner surface to achieve optical color adjustment and brightening effects, giving the three-dimensional dynamic effect rich colors and glossiness; the optical coating layer is attached to the transfer glue layer by an electron gun coating device. The optical coating layer is composed of two or more of silicon oxide, titanium oxide, silicon aluminum oxide, etc. The film thickness is 200nm-300nm, and the coating background vacuum is 3×10 -5 Up to 5×10 -5 The vacuum degree of the coating process is 5.0×10 -5 to 9.0×10 -5 .
[0086] Main functions:
[0087] The optical coating on the inner surface achieves optical color adjustment and brightening effects, and the three-dimensional flexible UV glue effect is superimposed to give the whole a rich gloss and texture.
[0088] 4) Silk screen printing cover color (formation Figure 6 Ink layer 6):
[0089] Five layers of ink are screen-printed on the inner surface, which not only protects the upper coating layer but also adjusts the color effect to ensure that the appearance effect and test performance are qualified; the ink thickness is 50μm-60μm, the baking temperature of each layer is 80℃, and the baking time of each layer is 60min.
[0090] Main functions:
[0091] ① Ensure qualified performance and protect the upper coating process layer;
[0092] ② Used for color matching, adjust different color effects according to design requirements to meet appearance requirements.
[0093] 5) External surface transfer printing of three-dimensional flexible UV glue (forming Figure 6 Magnetic powder glue 2) on the other side of the middle substrate 4:
[0094] A layer of three-dimensional flexible UV glue is printed on the outer surface (PMMA surface) of the composite board by roller transfer, two magnetic plates are placed above and below the transfer machine, and texture sub-molds are superimposed. Through primary curing by LED lamp on the transfer machine and secondary curing by mercury lamp, the rich effect of superposition of three-dimensional flexible 3D effect and texture effect can be achieved in one step, and at the same time, the hardness, wear resistance, weather resistance and other performance requirements of the outer surface of the product are guaranteed; wherein, the three-dimensional flexible UV glue used is the material prepared above, and the texture sub-mold includes but is not limited to photolithography texture, machined texture and etching texture, etc.; the film thickness of the transfer glue is 18μm-25μm, the roller pressure is 4kg-5kg, the roller speed is 40mm / s-60mm / s, and the primary curing energy of the LED lamp is 500mJ / cm 2 -800mJ / cm 2 , Mercury lamp secondary curing 2000mJ / cm 2 -3000mJ / cm 2 .
[0095] Main functions:
[0096] ① The same machine can achieve the rich effects of three-dimensional 3D effect and texture effect superposition at the same time, without repeatedly moving the magnetic plate mold, product and texture sub-mold, which is efficient and fast, and achieves rich effects;
[0097] ② The outer surface of the composite board achieves excellent effects while also having excellent hardness, wear resistance, weather resistance and other properties.
[0098] 6) CNC machining:
[0099] Processing is carried out according to the final structural drawings of the product.
[0100] like Figure 6 As shown, the prepared cover body includes a substrate 4, magnetic powder glue 2 located on both sides of the substrate 4, a coating layer 5 arranged on the surface of the magnetic powder glue 2 located on the inner side of the cover body, and an ink layer 6 located on the surface of the coating layer 5.
[0101] Process solution 2 (3D composite sheet battery cover):
[0102] 1) Composite sheet cutting (forming Figure 7 Substrate 4):
[0103] Use CNC cutting to cut large sheets of composite panels into designed sizes.
[0104] 2) Transfer three-dimensional flexible UV glue on the inner surface (forming Figure 7 The magnetic powder glue 2) located on one side of the substrate 4:
[0105] A layer of three-dimensional flexible UV glue is printed on the inner surface (PC surface) of the composite board by roller transfer, two magnetic plates are placed above and below the transfer machine, and texture sub-molds are superimposed. The three-dimensional flexible 3D effect and the rich effect of superimposed texture effect are achieved in one step, wherein the three-dimensional flexible UV glue used is the material prepared above, and the texture sub-mold involved includes but is not limited to photolithography texture, machined texture and etching texture, etc.; the film thickness of the transfer glue is 18μm-25μm, the roller pressure is 4kg-5kg, the roller speed is 40mm / s-60mm / s, and the LED lamp curing energy is 1000mJ / cm 2 -1800mJ / cm 2 .
[0106] Main functions:
[0107] The same machine can achieve the rich effects of three-dimensional dynamic 3D effect and superposition of texture effect in one step. There is no need to repeatedly move the magnetic plate mold, product and texture sub-mold. It is efficient and fast, and the effect is rich.
[0108] 3) External surface coating with three-dimensional flexible UV glue (forming Figure 7 The magnetic powder glue 2) located on the other side of the substrate 4:
[0109] A layer of three-dimensional flexible UV glue is printed on the outer surface of the composite board (PMMA surface, where PMMA is PolymethylMethacrylate) by pouring and rubbing. First, the three-dimensional flexible UV glue is diluted with a diluent to facilitate pouring and processing on the pouring line. Then the product is transferred to the transfer machine for rubbing and curing. Two magnetic plates are placed above and below the transfer machine, and the texture sub-mold is superimposed. The LED light on the transfer machine is used for primary curing and the mercury lamp is used for secondary curing, so that the three-dimensional flexible 3D effect and texture can be achieved in one step. The effect of superposition is rich, while ensuring the hardness, wear resistance, weather resistance and other performance requirements of the product's outer surface; the three-dimensional flexible UV glue used is the material prepared above, wherein the diluent includes but is not limited to one or more components such as ethyl acetate, butyl acetate, isophorone, etc., wherein the solid content ratio after dilution is 40%-60%, and the texture sub-mold includes but is not limited to photolithography texture, machined texture and etching texture, etc.; the coating baking temperature is 60℃-70℃, the baking time film thickness is 10μm-15μm, and the LED lamp one-time curing energy is 500mJ / cm 2 -800mJ / cm 2 , Mercury lamp secondary curing 1000mJ / cm 2 -1500mJ / cm 2 .
[0110] Main functions:
[0111] ① Through the same machine, the 3D composite sheet mobile phone shell can achieve the rich effects of three-dimensional and flexible 3D effect and texture effect superposition at the same time. There is no need to repeatedly move the magnetic plate mold, product and texture sub-mold. It is efficient and fast, and the effect is rich.
[0112] ② Achieve excellent effects on the outer surface of the composite board, while also having excellent hardness, wear resistance, weather resistance and other properties.
[0113] 4) High voltage:
[0114] The surface of the composite sheet is softened by high-pressure and high-temperature molding to achieve a 3D effect of the composite sheet modeling, wherein the high-pressure molding temperature is 300°C-400°C and the high-pressure molding time is 2min-3min.
[0115] Main functions:
[0116] ① Realize 3D modeling effect according to modeling design drawings through high pressure and high temperature molding;
[0117] ② Perform high pressure molding before the optical coating process to avoid high pressure film cracking problems caused by optical coating.
[0118] 5) Optical coating (forming Figure 7 Coating layer 5):
[0119] In order to enhance the three-dimensional and dynamic 3D effect of the transfer, an optical coating process is performed on the inner surface to achieve optical color adjustment and brightening effects, giving the three-dimensional dynamic effect rich colors and glossiness; the optical coating layer is attached to the transfer glue layer by an electron gun coating device. The optical coating layer is composed of two or more of silicon oxide, titanium oxide, silicon aluminum oxide, etc. The film thickness is 200nm-300nm, and the coating background vacuum is 3×10 -5 Up to 5×10 -5 The vacuum degree of the coating process is 5.0×10 -5 to 9.0×10 -5 .
[0120] Main functions:
[0121] The optical coating on the inner surface achieves optical color adjustment and brightening effects, and the three-dimensional flexible UV glue effect is superimposed to give the whole a rich gloss and texture.
[0122] 6) Spray the base color (forming Figure 7 Paint layer 7):
[0123] Five layers of paint are sprayed on the inner surface, which not only protects the upper coating layer but also adjusts the color to ensure that the appearance effect and test performance are qualified; the total thickness of the paint is 50μm-60μm, the baking temperature of each layer is 80℃, and the baking time of each layer is 60min.
[0124] Main functions:
[0125] ① Ensure qualified performance and protect the upper coating process layer.
[0126] ② Used for color matching, adjust different color effects according to design requirements to meet appearance requirements.
[0127] 7) CNC machining:
[0128] Processing is carried out according to the final structural drawings of the product.
[0129] The three-dimensional flexible ultraviolet rays (UV) glue proposed in this application has a stronger 3D effect than the silk-screen magnetic ink solution. The UV glue used is solvent-free and can be quickly cured and shaped by LED light, and the texture effect is more flexible and three-dimensional.
[0130] There are no special requirements for the current supplier's production line, transfer workshop and machines. Production and processing can be carried out on the existing line. Compared with the screen printing magnetic ink, a new screen printing baking line needs to be invested, which has increased costs, low efficiency, and too many magnetic plate molds. This process solution can transfer three-dimensional flexible powder using the existing transfer machine (single-station or four-station transfer machine), without special modification, and has extremely high efficiency (30s-60s). One machine only needs one set of magnetic plate molds. The lower magnetic plate is directly placed on the transfer machine, and the upper magnetic plate is placed on the top through a supporting lifting platform. There is no need to frequently move or move the magnetic plate molds and products. A transfer machine synchronously and automatically performs a series of processes such as loading-rolling-LED curing-unloading and product collection. The schematic diagram of the single-station transfer machine and the stacking structure of the loading area is shown as follows Figure 2 and Figure 3 As shown, among which, Figure 2 As shown, the machine 3 includes a support table 30 and a magnetic template 31 arranged on the support table 30, and a curing lamp 32 and a rubber roller 33 arranged on the other side. The feeding direction is shown by the arrow. Figure 3 As shown, the material stacking at the loading station is specifically as follows: a magnetic powder glue 2 is set on one side of the substrate 4, a texture template 34 is set at the bottom of the magnetic powder glue 2, and a magnetic template 31 is set at the bottom of the texture template 34. The magnetic template 31 at the bottom of the texture template 34 and the magnetic template 31 on the support table 30 work together to enhance the three-dimensional effect of the pattern on the cover. The schematic diagram of the four-station transfer machine and the material stacking structure in the loading area is shown in FIG. Figure 4 and Figure 5 As shown, Figure 4 As shown, the machine 3 includes a loading platform 36, a unloading platform 37, a rolling platform 35 and a curing lamp 32. Figure 5 As shown, the material stacking at the loading station (for example, the loading platform 36) is specifically as follows: a magnetic powder glue 2 is set on one side of the substrate 4, a texture template 34 is set at the bottom of the magnetic powder glue 2, and a magnetic template 31 is set at the bottom of the texture template 34. At the same time, a magnetic template 31 is also set on the other side of the substrate 4, and a support platform 30 is set on the top of the magnetic template 31. The magnetic template 31 at the bottom of the texture template 34 and the magnetic template 31 on the support platform 30 work together to enhance the three-dimensional effect of the pattern on the cover. The above can greatly save investment costs and improve efficiency.
[0131] This application solves at least the following technical problems:
[0132] 1. The problem of blackening and excessive impurities in three-dimensional dynamic powders is solved. The existing powders use magnetic materials to wrap (ferrite) silver powder or pearlescent powder, and the prepared powders have obvious problems of yellowing and blackening and impurities. This application optimizes the selection of wrapped magnetic materials and uses ferrite, neodymium iron boron, cobalt aluminum nickel and other mixed ratios to wrap to achieve the silvery and translucent effect of the powder.
[0133] 2. Solved the compatibility and dispersion uniformity problems of 3D smart powder and UV glue. First, the existing powder is directly wrapped with magnetic materials and then added to ink and paint. The solvent contained in it can disperse the powder well, but UV glue belongs to a solvent-free system. In order to ensure the dispersibility of UV glue and powder, the proportion of high-functionality resin in the UV glue system needs to be increased (the proportion of high-functionality resin in conventional glue is 20%-30%, and the proportion of high-functionality resin in 3D smart UV glue is 40%-60%), and the viscosity of the glue needs to be increased (the viscosity of conventional glue is 200c P-400cP, the viscosity of the three-dimensional flexible UV glue needs to reach 800cP-1000cP) to ensure that the powder can be evenly dispersed in the UV glue and is not easy to precipitate quickly; secondly, the proportion of high-functional group organic resin in the UV glue is too high, and the powder is an inorganic substance, there will be an incompatibility problem between the two. Therefore, the powder used in this application innovatively adds a double-layer coating, and a layer of ion complex (polydimethyldiallyl ammonium chloride PDADMAC and sodium polystyrene sulfonate PSS) is coated on the surface of the powder, which improves the compatibility between the powder and the UV glue.
[0134] The compatibility of the three-dimensional flexible UV glue and the transfer process has been solved. In order to ensure the three-dimensional flexible 3D effect, the film thickness of the UV glue transfer needs to reach 18μm-25μm, which is higher than the conventional glue film thickness (8μm-12μm). Uneven powder dispersion will cause uneven spots, glue scratches and streaks, and other poor appearances. In order to solve the above problems, first, the pre-dispersion effect of the powder and UV glue is further increased. The powder is pre-dispersed before adding. The pre-dispersion operation is to first use UV glue monomer resin and polymer dispersant (BYK-9076) for pre-dispersion, and then add it to the UV glue, which can further improve the compatibility and dispersibility of the mixture of the two. Second, before the construction of the three-dimensional flexible UV glue, a glue degassing process (0.3MPa, 15-30min) needs to be added to eliminate the bubbles in the glue and the microbubbles at the interface between the powder and the glue.
[0135] The problems of weak three-dimensional dynamic effect and poor effect are solved. First, compared with the weak three-dimensional effect caused by solvent volatilization and leveling in ink and paint systems, the three-dimensional dynamic UV glue adopts a solvent-free system. The glue is composed of monomer resin, high-functionality resin, photoinitiator, dispersant, and three-dimensional dynamic powder. UV light cures quickly and the formed texture effect has a strong three-dimensional sense. Second, in order to increase the richness of the three-dimensional dynamic effect, the application innovatively uses the upper and lower magnetic plates to act on the magnetic field at the same time, which can achieve richer design effects. Third, by using UV glue transfer method, the three-dimensional dynamic effect can also be superimposed with textures (including but not limited to photolithography textures, machined textures, and etching textures, etc.). If the three-dimensional dynamic UV glue is transferred on the inner and outer surfaces at the same time, a total of four layers of three-dimensional effect and two layers of texture superposition can be achieved, which greatly realizes the richness of the appearance effect.
[0136] The problem of low efficiency and increased costs in the production process is solved. Compared with the ink and paint system, the line and equipment need to be modified, the product needs to follow the magnetic plate and the line, the baking and curing time is long (30min-60min), and multiple magnetic plates are required to work at the same time to meet the production capacity (one line requires 20-30 magnetic plates), which is inefficient. This application innovatively adopts UV transfer method. The machine is the same as the conventional transfer machine. The magnetic plate is installed on the base or the top platform (no need to move or reverse), UV curing is fast (30s-60s), and one machine only uses one magnetic plate, which is highly efficient.
[0137] The embodiments proposed in this application can ensure that the performance of each unit and the whole machine test of the product is qualified.
[0138] The embodiment proposed in this application solves the problem of insufficient three-dimensional and flexible effects and insufficient richness based on the appearance effects of traditional mobile phone back covers. Three-dimensional flexible powder is added to UV glue, and the texture is printed on the inner and outer surfaces by transfer printing, and the upper and lower double-layer magnetic plates are used for magnetic field and magnetic domain effects, which can achieve the effect of four-layer three-dimensional 3D and two-layer texture superposition, greatly enriching the appearance effects, improving the appearance experience of the product and the feasibility of the design. By double-layer coating modification of three-dimensional flexible powder, the formula of UV glue is optimized, the compatibility and dispersibility with the UV glue system are improved, and the feasibility of mass production is improved.
[0139] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0140] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A method for preparing magnetic powder glue, It is characterized in that include: preparing a suspension using a magnetic material, a silane coupling agent and a solvent; adding a first powder to the suspension, and adding a first dispersant to obtain a first solution, and adding a silver nitrate solution to the first solution to obtain a first precipitate; Washing the first precipitate with deionized water to obtain a second powder; adding the second powder to a polydimethyldiallylammonium chloride solution to obtain a second precipitate, and adding the second precipitate to a sodium polystyrene sulfonate solution to obtain a third precipitate; Drying the third precipitate to obtain magnetic powder; The magnetic powder is added into a photosensitive adhesive to obtain the magnetic powder adhesive.
2. The method for preparing the magnetic powder glue according to claim 1, It is characterized in that After the step of adding the first powder to the suspension and adding the first dispersant, the method further comprises: subjecting the suspension to which the first powder and the first dispersant are added to the suspension to ultrasonic treatment; and / or adding dilute sodium hydroxide or dilute hydrochloric acid to the suspension to adjust the pH value of the first solution; Wherein, the pH value of the first solution is greater than or equal to 7 and less than or equal to 9.
3. The method for preparing the magnetic powder glue according to claim 1, It is characterized in that In the first solution, the weight of the first powder is 100 parts, the weight of the suspension is greater than or equal to 10 parts and less than or equal to 30 parts, and the weight of the first dispersant is greater than or equal to 1 part and less than or equal to 2 parts; The first dispersant includes: an alkyl ammonium salt.
4. The method for preparing magnetic powder glue according to claim 1, It is characterized in that The weight ratio of the sum of the mass of the polydimethyldiallylammonium chloride solution and the sodium polystyrene sulfonate solution to the magnetic powder is greater than or equal to 0.1% and less than or equal to 1%.
5. The method for preparing the magnetic powder glue according to claim 1, It is characterized in that After the step of adding the second powder to the polydimethyldiallylammonium chloride solution to obtain the second precipitate, the method further includes: washing the second precipitate with deionized water to remove the unabsorbed polydimethyldiallylammonium chloride; After the step of adding the second precipitate to the sodium polystyrene sulfonate solution to obtain the third precipitate, the method further includes: washing the third precipitate with deionized water to remove the unabsorbed sodium polystyrene sulfonate.
6. The method for preparing magnetic powder glue according to claim 1, It is characterized in that In the suspension, the weight portion of the magnetic material is 50 parts, the weight portion of the silane coupling agent is 1 part, and the weight portion of the solvent is 100 parts; and / or The magnetic material comprises a mixture of at least two of ferrite, neodymium iron boron and cobalt aluminum nickel; and / or The solvent includes at least one of ethanol and water.
7. The method for preparing the magnetic powder glue according to any one of claims 1 to 6, It is characterized in that The step of preparing the suspension using the magnetic material, the silane coupling agent and the solvent comprises: The magnetic material, the silane coupling agent and the solvent are mixed and stirred at a first stirring rate for a first time to obtain the suspension.
8. The method for preparing the magnetic powder glue according to any one of claims 1 to 6, It is characterized in that Also includes: The polydimethyldiallylammonium chloride solution to which the second powder is added is stirred at a second stirring rate for a second period of time.
9. The method for preparing the magnetic powder glue according to any one of claims 1 to 6, It is characterized in that The step of adding the magnetic powder into a photosensitive adhesive to obtain the magnetic powder adhesive comprises: Adding the magnetic powder to a photosensitive resin, and adding a second dispersant for pre-dispersion treatment to obtain a second solution; Adding the second solution into the photosensitive adhesive and stirring to obtain a third solution; The third solution is subjected to a degassing treatment to obtain the magnetic powder glue.
10. The method for preparing magnetic powder glue according to claim 9, It is characterized in that The photosensitive resin comprises one or more of the following compounds: functional acrylic monomers hexanediol diacrylate, tetrahydrofuran acrylate, N-vinyl pyrrolidone, N,N-dimethylacrylamide; and / or The second dispersant comprises: an alkyl ammonium salt; and / or The weight ratio of the magnetic powder, the photosensitive resin and the second dispersant is 5 parts:100 parts:1 part.
11. The method for preparing magnetic powder glue according to claim 9, It is characterized in that The components of the third solution include a high-functional group resin, a toughening resin, the photosensitive resin, a photoinitiator, the second dispersant and the magnetic powder; Wherein, the weight portion of the high-functional group resin is greater than or equal to 40 parts and less than or equal to 50 parts, the weight portion of the toughening resin is greater than or equal to 20 parts and less than or equal to 30 parts, the weight portion of the photosensitive resin is greater than or equal to 20 parts and less than or equal to 30 parts, the weight portion of the photoinitiator is greater than or equal to 3 parts and less than or equal to 4 parts, the weight portion of the second dispersant is greater than or equal to 1 part and less than or equal to 3 parts, and the weight portion of the magnetic powder is greater than or equal to 1 part and less than or equal to 5 parts; and / or The high-functional group resin is at least one of the following: high-functional polyurethane acrylate 9018E and high-functional polyurethane acrylate 7605B; and / or The toughening resin is at least one of the following: polyol functional acrylate and polyacid functional acrylate; and / or The photoinitiator is at least one of the following: 1-hydroxycyclohexyl phenyl ketone or 2,4,6-trimethylbenzoyl.