TPU (Thermoplastic Polyurethane) adhesive film, component and application
By preparing TPU film, combining polyester polyols and polyether polyols and other raw materials, the shortcomings of folding mobile phone protective film in terms of drop resistance and impact resistance are solved, and the mechanical properties stability and yellowing resistance under high temperature and high humidity are achieved. Performance, suitable for equipment with high bending performance requirements.
Patent Information
- Application Number
- CN202411243389.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
AI Technical Summary
The protective film of existing folding mobile phones has shortcomings in terms of drop resistance and impact resistance, and cannot meet the needs of bending performance.
Using TPU film, it is prepared by raw materials such as polyester polyol, polyether polyol, isocyanate curing agent, toluene, isopropanol, chain extender, light stabilizer, ultraviolet absorber, hydrolyzing agent and catalyst. After slit coating and oven film formation, it is combined with the protective film to form a TPU film that is resistant to hydrolysis, yellowing and bendable.
It achieves stable mechanical properties in high temperature and high humidity environments, excellent yellowing resistance, and low haze. It is suitable for optics that resist buffering and bending resistance, and solves the poor buffering resistance and bending resistance of original materials. Poor performance problem.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of folding screen protective films, and specifically relates to a TPU film, component and application. Background Art
[0002] TPU, or thermoplastic polyurethane elastomer, is a type of elastomer that can be plasticized by heating and dissolved by solvents. It has excellent comprehensive properties such as high strength, high toughness, wear resistance, and oil resistance, and has good processing performance. It is widely used in defense, medical, food and other industries. With the release of the first commercial flexible display smartphone FlexPai by Royole Technology in November 2018, the era of foldable phones officially began. In the following year of 2019, various terminal manufacturers launched foldable screen mobile phones one after another. Since then, foldable phones have officially entered the public's field of vision. For this reason, 2019 is also called the first year of foldable phones. Therefore, while the bending performance needs to be met, it is only protected by the existing protective film, and there are still deficiencies in drop resistance and impact resistance.
[0003] Therefore, in view of the above technical problems, it is necessary to provide a TPU film, component and application.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide a TPU film, a component and an application.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] The TPU film comprises a protective film, a TPU film and a hardening film which are arranged in sequence. The raw materials of the TPU film include, by mass: 20-30 parts of polyester polyol, 5-15 parts of polyether polyol, 1-10 parts of isocyanate curing agent, 30-40 parts of toluene, 15-20 parts of isopropanol, 3-10 parts of chain extender, 0.1-3 parts of light stabilizer, 0.1-3 parts of ultraviolet absorber, 0.1-3 parts of hydrolysis resistance agent and 0.1-0.5 parts of catalyst.
[0008] In one or more embodiments of the present invention, the polyester polyol is obtained by a melt condensation reaction of adipic acid and 1,4-butanediol or a polycondensation reaction of succinic acid and diethylene glycol.
[0009] In one or more embodiments of the present invention, the polyether polyol is selected from vinyl polymer grafted polyether polyol and polytetramethylene ether glycol.
[0010] In one or more embodiments of the present invention, the isocyanate curing agent is selected from HDI (1,6-hexamethylene diisocyanate), MDI (diphenylmethane diisocyanate), and IPDI (isophorone diisocyanate).
[0011] In one or more embodiments of the present invention, the chain extender is selected from ethylene glycol, propylene glycol, and butylene glycol.
[0012] In one or more embodiments of the present invention, the light stabilizer is a hindered amine light stabilizer.
[0013] In one or more embodiments of the present invention, the ultraviolet absorber is a reactive benzotriazole-based ultraviolet absorber.
[0014] In one or more embodiments of the present invention, the anti-hydrolysis agent is selected from polyether lipid anti-hydrolysis agents and polytetrafluoroethylene.
[0015] In one or more embodiments of the present invention, the catalyst is selected from organic tin, organic lead, and organic zinc. In one or more embodiments of the present invention, the method for preparing the adhesive film comprises the following steps:
[0016] A: Add polyester polyol and polyether polyol into a reaction kettle, heat to 95-105°C, vacuum dehydrate for 2-2.5 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 70-90°C, and stir for 2-3 hours to obtain a prepolymer;
[0017] B: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 95-105°C and evacuate for 2-2.5 hours, then add the prepolymer and mix and stir evenly, stir for 2-3 hours, cool to 40-50°C, add toluene and isopropanol solvents and stir and disperse for 1-1.5 hours, seal and store to obtain TPU slurry;
[0018] C: Take the hardened film as the substrate, and coat the TPU slurry on the substrate by slit coating. The coating thickness is 50-150μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃(±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 7-15min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0019] In one or more embodiments of the present invention, a display assembly includes a display body and a TPU adhesive film disposed on the body.
[0020] In one or more embodiments of the present invention, the display component is applied to an electronic device, and the electronic device is selected from a mobile communication terminal and a computer.
[0021] Compared with the prior art, the TPU film, components and applications of the present invention have excellent hydrolysis resistance, no obvious change in the mechanical properties of the product after high temperature and high humidity (85°C, 85% RH), excellent yellowing resistance, high transmittance and low haze, and can be applied to various types of anti-buffering and anti-bending optical devices, solving the defects of poor anti-buffering and anti-bending properties of the original materials. DETAILED DESCRIPTION
[0022] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0023] Including but not limited to the following embodiments: polyester polyol is obtained by melt condensation of adipic acid and 1,4-butanediol; polyether polyol is vinyl polymer grafted polyether polyol; isocyanate curing agent is HDI (1,6-hexamethylene diisocyanate); chain extender is butanediol; light stabilizer is hindered amine light stabilizer HS-508; ultraviolet absorber is reactive benzotriazole ultraviolet absorber Fisorb 328; catalyst is organic tin; hydrolysis resistance agent is polytetrafluoroethylene.
[0024] Example 1
[0025] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 3 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0026] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 95°C and then vacuum dehydrate for 2 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), maintain a constant temperature of 70°C, and stir for 2 hours to obtain a prepolymer.
[0027] 2: Mix the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 95℃ and evacuate for 2 hours, then add the prepolymer and mix evenly, stir for 2 hours, cool to 40℃, add toluene and isopropanol solvents and stir and disperse for 1 hour, and seal for storage.
[0028] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 50μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 7min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0029] Example 2
[0030] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 25 parts of polyester polyol, 10 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 3 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0031] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 95°C and then vacuum dehydrate for 2 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 70°C, and stir for 2 hours to obtain a prepolymer.
[0032] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 95℃ and evacuate for 2 hours, then add the prepolymer and mix evenly, stir for 2 hours, cool to 40℃, add toluene and isopropanol solvents, stir and disperse for 1 hour, and seal for storage.
[0033] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 50μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 7min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0034] Example 3
[0035] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 20 parts of polyester polyol, 15 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 3 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0036] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 95°C and then vacuum dehydrate for 2 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 70-90°C, and stir for 2 hours to obtain a prepolymer.
[0037] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 95℃ and evacuate for 2 hours, then add the prepolymer and mix evenly, stir for 2 hours, cool to 40℃, add toluene and isopropanol solvents, stir and disperse for 1 hour, and seal for storage.
[0038] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 50μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 7min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0039] Example 4
[0040] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 20 parts of polyester polyol, 15 parts of polyether polyol, 3 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 5 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0041] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 105°C and then vacuum dehydrate for 2.5 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 90°C, and stir for 3 hours to obtain a prepolymer.
[0042] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 105℃ and evacuate for 2.5 hours, then add the prepolymer and mix evenly, stir for 3 hours, cool to 50℃, add toluene and isopropanol solvents, stir and disperse for 1.5 hours, and seal for storage.
[0043] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 150μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 15min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0044] Example 5
[0045] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 3 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 5 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0046] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 105°C and then vacuum dehydrate for 2.5 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 90°C, and stir for 3 hours to obtain a prepolymer.
[0047] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 105℃ and evacuate for 2.5 hours, then add the prepolymer and mix evenly, stir for 3 hours, cool to 50℃, add toluene and isopropanol solvents, stir and disperse for 1.5 hours, and seal for storage.
[0048] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 150μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 15min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0049] Example 6
[0050] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 3 parts of chain extender, 0.3 parts of light stabilizer, 0.3 parts of ultraviolet absorber, 0.3 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0051] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 105°C and then vacuum dehydrate for 2.5 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 90°C, and stir for 3 hours to obtain a prepolymer.
[0052] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 105℃ and evacuate for 2.5 hours, then add the prepolymer and mix evenly, stir for 3 hours, cool to 50℃, add toluene and isopropanol solvents, stir and disperse for 1.5 hours, and seal for storage.
[0053] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 150μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 15min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0054] Example 7
[0055] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 3 parts of chain extender, 1 part of light stabilizer, 1 part of ultraviolet absorber, 1 part of hydrolysis resistance agent, and 0.1 part of catalyst.
[0056] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 100°C and then vacuum dehydrate for 2.25 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 80°C, and stir for 2.5 hours to obtain a prepolymer.
[0057] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 100℃ and evacuate for 2.25 hours, then add the prepolymer and mix evenly, stir for 2.5 hours, cool to 45℃, add toluene and isopropanol solvents, stir and disperse for 1.25 hours, and seal for storage.
[0058] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 100μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 10min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0059] Example 8
[0060] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 3 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.2 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0061] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 100°C and then vacuum dehydrate for 2.25 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), keep the temperature at 80°C, and stir for 2.5 hours to obtain a prepolymer.
[0062] 2: Stir the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 100℃ and evacuate for 2.25 hours, then add the prepolymer and mix evenly, stir for 2.5 hours, cool to 45℃, add toluene and isopropanol solvents, stir and disperse for 1.25 hours, and seal for storage.
[0063] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 100μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 10min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0064] Example 9
[0065] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 5 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0066] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 95°C and then vacuum dehydrate for 2 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), maintain a constant temperature of 70°C, and stir for 2 hours to obtain a prepolymer.
[0067] 2: Mix the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 95℃ and evacuate for 2 hours, then add the prepolymer and mix evenly, stir for 2 hours, cool to 40℃, add toluene and isopropanol solvents and stir and disperse for 1 hour, and seal for storage.
[0068] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 50μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 7min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0069] Example 10
[0070] In the embodiment of the present invention, a hydrolysis-resistant, yellowing-resistant and bendable TPU film includes the following raw materials in parts by weight: 30 parts of polyester polyol, 5 parts of polyether polyol, 10 parts of isocyanate curing agent, 40 parts of toluene, 20 parts of isopropanol, 10 parts of chain extender, 0.5 parts of light stabilizer, 0.5 parts of ultraviolet absorber, 0.5 parts of hydrolysis resistance agent, and 0.1 parts of catalyst.
[0071] The preparation method of hydrolysis-resistant, yellowing-resistant and bendable TPU film comprises the following steps: 1. Pour polyester polyol and polyether polyol into a reaction kettle in proportion, heat to 95°C and then vacuum dehydrate for 2 hours, introduce nitrogen into the reaction kettle, add isocyanate curing agent (sealed and stored at low temperature), maintain a constant temperature of 70°C, and stir for 2 hours to obtain a prepolymer.
[0072] 2: Mix the chain extender, light stabilizer, UV absorber, hydrolysis resistance agent and catalyst evenly, heat to 95℃ and evacuate for 2 hours, then add the prepolymer and mix evenly, stir for 2 hours, cool to 40℃, add toluene and isopropanol solvents and stir and disperse for 1 hour, and seal for storage.
[0073] 3: Take the hardened film as the substrate, and coat the TPU on the substrate by slit coating. The coating thickness is 50μm. The oven temperature is set to 50 / 60 / 60 / 70 / 90 / 120 / 130 / 130 / 130 / 100℃ (±10℃). After the TPU is formed into a film in the oven, it is compounded with the protective film and rolled up. The baking time is 7min. The product is stored under constant temperature and humidity conditions (23±3℃, 50±5%RH).
[0074] The following are the various test methods of various embodiments:
[0075] 1. Tensile modulus, elongation at break: Cut a sample strip with a length * width of 10cm * 1cm, tear off the protective film on both sides, set the tensile machine fixture spacing to 50mm, the tensile speed to 50mm / min, the test temperature and humidity to 25±5℃, 50±
[0076] 5% RH, tensile modulus is calculated as the slope of 0.2-0.5% strain, i.e. (0.5% stress-0.2% stress) / (0.5% strain-0.2% strain); elongation at break = tensile deformation / original length*100%
[0077] 2. Transmittance, haze: Cut a sample of 5cm*5cm, remove the protective film on both sides, and use a transmittance haze meter for testing
[0078] 3. Yellowing value △E: Remove the protective film on both sides of A4TPU and place the bare TPU in a QUV box, irradiance: (0.63±0.02)W / (m2*nm)@340nm; light + drying: 4H, blackboard temperature (60±3)℃; darkness + condensation: 4H, blackboard temperature (50±3)℃; lamp model: UVA-340, total cycle time 96H
[0079] 4. Bending test: Set the R angle to 1, test 200,000 times at room temperature, no creases
[0080] 5. Tensile modulus & elongation at break after double 85 ring test: Remove the protective film on both sides of A4TPU, place the bare TPU in a double 85 (85℃, 85%RH) ring test box for 120 hours, take it out and let it stand at room temperature for 1 hour, and test the tensile modulus and elongation at break normally according to the test method of Test 1.
[0081]
[0082]
[0083] The following are the test results of the embodiment:
[0084] It can be seen from the above embodiments and the corresponding test results that the hydrolysis-resistant and yellowing-resistant bendable TPU film of the present invention has excellent performance.
[0085] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0086] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A TPU film, comprising a protective film, a TPU film, and a curing film arranged in sequence, characterized in that: The raw materials of the TPU film include, by mass: 20-30 parts of polyester polyol, 5-15 parts of polyether polyol, 1-10 parts of isocyanate curing agent, 30-40 parts of toluene, 15-20 parts of isopropanol, 3-10 parts of chain extender, 0.1-3 parts of light stabilizer, 0.1-3 parts of ultraviolet absorber, 0.1-3 parts of hydrolysis resistance agent, and 0.1-0.5 parts of catalyst.
2. The TPU film according to claim 1, characterized in that: The polyester polyol is obtained by a melt condensation reaction of adipic acid and 1,4-butanediol or a polycondensation reaction of succinic acid and diethylene glycol.
3. The TPU film according to claim 1, characterized in that: The polyether polyol is selected from vinyl polymer grafted polyether polyol and polytetramethylene ether glycol.
4. The TPU film according to claim 1, characterized in that: The isocyanate curing agent is selected from HDI, MDI, IPDI 。 5. The TPU film according to claim 1, characterized in that: The chain extender is selected from ethylene glycol, propylene glycol and butanediol.
6. The TPU film according to claim 1, characterized in that: The light stabilizer is a hindered amine light stabilizer.
7. The TPU film according to claim 1, characterized in that: The ultraviolet absorber is a reactive benzotriazole ultraviolet absorber.
8. The TPU film according to claim 1, characterized in that: The anti-hydrolysis agent is selected from polyether lipid anti-hydrolysis agents and polytetrafluoroethylene.
9. A display assembly, comprising a display body and a TPU film according to any one of claims 1 to 8 arranged on the body.
10. Application of the display assembly according to claim 9 in an electronic device, wherein the electronic device is selected from a mobile communication terminal and a computer.