Ultra-soft composite silicon foam as well as preparation method and application thereof

By adding active hydroxyl substances and hydrogen-containing silicone oil to composite silicone foam, combined with heat-resistant agents and ceramic fillers, the problem of insufficient compressive elasticity of composite products is solved, achieving ultra-softness and high-temperature resistance.

CN118995078APending Publication Date: 2024-11-22SHENZHEN FUCHENGWEI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411362855.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing composite products made of fiberglass cloth or pre-oxidized fiber cloth and silicone rubber have low compression elasticity and cannot meet the needs of high-buffering application scenarios.

Method used

By adding active hydroxyl substances and hydrogen-containing silicone oil as foaming agents, combined with heat-resistant agents and ceramic fillers, ultra-soft composite silicone foam is prepared, controlling the cell structure and improving compression performance and high-temperature resistance.

Benefits of technology

The prepared ultra-soft composite silicone foam has ultra-soft properties, a Shore AO hardness of <25, a compressive stress of <40kPa required for 10% compression deformation, and can withstand high temperatures of 400-650℃, exhibiting excellent heat insulation and high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995078A_ABST
    Figure CN118995078A_ABST
Patent Text Reader

Abstract

The invention provides ultra-soft composite silicon foam as well as a preparation method and application thereof. The ultra-soft composite silicon foam comprises a base cloth layer and a silicon foam layer, the preparation raw materials of the silicon foam layer comprise glue A and glue B; the adhesive A comprises the following components in parts by weight: 50-70 parts of base adhesive, 1-8 parts of a heat-resistant agent, 15-30 parts of a flame retardant, 0.3-1.5 parts of a catalyst and 2-10 parts of a ceramic forming filler; and the glue B comprises the following components in parts by weight: 40-70 parts of base glue, 15-30 parts of a flame retardant, 6-8 parts of hydrogen-containing silicone oil, 1.5-2.5 parts of an active hydroxyl substance and 0.1-0.5 part of an inhibitor. The super-soft composite silicon foam provided by the invention has the characteristics of super softness, heat insulation and high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming materials, and specifically relates to an ultra-soft composite silicon foam and a preparation method and application thereof. Background Art

[0002] Glass fiber cloth or preoxidized silk fiber cloth has excellent high temperature resistance and good high temperature shape retention. The composite products of glass fiber cloth or preoxidized silk fiber cloth and silicone rubber have excellent high temperature resistance, low temperature resistance and thermal insulation performance, and are widely used in aerospace, chemical industry, electrical insulation, construction and other fields.

[0003] CN117901517A discloses a silicone cloth reinforced thermally conductive insulating gasket and a preparation method thereof, wherein the silicone cloth reinforced thermally conductive insulating gasket comprises a silicone cloth layer and a silicone body layer from bottom to top, wherein the silicone cloth layer adopts a single-sided coated silicone cloth, wherein the silicone cloth layer uses a glass fiber cloth as a base material and is compounded by a coating or calendering process with a mixed silicone. The silicone cloth reinforced thermally conductive insulating gasket provided by the technical solution has good adhesion between the silicone body layer and the silicone cloth layer and is not easy to separate.

[0004] CN112622370A discloses a silicone glass fiber cloth hot pressing buffer material and a preparation method thereof, wherein the silicone glass fiber cloth hot pressing buffer material comprises a liquid silicone layer, a heat conductive silicone layer and a glass fiber cloth coated with a silane coupling agent on both sides, wherein the glass fiber cloth is dried and coated with the liquid silicone layer on one side and the heat conductive silicone layer is calendered and compounded on the other side; the liquid silicone layer is a mixture of liquid silicone, a heat resistant agent and a heat conductive powder; the heat conductive silicone layer is obtained by filling a solid silicone with a heat conductive powder; wherein the raw material weight parts of the liquid silicone layer are as follows: 80-85 parts of liquid silicone, 5 parts of a heat resistant agent and 10-15 parts of a heat conductive powder; the raw material weight parts of the heat conductive silicone layer are as follows: 100 parts of solid silicone and 100-300 parts of a heat conductive powder. The silicone glass fiber cloth hot pressing buffer material provided by this technical solution can demonstrate its excellent insulation, high-speed heat transfer and high temperature resistance in extremely demanding applications.

[0005] In the prior art, the compressive elasticity of the composite product of glass fiber cloth or pre-oxidized silk fiber cloth and silicone rubber is relatively low and still needs to be further improved to meet the needs of high-buffering usage scenarios.

[0006] Therefore, it is necessary to develop a super soft, high temperature resistant super soft composite silicone foam. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide an ultra-soft composite silicone foam and a preparation method and application thereof, wherein the ultra-soft composite silicone foam has the characteristics of being ultra-soft, heat-insulating and high-temperature resistant.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides an ultra-soft composite silicone foam, wherein the ultra-soft composite silicone foam comprises a base fabric layer and a silicone foam layer;

[0010] The raw materials for preparing the silicone foam layer include glue A and glue B;

[0011] The A glue comprises the following components in parts by weight: 50-70 parts of base glue (for example, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts or 68 parts, etc.), 1-8 parts of heat-resistant agent (for example, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts or 7 parts, etc.), 15-30 parts of flame retardant (for example, 17 parts, 19 parts, 21 parts, 23 parts, 25 parts, 27 parts or 29 parts, etc.), 0.3-1.5 parts of catalyst (for example, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts or 1.4 parts, etc.) and 2-10 parts of porcelain-forming filler (for example, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts or 9 parts, etc.);

[0012] The B glue comprises the following components in parts by weight: 40-70 parts of base glue (for example, 43 parts, 46 parts, 49 parts, 52 parts, 55 parts, 58 parts, 61 parts, 64 parts or 67 parts, etc.), 15-30 parts of flame retardant (for example, 17 parts, 19 parts, 21 parts, 23 parts, 25 parts, 27 parts or 29 parts, etc.), 6-8 parts of hydrogen-containing silicone oil (for example, 6.2 parts, 6.4 parts, 6.6 parts, 6.8 parts, 7.0 parts, etc.). 1.5 to 2.5 parts (e.g., 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3 or 2.4 parts, etc.) of active hydroxyl substances and 0.1 to 0.5 parts (e.g., 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 or 0.45 parts, etc.) of inhibitors.

[0013] In the present invention, the ultra-soft composite silicone foam is prepared by adding active hydroxyl substances and hydrogen-containing silicone oil as foaming agents, so that the control of the pores is achieved, and the obtained ultra-soft composite silicone foam has a small compressive stress, thereby having ultra-soft characteristics. The ultra-soft composite silicone foam contains a large number of pore structures, which give the silicone foam good thermal insulation properties. In addition, by introducing a heat-resistant agent and a ceramic filler, and compounding a base fabric layer with excellent high-temperature resistance in the structure, the ultra-soft composite silicone foam has excellent high-temperature resistance.

[0014] In the present invention, the ultra-soft material means that the Shore AO hardness is less than 25, and the compressive stress required for 10% compression deformation is less than 40 kPa; the high temperature means 400-650°C.

[0015] Preferably, the base glue comprises a vinyl silicone oil mixture and a reinforcing filler.

[0016] Preferably, the mass ratio of the vinyl silicone oil mixture to the reinforcing filler is (3-6):(1-4), for example, 3:1, 3:2, 3:3, 3:4, 4:1, 4:3, 5:2, 5:3 or 5:4, etc.

[0017] Preferably, the vinyl silicone oil mixture is a combination of any two or at least three of vinyl silicone oils having a vinyl content of 0.05% to 0.5% (e.g., 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4% or 0.45%, etc.).

[0018] Preferably, the vinyl silicone oil having a vinyl content of 0.05% to 0.5% has a viscosity of 300 to 110,000 mm2 at 25°C. 2 / s(e.g. 1000mm 2 / s、5000mm 2 / s、10000mm 2 / s、40000mm 2 / s、70000mm 2 / s or 100000mm 2 / s, etc.).

[0019] Preferably, the reinforcing filler comprises fumed silica.

[0020] Preferably, the specific surface area of ​​the fumed silica is 100 to 400 m 2 / g, for example 150m 2 / g, 200m 2 / g, 250m 2 / g、300m 2 / g or 350m 2 / g, etc.

[0021] Preferably, the viscosity of the base glue at 25° C. is 5000-250000 mPa.s, for example, 10000 mPa.s, 50000 mPa.s, 100000 mPa.s, 150000 mPa.s or 200000 mPa.s, etc.

[0022] Preferably, the heat-resistant agent includes any one of cerium oxide, iron oxide or zinc oxide, or a combination of at least two of them.

[0023] Preferably, the particle size of the heat-resistant agent is 1.5 to 8 μm, for example, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm or 7 μm.

[0024] Preferably, the flame retardant includes any one of magnesium hydroxide, aluminum hydroxide or carbon black, or a combination of at least two of them.

[0025] Preferably, the particle size of the flame retardant is 3 to 8 μm, for example, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm or 7.5 μm.

[0026] Preferably, the catalyst comprises a Custer catalyst.

[0027] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 0.55% to 1.55% (eg, 0.65%, 0.75%, 0.85%, 0.95%, 1.05%, 1.15%, 1.25%, 1.35% or 1.45%, etc.).

[0028] Preferably, the viscosity of the hydrogenated silicone oil at 25°C is 10 to 110 mm 2 / s(e.g. 20mm 2 / s, 30mm 2 / s, 40mm 2 / s, 50mm 2 / s, 60mm 2 / s, 70mm 2 / s, 80mm 2 / s, 90mm 2 / s or 100mm 2 / s, etc.).

[0029] Preferably, the active hydroxyl substance includes deionized water and / or small molecule alcohol.

[0030] Preferably, the small molecule alcohol includes any one of methanol, ethanol, isopropanol, butanol, ethylene glycol or glycerol, or a combination of at least two thereof.

[0031] Preferably, the inhibitor comprises an acetylenic alcohol inhibitor.

[0032] Preferably, the porcelain-forming filler includes any one of silica fume, montmorillonite or kaolin, or a combination of at least two of them.

[0033] Preferably, the particle size of the ceramic filler is 6 to 10 μm, for example, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm or 9.5 μm.

[0034] Preferably, the mass ratio of glue A to glue B is (0.9-1.3):1, for example, 0.94:1, 0.97:1, 1:1, 1.03:1, 1.06:1, 1.09:1, 1.12:1, 1.15:1, 1.18:1, 1.21:1, 1.24:1 or 1.27:1, etc.

[0035] Preferably, the base fabric layer comprises glass fiber fabric or pre-oxidized silk fiber fabric.

[0036] In the present invention, both the glass fiber cloth and the pre-oxidized silk fiber cloth have excellent high temperature resistance.

[0037] Preferably, the glass fiber cloth comprises alkali-free glass fiber cloth.

[0038] Preferably, the thickness of the alkali-free glass fiber cloth is 0.05-0.5 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm or 0.4 mm.

[0039] Preferably, the thickness of the pre-oxidized silk fiber cloth is 0.05-2.0 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm or 0.4 mm.

[0040] Preferably, the thickness of the silicone foam layer is 1.0-8.0 mm, for example, 2.0 mm, 3.0 mm, 4.0 mm, 5.0 mm, 6.0 mm or 7.0 mm.

[0041] In a second aspect, the present invention provides a method for preparing the ultra-soft composite silicone foam as described in the first aspect, the preparation method comprising the following steps:

[0042] (1) mixing a base glue, a heat-resistant agent, a flame retardant, a ceramic filler and a catalyst to obtain glue A;

[0043] (2) mixing the base glue, the flame retardant, the hydrogen-containing silicone oil, the active hydroxyl substance and the inhibitor to obtain glue B;

[0044] (3) Mixing glue A and glue B, coating them on the base fabric layer, calendering, performing a first heat treatment, and a second heat treatment to obtain the ultra-soft composite silicone foam.

[0045] Preferably, the base glue is prepared by the following method: after the vinyl silicone oil mixture and the reinforcing filler are evenly mixed, the mixture is heated to 90-130°C (for example, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C or 125°C, etc.), and vacuumed for 0.5-2.0h (for example, 0.7h, 0.9h, 1.1h, 1.3h, 1.5h, 1.7h or 1.9h, etc.) to obtain the base glue.

[0046] Preferably, in the preparation method of the gum base, mixing includes kneading with a kneader.

[0047] Preferably, the step (3) specifically includes mixing glue A and glue B, applying them on the base fabric layer to form a glue layer, covering the glue layer with a release film, calendering, a first heat treatment, removing the release film, and a second heat treatment to obtain the ultra-soft composite silicone foam.

[0048] Preferably, the release film is a PET release film.

[0049] Preferably, the temperature of the first heat treatment is 70-100°C (for example, 75°C, 80°C, 85°C, 90°C or 95°C, etc.), and the time is 5-10 min (for example, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8.0 min, 8.5 min, 9 min or 9.5 min, etc.).

[0050] Preferably, the temperature of the second heat treatment is 120-160°C (for example, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C or 155°C, etc.), and the time is 15-30 min (for example, 17 min, 19 min, 21 min, 23 min, 25 min, 27 min or 29 min, etc.).

[0051] In a third aspect, the present invention provides an application of the ultra-soft composite silicone foam as described in the first aspect in a thermal insulation product or a cushioning product.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] In the present invention, the ultra-soft composite silicone foam prepared by compounding the base rubber, heat-resistant agent, flame retardant, ceramic filler, hydrogen-containing silicone oil, active hydroxyl substance, catalyst and inhibitor has low hardness, good compression performance and density ≤0.62g / cm 3 , Shore AO hardness ≤ 24, compression stress required for 10% compression deformation ≤ 32kPa, with super soft characteristics. The vertical flammability UL-94 of the super soft composite silicone foam is V0 grade, and the flame retardant performance is good. The super soft composite silicone foam can withstand high temperatures above 400℃, and the cold surface temperature of 650℃ insulation for 5min is ≤ 150℃, and has good insulation and high temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 A schematic diagram of the structure of the ultra-soft composite silicone foam provided in Example 1;

[0055] Among them, 1-base fabric layer; 2-silicon foam layer. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] The raw material vinyl silicone oil for the preparation of the following examples and comparative examples is as follows:

[0058] Vinyl silicone oil A, vinyl content is 0.08%, viscosity at 25℃ is 60000mm 2 / s;

[0059] Vinyl silicone oil B, vinyl content is 0.15%, viscosity at 25℃ is 5300mm 2 / s;

[0060] Vinyl silicone oil C, vinyl content is 0.1%, viscosity at 25℃ is 20000mm 2 / s;

[0061] Vinyl silicone oil D, vinyl content is 0.23%, viscosity at 25℃ is 2000mm 2 / s;

[0062] Vinyl silicone oil E, vinyl content is 0.5%, viscosity at 25℃ is 420mm 2 / s;

[0063] Vinyl silicone oil F, vinyl content is 0.05%, viscosity at 25℃ is 100000mm 2 / s.

[0064] Example 1

[0065] This embodiment provides a super soft composite silicon foam and a preparation method thereof, wherein the super soft composite silicon foam is Figure 1 As shown, it comprises a base fabric layer 1 and a silicone foam layer 2, wherein the base fabric layer is an alkali-free glass fiber fabric with a thickness of 0.5 mm; the silicone foam layer is 2.0 mm thick; the raw materials for preparing the silicone foam layer include A glue and B glue with a mass ratio of 1.15:1;

[0066] The A glue comprises the following components by weight: 50 parts of base glue, 1 part of heat-resistant agent (cerium oxide, particle size of 1.5 μm), 20 parts of flame retardant (magnesium hydroxide, particle size of 7 μm), 0.4 parts of catalyst (Kaster catalyst) and 3 parts of ceramic filler (montmorillonite, particle size of 7 μm);

[0067] The B glue comprises the following components by weight: 40 parts of base glue, 15 parts of flame retardant (magnesium hydroxide, particle size of 7 μm), hydrogen-containing silicone oil (hydrogen content of 0.8%, viscosity of 110 mm at 25°C), 2 / s) 8.0 parts, deionized water 1.8 parts, inhibitor (organic silicon inhibitor, 3,7,11-trimethyldodecyn-3-ol) 0.1 parts.

[0068] The above-mentioned base rubber is prepared by the following method: a vinyl silicone oil mixture formed by vinyl silicone oil A and vinyl silicone oil B in a mass ratio of 1:2 and fumed silica (specific surface area of ​​200 mm2 / g) was added into a kneader for kneading, the mass ratio of the vinyl silicone oil mixture to the fumed silica was 3:1, and after the powders were completely mixed, they were heated to 90° C. and vacuumed for 2 hours to obtain the base rubber.

[0069] The preparation method comprises the following steps:

[0070] (1) adding the base rubber, the heat-resistant agent, the flame retardant and the ceramic filler into a kneader and mixing them at 25° C. for 30 minutes to make the components uniformly mixed, then adding the catalyst and stirring at 25° C. for 10 minutes to obtain a rubber A;

[0071] (2) adding the base rubber, flame retardant, hydrogenated silicone oil and deionized water into a kneader and mixing them at 25° C. for 30 minutes to make the components uniformly mixed, then adding the inhibitor and mixing, stirring at 25° C. for 10 minutes to obtain rubber B;

[0072] (3) Glue A and glue B are mixed at 25° C., coated on the base fabric layer to form a glue layer, and then covered with a layer of PET release film on the glue layer, calendered, and then placed in an oven for a first heat treatment at 80° C. for 8 min, the PET release film is removed, and placed in an oven for a second heat treatment at 130° C. for 20 min, to obtain the ultra-soft composite silicone foam.

[0073] Example 2

[0074] The present embodiment provides an ultra-soft composite silicone foam and a preparation method thereof, wherein the ultra-soft composite silicone foam comprises a base fabric layer and a silicone foam layer, wherein the base fabric layer is an alkali-free glass fiber fabric with a thickness of 0.2 mm; the silicone foam layer has a thickness of 4.0 mm; and the raw materials for preparing the silicone foam layer include A glue and B glue with a mass ratio of 0.95:1;

[0075] The A glue comprises the following components by weight: 60 parts of base glue, 3 parts of heat-resistant agent (iron oxide and cerium oxide in a mass ratio of 1:1, the particle size of iron oxide is 3 μm, the particle size of cerium oxide is 5 μm), 20 parts of flame retardant (aluminum hydroxide, the particle size is 8 μm), 0.8 parts of catalyst (Kaster catalyst) and 10 parts of porcelain-forming filler (kaolin, the particle size is 10 μm);

[0076] The B glue comprises the following components by weight: 60 parts of base glue, 30 parts of flame retardant (aluminum hydroxide, particle size 7.5 μm), hydrogen-containing silicone oil (hydrogen content 1.0%, viscosity 10 mm at 25°C), 2 / s) 7 parts, deionized water 2 parts, inhibitor (organic silicon inhibitor, 3,7,11-trimethyldodecyn-3-ol) 0.2 parts.

[0077] The above-mentioned base rubber is prepared by the following method: a vinyl silicone oil mixture formed by vinyl silicone oil C and vinyl silicone oil D in a mass ratio of 1:1 and fumed silica (specific surface area of ​​400 mm 2 / g) was added to a kneader for kneading, the mass ratio of the vinyl silicone oil mixture to the fumed silica was 3:2, and after the powders were completely mixed, they were heated to 100° C. and added to a kneader for kneading. After the powders were completely mixed, they were heated to 100° C. and vacuumed for 2.0 hours to obtain the base rubber.

[0078] The preparation method comprises the following steps:

[0079] (1) adding the base rubber, the heat-resistant agent, the flame retardant and the ceramic filler into a kneader and mixing them at 25° C. for 30 minutes to make the components uniformly mixed, then adding the catalyst and stirring at 25° C. for 10 minutes to obtain a rubber A;

[0080] (2) adding the base rubber, flame retardant, hydrogenated silicone oil and deionized water into a kneader and mixing them at 25° C. for 30 minutes to make the components uniformly mixed, then adding the inhibitor and mixing, stirring at 25° C. for 10 minutes to obtain rubber B;

[0081] (3) Glue A and glue B are mixed at 25° C., coated on the base fabric layer to form a glue layer, and then covered with a layer of PET release film on the glue layer, calendered, and then placed in an oven for a first heat treatment at 80° C. for 8 min, the PET release film is torn off, and placed in an oven for a second heat treatment at 140° C. for 15 min to obtain the ultra-soft composite silicone foam.

[0082] Example 3

[0083] The present embodiment provides an ultra-soft composite silicone foam and a preparation method thereof, wherein the ultra-soft composite silicone foam comprises a base fabric layer and a silicone foam layer, wherein the base fabric layer is an alkali-free glass fiber fabric with a thickness of 0.1 mm; the silicone foam layer has a thickness of 8.0 mm; and the raw materials for preparing the silicone foam layer include A glue and B glue with a mass ratio of 0.94:1;

[0084] The A glue comprises the following components by weight: 70 parts of base glue, 1 part of heat-resistant agent (zinc oxide, particle size is 8 μm), 15 parts of flame retardant (magnesium hydroxide, particle size is 4 μm), 1.5 parts of catalyst (Kaster catalyst) and 5 parts of porcelain-forming filler (silica fume, particle size is 6 μm);

[0085] The B glue comprises the following components by weight: 70 parts of base glue, 20 parts of flame retardant (aluminum hydroxide, particle size 7 μm), hydrogen-containing silicone oil (hydrogen content 1.2%, viscosity 60 mm at 25°C), 2 / s) 6 parts, deionized water 2.3 parts and inhibitor (organic silicon inhibitor, 3,7,11-trimethyldodecene-3-ol alkynol) 0.5 parts.

[0086] The above-mentioned base rubber is prepared by the following method: a vinyl silicone oil mixture formed by vinyl silicone oil E and vinyl silicone oil F with a mass ratio of 1:0.5 and fumed silica (specific surface area of ​​200mm 2 / g) was added into a kneader for kneading, the mass ratio of the vinyl silicone oil mixture to the fumed silica was 5:2, and after the powders were completely mixed, they were heated to 130° C. and vacuumed for 0.5 h to obtain the base rubber.

[0087] The preparation method comprises the following steps:

[0088] (1) adding the base rubber, the heat-resistant agent and the flame retardant into a kneader and mixing them at 25° C. for 30 minutes to make the components uniformly mixed, then adding the catalyst and stirring at 25° C. for 10 minutes to obtain rubber A;

[0089] (2) adding the base rubber, flame retardant, hydrogenated silicone oil and deionized water into a kneader and mixing them at 25° C. for 30 minutes to make the components uniformly mixed, then adding the inhibitor and mixing, stirring at 25° C. for 10 minutes to obtain rubber B;

[0090] (3) Glue A and glue B are mixed at 25° C., coated on the base fabric layer to form a glue layer, and then a layer of PET release film is covered on the glue layer, calendered, and then placed in an oven for a first heat treatment at 100° C. for 5 min, the PET release film is torn off, and placed in an oven for a second heat treatment at 160° C. for 15 min to obtain the ultra-soft composite silicone foam.

[0091] Example 4

[0092] This embodiment provides an ultra-soft composite silicone foam and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of deionized water is adjusted to 1.5 parts, and other conditions are the same as Embodiment 1.

[0093] Example 5

[0094] This embodiment provides an ultra-soft composite silicone foam and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of deionized water is adjusted to 2.5 parts, and other conditions are the same as Embodiment 1.

[0095] Example 6

[0096] This embodiment provides an ultra-soft composite silicone foam and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the hydrogen-containing silicone oil (hydrogen content is 0.8%, viscosity is 110 mm at 25°C) is added to the foam. 2 / s) was replaced with the same mass (hydrogen content of 0.55%, viscosity of 60mm at 25°C) 2 / s), and other conditions are the same as those in Example 1.

[0097] Example 7

[0098] This embodiment provides an ultra-soft composite silicone foam and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the hydrogen-containing silicone oil (hydrogen content is 0.8%, viscosity is 110 mm at 25°C) is added to the foam. 2 / s) was replaced with the same mass of hydrogen-containing silicone oil (hydrogen content of 1.55%, viscosity of 30mm at 25°C) 2 / s), and other conditions are the same as those in Example 1.

[0099] Example 8

[0100] This embodiment provides an ultra-soft composite silicone foam and a preparation method thereof, which is different from Embodiment 1 only in that deionized water is replaced with ethylene glycol of the same mass and purity of 98%, and other conditions are the same as those in Embodiment 1.

[0101] Example 9

[0102] This embodiment provides an ultra-soft composite silicone foam and a preparation method thereof, which differs from Embodiment 1 only in that 1.8 parts by weight of deionized water is replaced with 1.8 parts by weight of a mixture of deionized water and 98% purity ethanol in a mass ratio of 1:1, and other conditions are the same as those in Embodiment 1.

[0103] Comparative Example 1

[0104] This comparative example provides a composite silicone foam and a preparation method thereof, which is different from Example 1 only in that the weight portion of deionized water is adjusted to 0.5 parts, and other conditions are the same as Example 1.

[0105] Comparative Example 2

[0106] This comparative example provides an ultra-soft composite silicone foam and a preparation method thereof, which is different from Example 1 only in that the weight portion of deionized water is adjusted to 3.0 parts, and other conditions are the same as Example 1.

[0107] Comparative Example 3

[0108] This comparative example provides a composite silicone rubber and a preparation method thereof, which is different from Example 2 only in that deionized water is not added, and other conditions are the same as those of Example 2.

[0109] Comparative Example 4

[0110] This comparative example provides a composite silicone foam and a preparation method thereof, which is different from Example 2 only in that the weight portion of hydrogen-containing silicone oil is adjusted to 5 parts, and other conditions are the same as Example 2.

[0111] The ultra-soft composite silicone foam, composite silicone foam and composite silicone rubber provided in the above embodiments and comparative examples were tested, and the specific testing method is as follows:

[0112] (1) Flame retardancy: tested in accordance with UL94 standard.

[0113] (2) Density: Tested in accordance with ISO 1183-1:2019 Method A.

[0114] (3) Compression: The test was conducted in accordance with ASTM D1056-20 to test the compressive stress required for the ultra-soft composite silicone foam to be compressed to 10%.

[0115] (4) Thermal insulation: Place one side of the base fabric layer on a 650°C hot plate and test the temperature of the foam layer on the other side.

[0116] (5) Shore hardness: tested in accordance with ISO 48-4:2018.

[0117] The results of the test are shown in Table 1 below.

[0118] Table 1

[0119]

[0120]

[0121] From the content of Table 1, it can be seen that the density of the ultra-soft composite silicone foam provided by Examples 1-9 is 0.35-0.62 g / cm 3 , vertical flammability UL-94 is V0 grade, Shore AO hardness ≤24, compression stress required for 10% compression deformation ≤32kPa, with the characteristics of ultra-soft, heat insulation and high temperature resistance.

[0122] Compared with Examples 1, 4, and 5, the amount of deionized water added will directly affect the density, compressive stress, and hardness of the ultra-soft composite silicone foam. When the amount of deionized water added is large, the porosity of the ultra-soft composite silicone foam is larger, and the density, hardness, and compressive stress of the ultra-soft composite silicone foam are smaller.

[0123] Compared with Example 1, if the hydrogen content of the hydrogen-containing silicone oil is lower (Example 6), the compressive stress is slightly larger; if the hydrogen content of the hydrogen-containing silicone oil is higher (Example 7), the obtained ultra-soft composite silicone foam has a smaller density and a lower compressive stress.

[0124] Compared with Example 1, if the weight percentage of deionized water is too low (Comparative Example 1), the compressive stress is too large, the density is too large, and the thermal insulation performance is poor; if the weight percentage of deionized water is too high (Comparative Example 2), although an ultra-soft composite silicone foam with low density and low compressive stress can be obtained, the surface state of the prepared ultra-soft composite silicone foam is poor and the surface is uneven. In the present invention, the ultra-soft composite silicone foam prepared by controlling the weight percentage of the active hydroxyl substance within a specific range has better performance.

[0125] Compared with Example 2, if deionized water is not added (Comparative Example 3), foaming cannot be performed to obtain solid silicone rubber.

[0126] Compared with Example 2, if the amount of hydrogen-containing silicone oil added is reduced (Comparative Example 4), the obtained composite silicone foam cannot be completely cross-linked, the surface of the composite silicone foam is sticky, and the pores are relatively small, the compressive stress is relatively large, and the density is relatively large.

[0127] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A super soft composite silicone foam, characterized in that: The super soft composite silicone foam comprises a base fabric layer and a silicone foam layer; The raw materials for preparing the silicon foam layer include glue A and glue B; The A glue comprises the following components by weight: 50-70 parts of base glue, 1-8 parts of heat-resistant agent, 15-30 parts of flame retardant, 0.3-1.5 parts of catalyst and 2-10 parts of porcelain-forming filler; The B glue comprises the following components in parts by weight: 40-70 parts of base glue, 15-30 parts of flame retardant, 6-8 parts of hydrogen-containing silicone oil, 1.5-2.5 parts of active hydroxyl substances and 0.1-0.5 parts of inhibitors.

2. The ultra-soft composite silicone foam according to claim 1, characterized in that: The base glue comprises a vinyl silicone oil mixture and a reinforcing filler; Preferably, the mass ratio of the vinyl silicone oil mixture to the reinforcing filler is (3-6): (1-4); Preferably, the vinyl silicone oil mixture is a combination of any two or at least three of the vinyl silicone oils having a vinyl content of 0.05% to 0.5%; Preferably, the vinyl silicone oil having a vinyl content of 0.05% to 0.5% has a viscosity of 300 to 110,000 mm2 at 25°C. 2 / s; Preferably, the reinforcing filler comprises fumed silica; Preferably, the specific surface area of ​​the fumed silica is 100 to 400 m 2 / g.

3. The ultra-soft composite silicone foam according to claim 1 or 2, characterized in that: The viscosity of the base glue at 25° C. is 5000-250000 mPa.s.

4. The super-soft composite silicone foam according to any one of claims 1 to 3, characterized in that: The heat-resistant agent includes any one of cerium oxide, iron oxide or zinc oxide, or a combination of at least two thereof; Preferably, the particle size of the heat-resistant agent is 1.5 to 8 μm; Preferably, the flame retardant comprises any one of magnesium hydroxide, aluminum hydroxide or carbon black, or a combination of at least two thereof; Preferably, the particle size of the flame retardant is 3 to 8 μm; Preferably, the catalyst comprises a Custer catalyst.

5. The super-soft composite silicone foam according to any one of claims 1 to 4, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 0.55% to 1.55%; Preferably, the viscosity of the hydrogenated silicone oil at 25°C is 10 to 110 mm 2 / s; Preferably, the active hydroxyl substance comprises deionized water and / or a small molecule alcohol; Preferably, the small molecule alcohol includes any one of methanol, ethanol, isopropanol, butanol, ethylene glycol or glycerol, or a combination of at least two thereof; Preferably, the inhibitor comprises an acetylenic alcohol inhibitor; Preferably, the ceramic-forming filler comprises any one of silica fume, montmorillonite or kaolin, or a combination of at least two thereof; Preferably, the particle size of the ceramic filler is 6 to 10 μm.

6. The super-soft composite silicone foam according to any one of claims 1 to 5, characterized in that: The mass ratio of the A glue and the B glue is (0.9-1.3):1; Preferably, the base fabric layer comprises glass fiber fabric or pre-oxidized silk fiber fabric; Preferably, the glass fiber cloth comprises alkali-free glass fiber cloth; Preferably, the thickness of the alkali-free glass fiber cloth is 0.05-0.5 mm; Preferably, the thickness of the pre-oxidized silk fiber cloth is 0.05 to 0.5 mm; Preferably, the thickness of the silicone foam layer is 0.5-8.0 mm.

7. A method for preparing the super-soft composite silicone foam according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) mixing a base glue, a heat-resistant agent, a flame retardant, a ceramic filler and a catalyst to obtain glue A; (2) mixing the base glue, the flame retardant, the hydrogen-containing silicone oil, the active hydroxyl substance and the inhibitor to obtain glue B; (3) Mixing glue A and glue B, coating them on the base fabric layer, calendering, performing a first heat treatment, and a second heat treatment to obtain the ultra-soft composite silicone foam.

8. The preparation method according to claim 7, characterized in that: The base glue is prepared by the following method: after the vinyl silicone oil mixture and the reinforcing filler are uniformly mixed, the mixture is heated to 90-130° C., and vacuumized for 0.5-2.0 hours to obtain the base glue.

9. The preparation method according to claim 7 or 8, characterized in that: The step (3) specifically comprises mixing glue A and glue B, applying the mixture on the base fabric layer to form a glue layer, covering the glue layer with a release film, calendering, performing a first heat treatment, removing the release film, and performing a second heat treatment to obtain the ultra-soft composite silicone foam; Preferably, the release film is a PET release film; Preferably, the temperature of the first heat treatment is 70-100°C and the time is 5-10 minutes; Preferably, the temperature of the second heat treatment is 120-160° C., and the time is 15-30 min.