Water-based adhesive applied to cigarette rolling manufacturing and preparation method of water-based adhesive
By introducing ε-polylysine, rosemary acid and spirocyclophosphoramantane structures into aqueous acrylate adhesives, the problem of insufficient antibacterial and flame retardant properties of the adhesive is solved, and long-term glue is achieved Adhesive performance improves the safety of cigarette coil manufacturing.
Patent Information
- Application Number
- CN202411435943.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The poor antibacterial and flame retardant properties of aqueous acrylate adhesives in cigarette rolling manufacturing limit their application. Conventional small molecule functional additives are prone to volatilization and migration, and it is difficult to achieve actual modification effect.
By grafting and complexing the antibacterial active ε-polylysine and rosmarinic acid, it is introduced into the aqueous acrylic resin adhesive structure through free radical polymerization, and a polymerization type combining spirocyclophosphoryl and adamantane colloidal structures. Monomers form modified monomers with synergistic antibacterial and flame retardant properties, and participate in the copolymerization process of adhesives.
The long-term antibacterial and flame retardant properties of the adhesive are achieved, avoiding the migration of additive materials, and improving hygiene and safety and product safety.
Smart Images

Figure CN118995097A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adhesives, and in particular to a water-based adhesive used in cigarette rolling and manufacturing and a preparation method thereof. Background Art
[0002] In the cigarette manufacturing industry, in order to ensure the stable connection of various parts of the cigarette, adhesives are needed to bond tobacco, filters and other parts to ensure that the cigarettes will not spread or fall off during transportation, storage and use. Therefore, adhesives are of great significance to the cigarette manufacturing industry. In recent years, with the enhancement of environmental awareness and the advancement of technology, water-based adhesives have gradually replaced traditional solvent-based adhesives due to their advantages such as environmental protection, low cost and non-flammability, and have become the new favorite in the field of cigarette rolling and splicing. Water-based acrylic adhesives have good bonding properties and are environmentally friendly and non-toxic, so they can be used in cigarette rolling and splicing.
[0003] During the cigarette production process, the growth of microorganisms will not only affect the quality of tobacco, but also pose a potential threat to human health. Therefore, the adhesive used for cigarette rolling should have good antibacterial properties. In addition, cigarettes are combustible items and there are fire hazards during production, storage and use. Therefore, the water-based adhesive used for cigarette rolling has good antibacterial and flame retardant properties to meet the hygiene and safety needs and product safety requirements in the cigarette production process.
[0004] However, water-based acrylic adhesives have poor flame retardancy and antibacterial properties, which limits their practical application in the cigarette rolling and joining industry. Therefore, it is necessary to develop water-based acrylic adhesives with good antibacterial and flame retardant properties. At present, the conventional method is mainly to achieve functional modification of adhesives through functional additives such as antibacterial agents and flame retardants. However, conventional small molecule functional additives are easy to volatilize and migrate, and it is difficult to achieve actual modification effects. Based on this, Benfu Mai Na provides a water-based acrylic adhesive that can be directly used in cigarette rolling and joining manufacturing. Summary of the invention
[0005] In order to solve the problems mentioned in the background technology, the purpose of the present invention is to provide a water-based adhesive used in cigarette rolling and manufacturing and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions: A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 90-100 parts of water-based acrylic resin emulsion; Defoaming agent 0.5-1.5 parts; 2-3 parts of thickener; The aqueous acrylic resin emulsion is prepared by the following method: Step S1, methyl methacrylate, butyl acrylate, glycidyl acrylate, modified monomer 1, modified monomer 2 and an emulsifier are mixed, and stirred and emulsified at 40-50° C. for 1-2 hours to form a premixed emulsion; Step S2, stirring and mixing the initiator and deionized water to prepare an initiator solution, then mixing the initiator solution with the premixed emulsion, introducing nitrogen for protection, then controlling the temperature at 75-82°C, heat preservation for 6-9h, cooling and discharging, and obtaining a water-based acrylic resin emulsion.
[0007] As a further embodiment of the present invention, the mass ratio of methyl methacrylate, butyl acrylate, glycidyl acrylate, modified monomer one, modified monomer two, emulsifier, initiator and deionized water is 10-20:5-7:0.5-1.5:1-2:1.5-4:0.5-1:0.1-0.2:80-100.
[0008] As a further embodiment of the present invention, the method for preparing the modified monomer 1 comprises the following steps: Step S10, ε-polylysine and tetrahydrofuran are mixed and stirred evenly, and then rosmarinic acid is added to the formed mixed solution under nitrogen protection, and a composite catalyst is added. After the addition, the mixture is stirred at room temperature for 3-6 hours, the material is collected by centrifugation, and washed and dried to obtain a polylysine modified body; Firstly, a composite catalyst is used to catalyze the condensation reaction between the amino group in the ε-polylysine structure and the carboxyl group in the rosmarinic acid structure, thereby introducing the natural antibacterial agent rosmarinic acid into the ε-polylysine structure to obtain a modified polylysine. Step S11, adding the modified polylysine to acetone, mechanically stirring and mixing to form a uniform mixed solution, adding the olefinic monomer to the mixed solution, stirring at room temperature for 1-2 hours, and centrifuging out the solid material to obtain a modified monomer 1.
[0009] Next, the polylysine modified body is subjected to olefination modification using an olefination monomer, so that polymerizable unsaturated carbon-carbon double bonds are generated in its structure, thereby obtaining a modified monomer 1.
[0010] As a further embodiment of the present invention, in step S10, the number average molecular weight of the ε-polylysine is 3800.
[0011] As a further solution of the present invention, in step S10, the composite catalyst is dicyclohexylcarbodiimide and 4-dimethylaminopyridine, and the mass ratio is 1:0.4-0.5.
[0012] As a further solution of the present invention, in step S20, the olefinic monomer is acryloyl chloride or methacryloyl chloride.
[0013] As a further embodiment of the present invention, the preparation method of the modified monomer 2 is as follows: Add spirocyclic phosphoryl dichloride and toluene to a polymerization kettle filled with nitrogen, start stirring, and after complete dissolution, add 1,3-adamantanediamine to the polymerization kettle. After the addition is completed, gradually increase the temperature to 60-70°C, keep warm for 2-4 hours, then add triethylamine to the polymerization kettle, and then continue stirring for 6-9 hours. Then, add a capping agent to the polymerization kettle, keep warm for 0.5-1 hour after the addition, evaporate under reduced pressure to remove the solvent, cool and discharge the material, and the modified monomer II can be obtained.
[0014] In the above technical scheme, spirocyclic phosphoryl dichloride and 1,3-adamantanediamine are used as copolymer monomers. Under the action of the acidifying agent triethylamine, the phosphoryl chloride group in the spirocyclic phosphoryl dichloride structure can be continuously condensed with the amino group in the 1,3-adamantanediamine structure to form a polymerized product in which spirocyclic phosphoryl dichloride and 1,3-adamantanediamine are alternately connected via phosphoramide groups. By controlling the dosage ratio of the two, the phosphoryl chloride group is contained at the end of the structure of the polymerized product. Then, the end of the structure is capped with a capping agent so that an unsaturated olefinic functional group capable of participating in a free radical polymerization reaction is generated at the end of the structure to obtain a modified monomer II.
[0015] As a further embodiment of the present invention, the molar ratio of the spirocyclic phosphoryl dichloride to 1,3-adamantanediamine is 1:0.8-1.
[0016] As a further embodiment of the present invention, the end-capping agent is hydroxyethyl methacrylate or hydroxyethyl acrylate.
[0017] A method for preparing a water-based adhesive used in cigarette rolling and manufacturing, comprising the following steps: Step S20, weighing each component according to weight for standby use; Step S21, add the water-based acrylic resin emulsion, defoamer, and thickener into a mixer, shear and mix them evenly at a speed of 2000-3000 r / min, and then let them stand for 1-2 hours to defoam, so as to obtain a water-based adhesive.
[0018] Beneficial effects of the present invention: (1) The present invention grafts and compounds ε-polylysine and rosmarinic acid with antibacterial activity, and then introduces them into the structure of a water-based acrylic resin adhesive through free radical polymerization. The ε-polylysine can destroy the bacterial cell membrane to cause bacterial death, and the rosmarinic acid can affect bacterial DNA replication and inhibit bacterial growth. The two cooperate with each other to give the adhesive excellent antibacterial activity. Moreover, after being introduced into the adhesive molecular chain through free radical polymerization, the migration and precipitation problem can be avoided, and the long-term antibacterial performance of the adhesive is guaranteed, thereby improving the hygiene and safety in the adhesive production process.
[0019] (2) The present invention prepares a polymerizable monomer having a spirocyclic phosphoryl and adamantane colloidal structure as the second modified monomer and participates in the copolymerization process of the water-based acrylic adhesive, thereby achieving the purpose of introducing a flame retardant into the molecular chain of the adhesive. The adamantane heterocycle contained in the modified monomer structure can serve as an expanding carbon source, and cooperates with the gas source and acid source provided by the nitrogen element and the phosphorus element to form a ternary expanding flame retardant. After it is introduced into the molecular chain of the adhesive, an expanding carbon layer can be quickly formed during the combustion process to prevent the combustion from continuing, thereby achieving the effect of greatly enhancing the flame retardant performance of the adhesive with a small amount of addition, thereby improving the safety requirements of the adhesive in the manufacture of cigarette rolling.
[0020] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0022] Figure 1 This is the infrared analysis test diagram of modified monomer 1; Figure 2 This is the infrared analysis test diagram of modified monomer 2. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0024] 1. Preparation of modified monomer 1 Step S10, 2.2 g of ε-polylysine with a number average molecular weight of 3800 was mixed with tetrahydrofuran and stirred evenly, and then 0.8 g of rosmarinic acid was added to the resulting mixed solution under nitrogen protection, and 0.5 g of dicyclohexylcarbodiimide and 0.2 g of 4-dimethylaminopyridine were added. After the addition, the mixture was stirred at room temperature for 4 h, the material was collected by centrifugation, washed, and dried to obtain a polylysine modified body; Step S11, adding 1.8 g of modified polylysine to acetone, mechanically stirring and mixing to form a uniform mixed solution, then adding 0.2 g of acryloyl chloride to the mixed solution, stirring at room temperature for 2 h, and centrifuging out the solid material to obtain modified monomer 1.
[0025] Figure 1 This is the infrared analysis test chart of the modified monomer 1, where 3409cm -1 The characteristic absorption peak of NH is at 3096cm -1 and 3064cm -1 The characteristic absorption peak of CH on the benzene ring of rosmarinic acid is 3021cm -1 The absorption peak at the unsaturated carbon-carbon double bond is the characteristic absorption peak of CH, 1753 cm -1 The absorption peak at 1695 cm is the characteristic absorption peak of ester C=O. -1 The absorption peak that appears at is the C=O characteristic absorption peak of the amide bond.
[0026] 2. Preparation of modified monomer 2 Add 0.8 g of spirocyclic phosphoryl dichloride and toluene to a polymerization kettle filled with nitrogen, start stirring, and after complete dissolution, add 0.4 g of 1,3-adamantanediamine to the polymerization kettle. After the addition is completed, gradually increase the temperature to 65°C. After keeping warm for 3 hours, add 0.2 g of triethylamine to the polymerization kettle, and then continue stirring for 8 hours. Then, add 0.1 g of hydroxyethyl methacrylate to the polymerization kettle. After adding, keep warm for 0.5 hours, evaporate the solvent under reduced pressure, cool and discharge the material, and the modified monomer II can be obtained.
[0027] Figure 2 This is the infrared analysis test chart of the modified monomer 2, where 3179cm -1 The absorption peak at 3002cm is the characteristic absorption peak of NH. -1 The absorption peak at 2800-3000cm is the characteristic absorption peak of CH on the unsaturated carbon-carbon double bond. -1 The absorption peak at 1292 cm is the characteristic absorption peak of CH in the adamantane structure. -1 The absorption peak at 930cm is the characteristic absorption peak of P=O. -1 The absorption peak that appears at is the PN characteristic absorption peak.
[0028] 3. Preparation of water-based acrylic resin emulsion Step S1, 15g of methyl methacrylate, 6g of butyl acrylate, 1g of glycidyl acrylate, 1.5g of modified monomer 1, 3g of modified monomer 2 and 0.6g of sodium dodecyl sulfonate were mixed, and stirred and emulsified at 45°C for 2h to form a premixed emulsion; Step S2, 0.1 g of azobisisobutyronitrile and 100 mL of deionized water were stirred and mixed to prepare an initiator solution, and then the initiator solution was mixed with the premixed emulsion, and nitrogen was introduced for protection, and then the temperature was controlled at 78° C., and the heat treatment was carried out for 8 hours, and the temperature was lowered and the material was discharged to obtain a water-based acrylic resin emulsion. Example 2
[0029] A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 90 parts of water-based acrylic resin emulsion; Defoaming agent alkylphenol polyoxyethylene ether 0.5 parts; Thickener hydroxyethyl cellulose 2 parts; The water-based adhesive is prepared by the following method: Step S20, weighing each component according to weight for standby use; Step S21, add water-based acrylic resin emulsion, defoaming agent alkylphenol polyoxyethylene ether, and thickener hydroxyethyl cellulose into a mixer, shear and mix them evenly at a speed of 2500 r / min, and then let it stand for 1 hour to defoam, so as to obtain a water-based adhesive.
[0030] The preparation method of the aqueous acrylic resin emulsion is shown in Example 1. Example 3
[0031] A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 95 parts of water-based acrylic resin emulsion; 1 part of defoaming agent alkylphenol polyoxyethylene ether; Thickener hydroxyethyl cellulose 3 parts; The water-based adhesive is prepared by the following method: Step S20, weighing each component according to weight for standby use; Step S21, add water-based acrylic resin emulsion, defoaming agent alkylphenol polyoxyethylene ether, and thickener hydroxyethyl cellulose into a mixer, shear and mix them evenly at a speed of 2500 r / min, and then let it stand for 2 hours to defoam, so as to obtain a water-based adhesive.
[0032] The preparation method of the aqueous acrylic resin emulsion is shown in Example 1. Example 4
[0033] A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 100 parts of water-based acrylic resin emulsion; 1.5 parts of defoaming agent alkylphenol polyoxyethylene ether; Thickener hydroxyethyl cellulose 3 parts; The water-based adhesive is prepared by the following method: Step S20, weighing each component according to weight for standby use; Step S21, add water-based acrylic resin emulsion, defoaming agent alkylphenol polyoxyethylene ether, and thickener hydroxyethyl cellulose into a mixer, shear and mix them evenly at a speed of 2500 r / min, and then let it stand for 2 hours to defoam, so as to obtain a water-based adhesive.
[0034] The preparation method of the aqueous acrylic resin emulsion is shown in Example 1.
[0035] Comparative Example 1 A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 95 parts of water-based acrylic resin emulsion; 1 part of defoaming agent alkylphenol polyoxyethylene ether; Thickener hydroxyethyl cellulose 3 parts; 1 part of ε-polylysine; The water-based adhesive is prepared by the following method: Step S20, weighing each component according to weight for standby use; Step S21, add water-based acrylic resin emulsion, defoaming agent alkylphenol polyoxyethylene ether, thickener hydroxyethyl cellulose, and ε-polylysine into a mixer, shear and mix them evenly at a speed of 2500 r / min, and then let it stand for 2 hours to defoam, so as to obtain a water-based adhesive.
[0036] The preparation method of the aqueous acrylic resin emulsion is different from that of Example 1 in that no modified monomer 1 is added.
[0037] Comparative Example 2 A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 90 parts of water-based acrylic resin emulsion; Defoaming agent alkylphenol polyoxyethylene ether 0.5 parts; Thickener hydroxyethyl cellulose 2 parts; The water-based adhesive is prepared by the following method: Step S20, weighing each component according to weight for standby use; Step S21, add water-based acrylic resin emulsion, defoaming agent alkylphenol polyoxyethylene ether, and thickener hydroxyethyl cellulose into a mixer, shear and mix them evenly at a speed of 2500 r / min, and then let it stand for 1 hour to defoam, so as to obtain a water-based adhesive.
[0038] The preparation method of the aqueous acrylic resin emulsion is different from that of Example 1 in that no modified monomer 1 is added.
[0039] Comparative Example 3 A water-based adhesive for cigarette rolling and splicing, comprising the following raw materials in parts by weight: 95 parts of water-based acrylic resin emulsion; 1 part of defoaming agent alkylphenol polyoxyethylene ether; Thickener hydroxyethyl cellulose 3 parts; The water-based adhesive is prepared by the following method: Step S20, weighing each component according to weight for standby use; Step S21, add water-based acrylic resin emulsion, defoaming agent alkylphenol polyoxyethylene ether, and thickener hydroxyethyl cellulose into a mixer, shear and mix them evenly at a speed of 2500 r / min, and then let it stand for 2 hours to defoam, so as to obtain a water-based adhesive.
[0040] The preparation method of the aqueous acrylic resin emulsion is different from that of Example 1 in that no modified monomer 2 is added.
[0041] Test Case a. Antibacterial rate test: The water-based adhesives in Examples 2 to 4 and Comparative Examples 1 to 3 were uniformly coated on the surface of a clean glass plate, and after curing, the film was removed to form a test film, which was made into a circular test sample with a diameter of 10 mm. 1 mL of Staphylococcus aureus suspension was added to beef broth and cultured for 8 h, and then diluted to 10 -5 CFU / mL, use a pipette to take 0.5mL of the diluted bacterial suspension, drop it on the surface of the sample, continue to culture for 4h, then wash the sample with sterile water, collect the washing liquid, and transfer 0.5mL of the washing liquid to the culture dish for culture for 8h. The culture process is carried out at 37℃, observe the colony count, and do a blank test at the same time. Use the formula [(blank test colony count-sample colony count) / blank test colony count]×100% to calculate the antibacterial rate of each sample; b. The adhesives of Examples 2 to 4 and Comparative Examples 1 to 3 were made into test samples with a specification of 10 cm×6.5 mm×3 mm, and the limiting oxygen index test was performed using a JF-3 limiting oxygen index instrument; The above test results are recorded in Table 1: Table 1 - Test results
[0042] The analysis and test results show that the adhesive prepared using the aqueous acrylic resin emulsion prepared in Example 1 of the present invention as the main raw material obviously has good antibacterial and flame retardant properties.
[0043] After the modified monomer was removed, the antibacterial properties of the adhesive decreased significantly when ε-polylysine was used alone as an antibacterial agent, proving that the combination of ε-polylysine and rosmarinic acid can produce a synergistic effect and make the adhesive have better antibacterial properties.
[0044] After removing ε-polylysine, the adhesive does not contain any antibacterial agent, so the antibacterial performance is poor.
[0045] The adhesive using the water-based acrylic resin emulsion prepared by removing the modified monomer II as the main raw material does not contain an intumescent flame retardant in its structure, so its flame retardant performance is greatly reduced.
[0046] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A water-based adhesive used in cigarette rolling and manufacturing, characterized in that: The invention comprises the following raw materials in parts by weight: 90-100 parts of water-based acrylic resin emulsion; Defoaming agent 0.5-1.5 parts; 2-3 parts of thickener; The aqueous acrylic resin emulsion is prepared by the following method: Step S1, methyl methacrylate, butyl acrylate, glycidyl acrylate, modified monomer 1, modified monomer 2 and an emulsifier are mixed, and stirred and emulsified at 40-50° C. for 1-2 hours to form a premixed emulsion; Step S2, stirring and mixing the initiator and deionized water to prepare an initiator solution, then mixing the initiator solution with the premixed emulsion, introducing nitrogen for protection, then controlling the temperature at 75-82°C, heat preservation for 6-9h, cooling and discharging, and obtaining a water-based acrylic resin emulsion.
2. The water-based adhesive used in cigarette rolling and manufacturing according to claim 1, characterized in that: The mass ratio of the methyl methacrylate, butyl acrylate, glycidyl acrylate, modified monomer one, modified monomer two, emulsifier, initiator and deionized water is 10-20:5-7:0.5-1.5:1-2:1.5-4:0.5-1:0.1-0.2:80-100.
3. A water-based adhesive for cigarette rolling and manufacturing according to any one of claims 1 or 2, characterized in that: The preparation method of the modified monomer 1 comprises the following steps: Step S10, ε-polylysine and tetrahydrofuran are mixed and stirred evenly, and then rosmarinic acid is added to the formed mixed solution under nitrogen protection, and a composite catalyst is added. After the addition, the mixture is stirred at room temperature for 3-6 hours, the material is collected by centrifugation, and washed and dried to obtain a polylysine modified body; Step S11, adding the modified polylysine to acetone, mechanically stirring and mixing to form a uniform mixed solution, adding the olefinic monomer to the mixed solution, stirring at room temperature for 1-2 hours, and centrifuging out the solid material to obtain a modified monomer 1.
4. The water-based adhesive used in cigarette rolling and manufacturing according to claim 3, characterized in that: In step S10, the number average molecular weight of the ε-polylysine is 3800.
5. The water-based adhesive used in cigarette rolling and splicing according to claim 3, characterized in that: In step S10, the composite catalyst is dicyclohexylcarbodiimide and 4-dimethylaminopyridine, and the mass ratio is 1:0.4-0.
5.
6. The water-based adhesive used in cigarette rolling and splicing according to claim 3, characterized in that: In step S20, the olefinic monomer is acryloyl chloride or methacryloyl chloride.
7. A water-based adhesive for cigarette rolling and manufacturing according to any one of claims 1 or 2, characterized in that: The preparation method of the modified monomer 2 is as follows: Add spirocyclic phosphoryl dichloride and toluene to a polymerization kettle filled with nitrogen, start stirring, and after complete dissolution, add 1,3-adamantanediamine to the polymerization kettle. After the addition is completed, gradually increase the temperature to 60-70°C, keep warm for 2-4 hours, then add triethylamine to the polymerization kettle, and then continue stirring for 6-9 hours. Then, add a capping agent to the polymerization kettle, keep warm for 0.5-1 hour after the addition, evaporate under reduced pressure to remove the solvent, cool and discharge the material, and the modified monomer II can be obtained.
8. The water-based adhesive used in cigarette rolling and manufacturing according to claim 7, characterized in that: The molar ratio of the spirocyclic phosphoryl dichloride to 1,3-adamantanediamine is 1:0.8-1.
9. The water-based adhesive used in cigarette rolling and splicing according to claim 7, characterized in that: The end-capping agent is hydroxyethyl methacrylate or hydroxyethyl acrylate.
10. A method for preparing a water-based adhesive for cigarette rolling and manufacturing, characterized in that: The following steps are involved: Step S20, weighing each component according to weight for standby use; Step S21, add the water-based acrylic resin emulsion, defoamer, and thickener into a mixer, shear and mix them evenly at a speed of 2000-3000 r / min, and then let them stand for 1-2 hours to defoam, so as to obtain a water-based adhesive.
Citation Information
Patent Citations
Hydrogel prepared by using grafted modified material as well as preparation method and application of hydrogel
CN108484936A
Method for preparing flame-retardant polymer polyol, application of flame-retardant polymer polyol, and polyurethane foam plastic prepared from flame-retardant polymer polyol
CN112250858A
Preparation method and application of acrylic acid / epsilon-polylysine adhesive antibacterial hydrogel
CN112876694A
Water-based acrylate pressure-sensitive adhesive and preparation method thereof
CN113999632A
Controlled crosslinking of latex polymers with polyfunctional amines
WO2017049025A1