Method for automatically adding cold charge in converter vanadium extraction blowing process

Through the computer secondary static model and automation system, the problem of irregular cold material addition caused by manual operation is solved, the automation and standardization of cold material is realized, and the vanadium recovery rate and technical economy in the converter vanadium extraction process is improved. index.

CN118996037APending Publication Date: 2024-11-22HEBEI IRON AND STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174673.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the vanadium extraction and blowing process of converter, the timing and amount of cold material are not standardized due to manual operations, resulting in large fluctuations in the melt pool temperature, affecting the control of vanadium conversion rate and vanadium extraction end point.

Method used

The secondary static model of the computer is used to calculate the cold material and oxygen supply, and the cold material is distributed to the high-level silo through the automation system. The cold material is distributed according to the oxygen step, and the addition of cold material is controlled by using PLC and automatic procedures to ensure the cold material. evenly and reasonably added.

Benefits of technology

The automation, intelligence and standardization of cold material addition have been achieved, the stability of the melt pool temperature has been improved, the vanadium recovery rate and technical and economic indicators of the vanadium extraction process have been improved, and the semi-steel residual vanadium and temperature hit rate have been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996037A_ABST
    Figure CN118996037A_ABST
Patent Text Reader

Abstract

The invention relates to a method for automatically adding cold charge in the vanadium extraction blowing process of a converter, which comprises the following steps of: distributing the cold charge required in the vanadium extraction process to each high-level bunker, sending data to a primary PLC (Programmable Logic Controller) to execute an automatic control program, and automatically adding the cold charge into the high-level bunker through a set oxygen step, adding proportion of each step and opening and closing time interval of a summary hopper in the vanadium extraction process. And automation, standardization and standardization of cold charge adding are achieved. By means of the method, the problem that the cold charge adding time and adding amount are not standard through traditional manual operation is solved, the adding uniformity and reasonability of the cold charge in the process can be effectively guaranteed, stable control over the temperature of a molten pool is better facilitated, and the method plays an important role in reducing semisteel residual vanadium, increasing the vanadium recovery rate and improving the technical and economic indexes of the vanadium extraction process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present patent application belongs to the technical field of converter vanadium extraction, and more specifically, relates to a method for automatically adding cold material during the converter vanadium extraction blowing process. Background Art

[0002] The converter vanadium extraction is a process of oxidizing the vanadium in the vanadium-containing hot metal into vanadium slag before steelmaking. It is an important method widely used in many hot metal vanadium extraction processes. The converter vanadium extraction process mainly uses an oxygen lance to supply oxygen to the vanadium-containing hot metal in the converter to oxidize the vanadium element to form vanadium slag, and then extract the vanadium element from the vanadium-containing hot metal.

[0003] The vanadium extraction and blowing process in the converter is an exothermic process. The oxidation of the easily oxidizable elements in the molten iron causes the molten pool to heat up rapidly. When the temperature exceeds the carbon-vanadium conversion temperature, the oxidation rate of carbon increases and the oxidation rate of vanadium decreases. Therefore, in order to obtain a high vanadium oxidation rate, a coolant must be added through the silo during the blowing process to control the molten pool temperature within a reasonable range, so as to achieve the purpose of vanadium extraction and carbon preservation and ensure the technical and economic indicators of vanadium extraction.

[0004] At present, vanadium extraction from converters is still basically controlled by manual operation mode. In particular, the temperature of the molten pool fluctuates greatly due to the irregular timing of adding cold materials and the amount of each batch added, which in turn affects the vanadium conversion rate of the vanadium extraction process and the control of the vanadium extraction end point.

[0005] Therefore, it is necessary to find a method to automatically add cold material during the blowing process, and to increase the temperature level of the molten pool during the blowing process by normalizing and standardizing the addition of cold material, thereby ensuring various technical and economic indicators in the vanadium extraction process. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for automatically adding cold material during the converter vanadium extraction blowing process, stably control the temperature of the converter vanadium extraction process, improve vanadium extraction indicators and stabilize semi-steel conditions.

[0007] In order to solve the above problems, the technical solution adopted by the present invention is: A method for automatically adding cold material during the vanadium extraction and blowing process of a converter comprises the following steps: S1. After the vanadium-containing molten iron is added into the converter, the weight of the cold material and the oxygen supply required for vanadium extraction are calculated by the computer secondary static model; S2. The calculated weight of cold material is distributed to each high-level silo of the selected material according to a certain ratio. The weight of cold material distributed to each silo accounts for 5%-50% of the total amount of cold material. The calculated oxygen supply is distributed in different oxygen steps according to the total amount of cold material, and the oxygen steps are divided into 2-4.

[0008] S3. After the secondary model is calculated and the data is sent to the primary PLC, the "material preparation" button is clicked manually or the "material preparation" is carried out according to the automatic program, wherein: the first batch of materials passes through the weighing bucket and enters the two summary buckets for standby, the second batch of materials is placed in the weighing bucket for standby, and the remaining batches of cold materials are temporarily stored in the high-level silo. After the weighing bucket is emptied, the materials are prepared in sequence according to the program; S4. After the oxygen lance starts to supply oxygen, when the cumulative oxygen supply reaches the set oxygen step, the collection bucket starts to open automatically, and the vanadium cold material is added into the converter along the slide pipe. The interval between the opening time of the two collection buckets is 0-40 seconds; S5. After the automatic feeding starts, after the first batch of materials in the summary hopper is added to the converter, the weighing hopper plug valve automatically opens to put the second batch of materials into the summary hopper, and the third batch of materials begins to be automatically prepared until the last batch of materials is added to the converter, completing the automatic feeding.

[0009] Further, in S1, the method is applicable to molten iron conditions where the weight of the cold material is ≤60kg / ton iron, and the type of the vanadium extraction cold material is one or more of pellets, iron balls, iron powder balls, and mixed balls.

[0010] Further, in S2, when the oxygen step is divided into 2 steps, the first batch of materials is added at 30%-40% of the oxygen step, and the second batch of materials is added at 50%-60% of the oxygen step; when the oxygen step is divided into 3 steps, the first batch of materials is added at 10%-15% of the oxygen step, the second batch of materials is added at 30%-35% of the oxygen step, and the third batch of materials is added at 55%-60% of the oxygen step; when the oxygen step is divided into 4 steps, the first batch of materials is added at 5%-10% of the oxygen step, the second batch of materials is added at 20%-25% of the oxygen step, the third batch of materials is added at 40%-45% of the oxygen step, and the fourth batch of materials is added at 55%-60% of the oxygen step.

[0011] Further, in S2, when the oxygen step is divided into 2 steps, the amount of oxygen added to each high-level silo in the first step is 50%-60% of the total amount allocated to the silo, and the amount of oxygen added in the second step is 40%-50% of the total amount allocated to the silo; when the oxygen step is divided into 3 steps, the amount of oxygen added to each high-level silo in the first step is 35%-45% of the total amount allocated to the silo, the amount of oxygen added in the second step is 25%-35% of the total amount allocated to the silo, and the amount of oxygen added in the third step is 15%-25% of the total amount allocated to the silo; when the oxygen step is divided into 4 steps, the amount of oxygen added to each high-level silo in the first step is 30%-40% of the total amount allocated to the silo, the amount of oxygen added in the second step is 25%-35% of the total amount allocated to the silo, the amount of oxygen added in the third step is 20%-30% of the total amount allocated to the silo, and the amount of oxygen added in the fourth step is 10%-20% of the total amount allocated to the silo.

[0012] Furthermore, the number of high-level silos is 2 to 4, and the number of summary buckets is two; when the number of high-level silos is 2, each corresponds to two summary buckets; when the number of high-level silos is greater than 2, the first two silos correspond to 1 summary bucket, and the remaining silos correspond to 1 summary bucket.

[0013] Further, in S2, when the selected high-level silo is deselected, the allocation ratio borne by the silo is evenly distributed to the remaining silos.

[0014] By utilizing the method of the present invention, the hit rate of residual vanadium in semi-steel is ≥95%, the hit rate of semi-steel temperature is ≥93%, and the vanadium recovery rate is ≥75%.

[0015] Due to the adoption of the above technical solution, the beneficial effects achieved by the present invention are: The present invention automatically adds cold material in the vanadium extraction process, thereby changing the problems of irregular timing and amount of adding cold material in the traditional manual operation, improving the accuracy of adding cold material in the blowing process, and realizing the automation, intelligence, standardization and standardization of adding cold material.

[0016] The automatic addition of cold material during the converter vanadium extraction process adapts to different molten iron conditions. Through different oxygen steps and the switching time intervals of the summing bucket gate valve, it can effectively ensure the uniformity and rationality of the addition of cold material in the process, and is more conducive to the stable control of the molten pool temperature. It plays an important role in reducing the residual vanadium in semi-steel, increasing the vanadium recovery rate, and improving the technical and economic indicators of the vanadium extraction process. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is the process route diagram of the present invention. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below with reference to the embodiments.

[0019] A method for automatically adding cold material during the vanadium extraction blowing process in a converter, such as Figure 1 The process / steps shown, After the vanadium-containing molten iron is added to the converter, the computer secondary static model calculates the weight of the cold material and the oxygen supply required for vanadium extraction. The calculated weight of the cold material is distributed to each high-level silo for the selected charging according to a certain ratio, and the weight of the cold material distributed to each high-level silo accounts for 5%-50% of the total amount of cold material; the calculated oxygen supply is distributed in different oxygen steps according to the total amount of cold material, and the oxygen steps are divided into 2-4. The high-level silo here is the silo for storing cold material. Since the location of the silo is above the tower of the workshop, it is generally called a high-level silo.

[0020] After the computer's secondary static model is calculated and the data is sent to the primary PLC, the "material preparation" button is clicked manually or according to the automatic program to carry out "material preparation", in which: the first batch of materials passes through the weighing bucket and enters the two summary buckets for standby, the second batch of materials is placed in the weighing bucket for standby, and the remaining batches of cold materials are temporarily stored in the high-level silo. After the weighing bucket is emptied, the materials are prepared in sequence according to the procedure.

[0021] After the oxygen lance starts supplying oxygen, when the cumulative oxygen supply reaches the set oxygen step, the summing bucket starts to open automatically, and the vanadium cold material is added into the converter along the chute. The interval between the opening time of the two summing buckets is 0-40 seconds. After the automatic feeding starts, after the first batch of materials in the summing bucket is added into the converter, the gate valve of the weighing bucket automatically opens to put the second batch of materials into the summing bucket, and the third batch of materials starts to be automatically prepared until the last batch of materials is added into the converter, and the automatic feeding is completed.

[0022] The number of high-level silos is 2 to 4, and there are two summary buckets; when the number of high-level silos is 2, each corresponds to two summary buckets; when the number of high-level silos is greater than 2, the first two silos correspond to 1 summary bucket, and the remaining silos correspond to 1 summary bucket.

[0023] This method is applicable to molten iron conditions where the weight of the cold material is ≤60kg / ton iron, and the types of the vanadium extraction cold material are one or more of pellets, iron balls, iron powder balls, and mixed balls.

[0024] Since the oxygen step is divided into 2-4 steps, when the oxygen step is divided into 2 steps, the first batch of materials is added at 30%-40% of the oxygen step, and the added amount is 50%-60% of the total amount allocated to the silo; the second batch of materials is added at 50%-60% of the oxygen step, and the added amount is 40%-50% of the total amount allocated to the silo.

[0025] When the oxygen step is divided into three steps, the first batch of materials is added at 10%-15% of the oxygen step, and the amount added is 35%-45% of the total amount allocated to the silo; the second batch of materials is added at 30%-35% of the oxygen step, and the amount added is 25%-35% of the total amount allocated to the silo; the third batch of materials is added at 55%-60% of the oxygen step, and the amount added is 15%-25% of the total amount allocated to the silo.

[0026] When the oxygen step is divided into 4 steps, the first batch of materials is added at 5%-10% of the oxygen step, and the amount added is 30%-40% of the total amount allocated to the silo; the second batch of materials is added at 20%-25% of the oxygen step, and the amount added is 25%-35% of the total amount allocated to the silo; the third batch of materials is added at 40%-45% of the oxygen step, and the amount added is 20%-30% of the total amount allocated to the silo; the fourth batch of materials is added at 55%-60% of the oxygen step, and the amount added is 10%-20% of the total amount allocated to the silo.

[0027] When the selected high-level silo is deselected, the allocation ratio borne by the silo is evenly distributed to the remaining silos.

[0028] From the above description, it can be seen that through this method, the automation, normalization and standardization of cold material addition are realized, the disadvantages of manual material addition are changed, the uniformity and rationality of the addition of cold material in the process are effectively guaranteed, and it is more conducive to the stable control of the molten pool temperature. It plays an important role in reducing the residual vanadium in semi-steel, improving the vanadium recovery rate, and improving the technical and economic indicators of the vanadium extraction process.

[0029] A more specific embodiment of the present invention is provided below: Example

[0030] The production process of the vanadium extraction automatic charging of the present invention is applied to a 150-ton vanadium extraction converter of a certain factory: After the vanadium-containing molten iron is added to the converter, the computer secondary static model calculates that the weight of the cold material required for vanadium extraction is 2300kg and the oxygen supply is 1550m 3 , select 2 high-level silos, each silo is allocated 50% of cold material, corresponding to two summary hoppers, the oxygen step is divided into 2 steps, the first batch of materials is added with 30% of oxygen step, the amount added is 60% of the amount allocated in the silo, the second batch of materials is added with 50% of oxygen step, the amount added is 40% of the amount allocated in the silo. The secondary model starts to prepare materials after transmitting data to the first level, and feeds according to the set program after the oxygen gun is opened. The time interval between the opening of the two summary hoppers is 0 seconds, that is, they are opened and closed at the same time, and the above procedures are followed until the vanadium extraction process is completed and the material is automatically added. The vanadium extraction blowing process is completed, and the semi-steel residual vanadium and semi-steel temperature both hit the target. Example

[0031] The production process of the vanadium extraction automatic charging of the present invention is applied to a 150-ton vanadium extraction converter of a certain factory: After the vanadium-containing molten iron is added to the converter, the computer secondary static model calculates that the weight of the cold material required for vanadium extraction is 4500kg and the oxygen supply is 1600m 3 , select 3 high-level silos, and the proportion of cold material allocated to each silo is 25%, 25%, and 50% respectively. The first two silos correspond to 1 summary bucket, and the remaining silos correspond to 1 summary bucket.

[0032] The oxygen step is divided into 3 steps. The first batch of materials is added with 15% oxygen step, and the added amount is 40% of the allocated amount in the silo. The second batch of materials is added with 35% oxygen step, and the added amount is 35% of the allocated amount in the silo. The third batch of materials is added with 55% oxygen step, and the added amount is 25% of the allocated amount in the silo. The secondary model transmits the data to the first level and starts to prepare materials. After the oxygen gun is opened, the materials are added according to the set program. The time interval between the opening of the two summary buckets is 15 seconds. The cold materials are added at intervals during the process to ensure the uniformity of the cold materials. According to the above procedures, the vanadium extraction process is automatically added until the vanadium extraction process is completed. At the end of the vanadium extraction blowing process, the residual vanadium in the semi-steel and the temperature of the semi-steel are both on target. Example

[0033] The production process of the vanadium extraction automatic charging of the present invention is applied to a 150-ton vanadium extraction converter of a certain factory: After the vanadium-containing molten iron is added to the converter, the computer secondary static model calculates that the weight of the cold material required for vanadium extraction is 9000kg and the oxygen supply is 1680m 3 , select 4 high-level silos, and the proportion of cold material allocated to each silo is 25%, 25%, 25%, and 25% respectively. The first two silos correspond to 1 summary bucket, and the remaining silos correspond to 1 summary bucket.

[0034] The oxygen step is divided into 4 steps. The first batch of materials is added with 5% oxygen step, and the amount added is 30% of the amount allocated in the silo. The second batch of materials is added with 22% oxygen step, and the amount added is 30% of the amount allocated in the silo. The third batch of materials is added with 42% oxygen step, and the amount added is 25% of the amount allocated in the silo. The fourth batch of materials is added with 60% oxygen step, and the amount added is 15% of the amount allocated in the silo. The secondary model transmits the data to the first level and starts to prepare materials. After the oxygen gun is opened, the materials are added according to the set program. The time interval between the opening of the two summary buckets is 40 seconds. The cold materials are added at intervals during the process to ensure the uniformity of the cold materials. According to the above procedures, the vanadium extraction process is automatically added until the vanadium extraction process is completed. The vanadium extraction blowing process is completed, and the semi-steel residual vanadium and semi-steel temperature are both on target. Example

[0035] The production process of the vanadium extraction automatic charging of the present invention is applied to a 150-ton vanadium extraction converter of a certain factory: After the vanadium-containing molten iron is added into the converter, the computer secondary static model calculates that the weight of cold material required for vanadium extraction is 8500kg, the oxygen supply is 1580m3, and the original plan for selecting high-level silos is 4. The proportion of cold material allocated to each high-level silo is 30%, 20%, 30%, and 20%, respectively. The first two high-level silos correspond to 1 summary hopper, and the remaining high-level silos correspond to 1 summary hopper. Affected by the failure of the first high-level silo, the high-level silo is reselected and the selection of the first high-level silo is cancelled. The 30% cold material addition borne by the first high-level silo is automatically and evenly distributed to other high-level silos. The proportion of cold material allocated to each high-level silo is 30%, 40%, and 30%, respectively. The first high-level silo corresponds to 1 summary hopper, and the remaining high-level silos correspond to 1 summary hopper.

[0036] The oxygen step is divided into 4 steps. The first batch of materials is added with 6% oxygen step, which is 32% of the allocated amount in the silo. The second batch of materials is added with 23% oxygen step, which is 28% of the allocated amount in the silo. The third batch of materials is added with 43% oxygen step, which is 24% of the allocated amount in the silo. The fourth batch of materials is added with 58% oxygen step, which is 16% of the allocated amount in the silo. The secondary model starts to prepare materials after transmitting data to the first level. After the oxygen gun is opened, the materials are added according to the set program. The time interval between the opening of the two summary buckets is 18 seconds. The cold materials are added at intervals during the process to ensure the uniformity of the cold materials. According to the above procedures, the vanadium extraction process is automatically added until the vanadium extraction process is completed. The vanadium extraction blowing process is completed, and the semi-steel residual vanadium and semi-steel temperature are both on target.

[0037] Comparative Example: To further illustrate the beneficial effects of the present invention, the semi-steel index of the end point after vanadium extraction by the method of manual feeding and automatic feeding is compared, and the results are shown in the following table:

[0038] Compared with manual feeding in the vanadium extraction process, the method of the present invention increases the hit rate of residual vanadium in semi-steel by 9.1%, the hit rate of semi-steel temperature by 10.9%, and the vanadium recovery rate by 3.5%, thereby effectively improving the technical and economic indicators of the vanadium extraction process.

Claims

1. A method for automatically adding cold material during the vanadium extraction and blowing process in a converter. Features The steps include: S1. After the vanadium-containing molten iron is added into the converter, the amount of cold material added and the amount of oxygen supplied required for vanadium extraction are calculated by the computer secondary static model. The amount of cold material added is the weight of the cold material; S2. The calculated weight of cold material is distributed to each high-level material bin of the selected material according to a certain proportion. The weight of cold material distributed to each high-level material bin accounts for 5% to 50% of the total amount of cold material. The calculated oxygen supply is distributed in different oxygen steps according to the total amount of cold material, and the oxygen steps are divided into 2 to 4 steps. S3. After the computer secondary static model is calculated and the data is sent to the primary PLC, the "material preparation" button is clicked manually or the "material preparation" is carried out according to the automatic program, wherein: the first batch of materials passes through the weighing bucket and enters the two summary buckets for standby, the second batch of materials is placed in the weighing bucket for standby, and the remaining batches of cold materials are temporarily stored in the high-level silo. After the weighing bucket is emptied, the materials are prepared in sequence according to the program; S4. After the oxygen lance starts to supply oxygen, when the cumulative oxygen supply reaches the set oxygen step, the collection bucket starts to open automatically, and the vanadium cold material is added into the converter along the chute. The time interval between the opening of the two collection buckets is 0 to 40 seconds; S5. Automatically add cold materials in batches: After the automatic feeding starts, after the first batch of materials in the summary bucket is added to the converter, the gate valve of the weighing bucket automatically opens to put the second batch of materials into the summary bucket, and the third batch of materials begins to be automatically prepared until the last batch of materials is added to the converter, completing the automatic feeding.

2. The method for automatically adding cold material during the vanadium extraction and blowing process of a converter according to claim 1, Features: In S1, it is applicable to the molten iron condition that the weight of cold material is ≤60kg / ton iron, and the type of cold material required for vanadium extraction is one or more of pellets, iron balls, iron powder balls, and mixed balls.

3. The method for automatically adding cold material during the vanadium extraction and blowing process of a converter according to claim 2, Features: In S2, the oxygen step is divided into 2 to 4 steps, specifically: When the oxygen step is divided into two steps, the first batch is added at 30%-40% of the oxygen step, and the second batch is added at 50%-60% of the oxygen step; When the oxygen step is divided into three steps, the first batch is added at 10%-15% of the oxygen step, the second batch is added at 30%-35% of the oxygen step, and the third batch is added at 55%-60% of the oxygen step; When the oxygen step is divided into 4 steps, the first batch of materials is added at 5%-10% of the oxygen step, the second batch of materials is added at 20%-25% of the oxygen step, the third batch of materials is added at 40%-45% of the oxygen step, and the fourth batch of materials is added at 55%-60% of the oxygen step.

4. The method for automatically adding cold material during vanadium extraction and blowing in a converter according to claim 2, Features: When the oxygen step is divided into two steps, the amount of oxygen added to each high-level silo in the first step is 50%-60% of the total amount allocated to the silo, and the amount of oxygen added in the second step is 40%-50% of the total amount allocated to the silo; When the oxygen step is divided into three steps, the amount of oxygen added to each high-level silo in the first step is 35%-45% of the total amount allocated to the silo, the amount of oxygen added in the second step is 25%-35% of the total amount allocated to the silo, and the amount of oxygen added in the third step is 15%-25% of the total amount allocated to the silo; When the oxygen step is divided into 4 steps, the amount of oxygen added to each high-level silo in the first step is 30%-40% of the total amount allocated to the silo, the amount of oxygen added in the second step is 25%-35% of the total amount allocated to the silo, the amount of oxygen added in the third step is 20%-30% of the total amount allocated to the silo, and the amount of oxygen added in the fourth step is 10%-20% of the total amount allocated to the silo.

5. The method for automatically adding cold material during the vanadium extraction and blowing process of a converter according to claim 1, Features: The number of high-level silos is 2 to 4, and there are two summary buckets; when the number of high-level silos is 2, each corresponds to two summary buckets; when the number of high-level silos is greater than 2, the first two silos correspond to 1 summary bucket, and the remaining silos correspond to 1 summary bucket.

6. A method for automatically adding cold material during vanadium extraction and blowing in a converter according to any one of claims 1 to 5, Features: When the selected high-level silo is deselected, the allocation ratio borne by the silo is evenly distributed to the remaining high-level silos.

7. The method for automatically adding cold material during the vanadium extraction and blowing process of a converter according to claim 6, Features: The hit rate of residual vanadium in semi-steel is ≥95%, the hit rate of semi-steel temperature is ≥93%, and the vanadium recovery rate is ≥75%.