Mn-Cu series high-damping alloy for vibration and noise reduction and preparation method of Mn-Cu series high-damping alloy

By adding Cr elements to Mn-Cu high-damping alloy and optimizing casting and heat treatment processes, the problems of poor strength and damping performance of Mn-Cu alloy are solved, and the high damping performance and strength of the alloy are improved, suitable for reducing Oscillation noise reduction.

CN118996216APending Publication Date: 2024-11-22SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411101084.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing Mn-Cu alloys have low strength, damping properties and martensite transition temperature, which limit their use in practical engineering applications.

Method used

Cr elements are added to the Mn-Cu high-damping alloy to increase the martensite transition temperature of the alloy. Through casting method and heat treatment process optimization, an alloy with high damping performance and strength was prepared.

Benefits of technology

By adding Cr elements, the damping performance and strength of the alloy are significantly improved, suitable for vibration and noise reduction, reducing vibration and noise of industrial equipment, and reducing harm to human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996216A_ABST
    Figure CN118996216A_ABST
Patent Text Reader

Abstract

The invention discloses a Mn-Cu series high-damping alloy for vibration and noise reduction and a preparation method of the Mn-Cu series high-damping alloy, and belongs to the technical field of high-damping alloys. The Mn-Cu series high-damping alloy for vibration and noise reduction comprises the following raw materials in percentage by mass: 20%-25% of Cu, 5.0%-5.5% of Ni, 1.5%-2.5% of Fe, 0.3%-0.5% of Cr and the balance of Mn. According to the Mn-Cu series high-damping alloy for vibration and noise reduction and the preparation method of the Mn-Cu series high-damping alloy, the required raw materials are low in cost, the preparation method is simple in process, and production is easy; the Cr element is added, so that the martensite transformation temperature of the alloy is effectively increased, alloy martensite transformation is facilitated, alloy amplitude modulation decomposition is promoted, the damping performance of the alloy is improved, and when the alloy is applied to modern industrial equipment, vibration and noise can be effectively reduced, and harm to body health of people is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high damping alloys, and in particular to a Mn-Cu series high damping alloy for vibration and noise reduction and a preparation method thereof. Background Art

[0002] In modern production and life with the rapid development of science and technology, the noise generated by the vibration of mechanical equipment has seriously affected people's normal production and life. At the same time, being in a high-noise environment for a long time will have a serious adverse impact on human health. Therefore, how to reduce the noise of mechanical equipment has become a problem that people are paying more and more attention to. There are three main ways to reduce noise in industrial production: First, strengthen the vibrating components in the machinery to achieve the effect of suppressing noise. Second, install sound insulation devices to block the spread of noise. Third, use damping materials in machinery to achieve noise reduction. Among them, damping materials refer to a class of materials with special physical properties that convert mechanical vibration energy into heat energy and dissipate it. In the field of vibration reduction and noise reduction, compared with the traditional method of strengthening components to suppress vibration and reduce noise or installing sound insulation devices, the use of damping materials in machinery can achieve better vibration reduction and noise reduction effects at a lower cost without increasing the weight of the machinery. Damping alloys also have the ability to serve under high temperature and high pressure harsh working conditions, and good mechanical properties and high damping properties have broad prospects.

[0003] The damping capacity of Mn-Cu based alloys is mainly attributed to the movement of twins and the phase boundary between the parent phase and martensite. Its damping mechanism is significantly different from other types of damping alloys. The current mainstream view is that Mn-Cu based damping alloys form a spinodal decomposition structure composed of manganese-rich and copper-rich regions due to the occurrence of spinodal decomposition, and the FCC-FCT phase transition temperature in the alloy is linearly related to the Mn content. Therefore, current research is mainly focused on increasing the phase transition temperature of the alloy through alloying and heat treatment processes, so as to make the alloy have a large number of twins at room temperature, and ultimately achieve the effect of improving the damping capacity of the alloy.

[0004] However, the strength, damping properties, martensitic transformation temperature, etc. of Mn-Cu alloys are currently far behind those of other Cu-based alloys, which greatly limits the use of Mn-Cu alloys in practical engineering applications. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a Mn-Cu series high damping alloy for vibration and noise reduction and a preparation method thereof, so as to solve the problems of poor strength and damping performance, low martensitic transformation temperature and other problems of existing Mn-Cu alloys.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] A Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following raw materials in mass percentage: 20-25% Cu, 5.0-5.5% Ni, 1.5-2.5% Fe and 0.3-0.5% Cr, and the balance is Mn.

[0008] The beneficial effects of the present invention are as follows: the present invention adds Cr element to the high manganese Mn-Cu alloy to increase the martensitic transformation temperature of the alloy, which is more conducive to the martensitic transformation of the alloy and further promotes the spinodal decomposition of the alloy, thereby improving the damping performance and strength of the alloy.

[0009] Further, the raw materials include the following mass percentages: 22.3% Cu, 5.2% Ni, 2% Fe and 0.4% Cr, and the balance is Mn.

[0010] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0011] The raw materials are first mixed, smelted and refined in sequence, then cast and molded for homogenization heat treatment, and finally forged and annealed to obtain the product.

[0012] The beneficial effects of the present invention are as follows: the present invention adopts a casting method to prepare the Mn-Cu series high damping alloy, the preparation method has a simple process and is easy to be industrialized on a large scale.

[0013] Furthermore, the smelting power is 28-32 kW and the smelting time is 30-50 min.

[0014] Preferably, the smelting power is 32 kW and the smelting time is 40 min.

[0015] The beneficial effect of adopting the above further technical solution is that the present invention performs preliminary smelting on the raw materials so that the raw materials are fully melted into liquid state, which facilitates subsequent alloy processing and improves the uniformity of the alloy components.

[0016] Furthermore, the refining power is 18-24 kW and the refining time is 10-15 min.

[0017] Preferably, the refining power is 20 kW and the refining time is 10 min.

[0018] The beneficial effect of adopting the above further technical solution is that the present invention further refines the smelted product by reducing the power, thereby effectively ensuring the uniformity of each component in the alloy.

[0019] Furthermore, foam-like refractory ceramics are used as filters during the casting process, and rare gases are used for protection.

[0020] The beneficial effect of adopting the above further technical solution is: the present invention adopts foam-like refractory ceramics as the filter sheet, so that the prepared alloy has fewer impurities, which is beneficial to improving the damping performance of the alloy.

[0021] Furthermore, the temperature of the homogenization heat treatment is 1100-1200° C., and the time is 10-20 hours.

[0022] Preferably, the temperature of the homogenization heat treatment is 1150° C. and the time is 15 h.

[0023] Furthermore, the starting forging temperature of the forging is 800-850°C, and the ending forging temperature is 600-650°C.

[0024] Preferably, the starting forging temperature of forging is 820°C and the ending forging temperature is 620°C.

[0025] Furthermore, the annealing heat treatment conditions are: first heat treatment at 800-1000°C for 30-90 minutes, then air cooling to room temperature, and finally heating to 350-450°C for 1-6 hours, and air cooling to room temperature.

[0026] Preferably, the annealing heat treatment conditions are: first heat treatment at 900° C. for 60 min, then air cooling to room temperature, and finally heating to 400° C. for 2 h, and air cooling to room temperature.

[0027] The beneficial effect of adopting the above-mentioned further technical solution is as follows: the present invention performs homogenization heat treatment and annealing heat treatment on the metal ingots before and after forging, and improves and optimizes the heat treatment conditions, thereby effectively improving the uniformity of the structure and composition of the obtained alloy, and improving the strength and damping performance of the alloy.

[0028] The above-mentioned Mn-Cu series high damping alloy for vibration and noise reduction is used in reducing vibration and noise in industry.

[0029] The present invention has the following beneficial effects:

[0030] The invention provides a Mn-Cu series high damping alloy for vibration and noise reduction and a preparation method thereof. The raw material cost required is low, the preparation method is simple and easy to produce. The martensitic transformation temperature of the alloy is effectively increased by adding the Cr element, which is more conducive to the martensitic transformation of the alloy and further promotes the amplitude modulation decomposition of the alloy, thereby improving the damping performance of the alloy. The alloy can be applied to modern industrial equipment to effectively reduce vibration and noise, and reduce the harm to people's health. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The loss factor of the Mn-Cu high damping alloys prepared in Example 1 and Comparative Example 1 varies with strain amplitude;

[0032] Figure 2 The loss factor of the Mn-Cu high damping alloys prepared in Example 2 and Comparative Example 2 varies with strain amplitude;

[0033] Figure 3 The loss factor of the Mn-Cu high damping alloys prepared in Example 3 and Comparative Example 3 varies with strain amplitude;

[0034] Figure 4 The DSC curve of the Mn-Cu high damping alloy prepared in Comparative Example 2-4 during the cooling process;

[0035] Figure 5 This is the DSC curve of the Mn-Cu high damping alloy obtained in Example 2-4 during the cooling process. DETAILED DESCRIPTION

[0036] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] Embodiment 1:

[0038] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in percentage by mass: 22.3% Cu, 5.2% Ni, 2% Fe and 0.4% Cr, with the balance being Mn.

[0039] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0040] (1) Preparation of a new crucible: Use magnesia sand and water glass to install the crucible on the induction coil, then coat the outermost layer and the pouring mouth with refractory cement, and finally dry it to make a new crucible.

[0041] (2) Charging: The weighed raw materials are loaded into a crucible installed in a ZG-25 vacuum induction melting furnace.

[0042] (3) Melting: Open the mechanical pump, bottom valve and Roots pump in sequence to evacuate the vacuum, increase the power of the vacuum induction melting furnace to 30 kW, and melt for 40 minutes to fully melt the raw materials into liquid.

[0043] (4) Refining: Refining the smelted material, reducing the power of the vacuum induction furnace to 18 kW, and refining for 10 minutes to make the components uniform.

[0044] (5) Casting: Open the argon flushing valve to fill the vacuum induction furnace with argon gas, and cast the molten mixture under the protection of argon gas. During the casting process, use foam refractory ceramics (Baoding Ningxin Group Co., Ltd.) as a filter, and slowly reduce the power until the casting process is completed and the power drops to zero.

[0045] (6) Homogenization heat treatment: The ingot obtained after casting is kept at 1150°C for 15 hours for homogenization heat treatment to obtain a cast alloy with uniform structure and composition.

[0046] (7) Forging: The cast alloy obtained in step (6) is forged, with the initial forging temperature being 820°C and the final forging temperature being 620°C.

[0047] (8) Annealing heat treatment: The alloy forged in step (7) was heat treated at 900°C for 1 hour, then air-cooled to room temperature, and finally heated to 400°C for 1 hour, and air-cooled to room temperature to obtain a Mn-Cu high damping alloy for vibration and noise reduction, named 0.4Cr-1h.

[0048] Embodiment 2:

[0049] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni, 2% Fe and 0.4% Cr, with the balance being Mn.

[0050] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0051] The preparation method is the same as that of Example 1, except that the holding time of heating to 400°C in step (8) is changed to 2 hours, and a Mn-Cu high damping alloy for vibration and noise reduction is obtained, which is named 0.4Cr-2h.

[0052] Embodiment 3:

[0053] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni, 2% Fe and 0.4% Cr, with the balance being Mn.

[0054] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0055] The preparation method is the same as that of Example 1, except that the holding time of heating to 400°C in step (8) is changed to 4 hours, and a Mn-Cu high damping alloy for vibration and noise reduction is obtained, which is named 0.4Cr-4h.

[0056] Embodiment 4:

[0057] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni, 2% Fe and 0.4% Cr, with the balance being Mn.

[0058] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0059] The preparation method is the same as that of Example 1, except that the holding time of heating to 400°C in step (8) is changed to 6 hours, and a Mn-Cu high damping alloy for vibration and noise reduction is obtained, which is named 0.4Cr-6h.

[0060] Embodiment 5:

[0061] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 21.3% Cu, 5.5% Ni, 2.5% Fe and 0.4% Cr, with the balance being Mn.

[0062] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0063] (1) Preparation of a new crucible: Use magnesia sand and water glass to install the crucible on the induction coil, then coat the outermost layer and the pouring mouth with refractory cement, and finally dry it to make a new crucible.

[0064] (2) Charging: The weighed raw materials are loaded into a crucible installed in a ZG-25 vacuum induction melting furnace.

[0065] (3) Melting: Open the mechanical pump, bottom valve and Roots pump in sequence to evacuate the vacuum, increase the power of the vacuum induction melting furnace to 32 kW, and melt for 30 minutes to fully melt the raw materials into liquid.

[0066] (4) Refining: Refining the smelted material, reducing the power of the vacuum induction furnace to 24 kW, and refining for 10 minutes to make the components uniform.

[0067] (5) Casting: Open the argon flushing valve to fill the vacuum induction furnace with argon gas, and cast the molten mixture under the protection of argon gas. During the casting process, use foam refractory ceramics (Baoding Ningxin Group Co., Ltd.) as a filter, and slowly reduce the power until the casting process is completed and the power drops to zero.

[0068] (6) Homogenization heat treatment: The ingot obtained after casting is kept at 1100°C for 18 hours for homogenization heat treatment to obtain a cast alloy with uniform structure and composition.

[0069] (7) Forging: The cast alloy obtained in step (6) is forged, with the initial forging temperature being 850°C and the final forging temperature being 650°C.

[0070] (8) Annealing heat treatment: The alloy forged in step (7) is heat treated at 950°C for 1 hour, then air-cooled to room temperature, and finally heated to 400°C for 2 hours, and air-cooled to room temperature to obtain a Mn-Cu high damping alloy for vibration and noise reduction.

[0071] Embodiment 6:

[0072] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 23.3% Cu, 5.0% Ni, 1.5% Fe and 0.4% Cr, with the balance being Mn.

[0073] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0074] (1) Preparation of a new crucible: Use magnesia sand and water glass to install the crucible on the induction coil, then coat the outermost layer and the pouring mouth with refractory cement, and finally dry it to make a new crucible.

[0075] (2) Charging: The weighed raw materials are loaded into a crucible installed in a ZG-25 vacuum induction melting furnace.

[0076] (3) Melting: Open the mechanical pump, bottom valve and Roots pump in sequence to evacuate the vacuum, increase the power of the vacuum induction melting furnace to 28 kW, and melt for 50 minutes to fully melt the raw materials into liquid.

[0077] (4) Refining: Refining the smelted material, reducing the power of the vacuum induction furnace to 20 kW, and refining for 10 minutes to make the components uniform.

[0078] (5) Casting: Open the argon flushing valve to fill the vacuum induction furnace with argon gas, and cast the molten mixture under the protection of argon gas. During the casting process, use foam refractory ceramics (Baoding Ningxin Group Co., Ltd.) as a filter, and slowly reduce the power until the casting process is completed and the power drops to zero.

[0079] (6) Homogenization heat treatment: The ingot obtained after casting is kept at 1100°C for 12 hours for homogenization heat treatment to obtain a cast alloy with uniform structure and composition.

[0080] (7) Forging: The cast alloy obtained in step (6) is forged, with the initial forging temperature being 800°C and the final forging temperature being 600°C.

[0081] (8) Annealing heat treatment: The alloy forged in step (7) is heat treated at 850°C for 1 hour, then air-cooled to room temperature, and finally heated to 400°C for 2 hours, and air-cooled to room temperature to obtain a Mn-Cu high damping alloy for vibration and noise reduction.

[0082] Comparative Example 1:

[0083] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni and 2% Fe, with the balance being Mn.

[0084] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0085] (1) Preparation of a new crucible: Use magnesia sand and water glass to install the crucible on the induction coil, then coat the outermost layer and the pouring mouth with refractory cement, and finally dry it to make a new crucible.

[0086] (2) Charging: The weighed raw materials are loaded into a crucible installed in a ZG-25 vacuum induction melting furnace.

[0087] (3) Melting: Open the mechanical pump, bottom valve and Roots pump in sequence to evacuate the vacuum, increase the power of the vacuum induction melting furnace to 30 kW, and melt for 40 minutes to fully melt the raw materials into liquid.

[0088] (4) Refining: Refining the smelted material, reducing the power of the vacuum induction furnace to 18 kW, and refining for 10 minutes to make the components uniform.

[0089] (5) Casting: Open the argon flushing valve to fill the vacuum induction furnace with argon gas, and cast the molten mixture under the protection of argon gas. During the casting process, use foam refractory ceramics (Baoding Ningxin Group Co., Ltd.) as a filter, and slowly reduce the power until the casting process is completed and the power drops to zero.

[0090] (6) Homogenization heat treatment: The ingot obtained after casting is kept at 1150°C for 15 hours for homogenization heat treatment to obtain a cast alloy with uniform structure and composition.

[0091] (7) Forging: The cast alloy obtained in step (6) is forged, with the initial forging temperature being 820°C and the final forging temperature being 620°C.

[0092] (8) Annealing heat treatment: The alloy forged in step (7) was heat treated at 900°C for 1 h, then air-cooled to room temperature, and finally heated to 400°C for 1 h, and air-cooled to room temperature to obtain a Mn-Cu high damping alloy for vibration and noise reduction, named M2052-1 h.

[0093] Comparative Example 2:

[0094] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni and 2% Fe, with the balance being Mn.

[0095] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0096] The preparation method is the same as that of comparative example 1, except that the holding time of heating to 400°C in step (8) is changed to 2h, and a Mn-Cu high damping alloy for vibration reduction and noise reduction is obtained, which is named M2052-2h.

[0097] Comparative Example 3:

[0098] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni and 2% Fe, with the balance being Mn.

[0099] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0100] The preparation method is the same as that of comparative example 1, except that the holding time of heating to 400°C in step (8) is changed to 4 hours, and a Mn-Cu high damping alloy for vibration reduction and noise reduction is obtained, which is named M2052-4h.

[0101] Comparative Example 4:

[0102] A Mn-Cu series high damping alloy for vibration and noise reduction comprises the following raw materials in the following mass percentages: 22.3% Cu, 5.2% Ni and 2% Fe, with the balance being Mn.

[0103] The preparation method of the above-mentioned Mn-Cu series high damping alloy for vibration reduction and noise reduction comprises the following steps:

[0104] The preparation method is the same as that of comparative example 1, except that the holding time of heating to 400°C in step (8) is changed to 6 hours, and a Mn-Cu high damping alloy for vibration reduction and noise reduction is obtained, which is named M2052-6 h.

[0105] Test example:

[0106] The alloys prepared in Examples 1-4 and Comparative Examples 1-4 were characterized, and the change curves of their loss factors with strain amplitude were measured, and DSC tests were performed.

[0107] The experimental results are as follows Figure 1-Figure 5 shown.

[0108] From the curve of the change of loss factor with strain amplitude, it can be seen that the alloys prepared in Examples 1-3 significantly improve the damping performance of the alloys by adding Cr to the Mn-Cu damping alloy. According to the DSC test results, the martensitic transformation temperature of the alloys prepared in Examples 2-4 is significantly increased. The results show that by adding Cr elements to the Mn-Cu damping alloy system, the martensitic transformation temperature of the alloy is increased, which is more conducive to the martensitic transformation of the alloy and thus promotes the alloy amplitude modulation decomposition and improves the damping performance.

[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A Mn-Cu high damping alloy for vibration and noise reduction, characterized in that: The invention comprises the following raw materials in percentage by mass: 20-25% Cu, 5.0-5.5% Ni, 1.5-2.5% Fe and 0.3-0.5% Cr, and the balance is Mn.

2. The Mn-Cu series high damping alloy for vibration and noise reduction according to claim 1, characterized in that: The raw materials include the following mass percentages: 22.3% Cu, 5.2% Ni, 2% Fe and 0.4% Cr, and the balance is Mn.

3. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 1 or 2, characterized in that: The following steps are involved: The raw materials are first mixed, then smelted and refined in sequence, then cast and molded for homogenization heat treatment, and finally forged and annealed to obtain the product.

4. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 3, characterized in that: The smelting power is 28-32 kW and the smelting time is 30-50 min.

5. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 3, characterized in that: The refining power is 18-24 kW and the refining time is 10-15 min.

6. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 3, characterized in that: In the casting process, foam-like refractory ceramics are used as filter sheets, and rare gas is used for protection.

7. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 3, characterized in that: The temperature of the homogenization heat treatment is 1100-1200° C. and the time is 10-20 hours.

8. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 3, characterized in that: The starting forging temperature of the forging is 800-850°C, and the ending forging temperature is 600-650°C.

9. The method for preparing the Mn-Cu series high damping alloy for vibration and noise reduction according to claim 3, characterized in that: The annealing heat treatment conditions are: first heat treatment at 800-1000° C. for 30-90 min, then air cooling to room temperature, and finally heating to 350-450° C. for 1-6 h, and air cooling to room temperature.

10. Use of the Mn-Cu series high damping alloy for vibration and noise reduction as claimed in claim 1 or 2 in reducing vibration and noise in industry.