30CrMnSi steel and temperature-controlled quenching heat treatment production method
Through the 30CrMnSi steel temperature-controlled quenching process, segmented quenching and tempering treatment are adopted to solve the problems of large deformation of workpieces and coarse grains in traditional processes, and efficient production and optimized mechanical properties are achieved, energy consumption and cost are reduced, and energy consumption and cost are improved. The comprehensive performance of the material.
Patent Information
- Application Number
- CN202411067031.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
The traditional reheating and quenching process produces 30CrMnSi steel workpieces with large deformation, many processes, long manufacturing cycles and high costs. The direct quenching process is prone to problems such as low surface hardness of the workpiece, a large amount of residual austenite in the seepage layer, and coarse surface grains.
The heat treatment production method adopts the temperature-controlled quenching of 30CrMnSi steel, including forging, reheating, oil-cooled-water-oil-cooled segmented quenching and tempering steps, and controls the cooling speed and Temperature, optimize grain structure, reduce internal stress, and improve material toughness.
Shorten the offline secondary heating time of steel, reduce energy consumption and production cycle, improve production efficiency, optimize internal grain structure, avoid coarse grains, and improve the comprehensive mechanical properties of the material. The obtained 30CrMnSi steel has good strength and toughness.
Smart Images

Figure CN118996253A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel manufacturing, and in particular to a 30CrMnSi steel and a heat treatment production method for temperature-controlled quenching. Background Art
[0002] 30CrMnSi steel is a low-alloy structural steel with high strength and toughness. It has high strength and toughness and has been widely used in the production and manufacturing of military and civilian parts, and is often used to manufacture important parts.
[0003] At present, the traditional reheating quenching process is widely used at home and abroad to produce 30CrMnSi steel. When this process is used, the workpiece is greatly deformed, there are many processes, the manufacturing cycle is long, and the cost is high. Compared with the traditional reheating quenching process, the direct quenching process after forging eliminates the reheating process of the workpiece, simplifies the process flow, reduces production costs, and improves the utilization rate of online heat treatment equipment. However, compared with reheating quenching, direct quenching is prone to the following problems: the surface hardness of the workpiece is slightly lower; the amount of residual austenite in the carburized layer is large; the surface grains are coarse.
[0004] To this end, the present invention is specially proposed to solve the above-mentioned technical problems. Summary of the invention
[0005] The object of the present invention is to provide a 30CrMnSi steel, which contains, by weight percentage, 0.27% to 0.34% C, 0.90% to 1.20% Si, 0.80% to 1.10% Mn, 0.80% to 1.10% Cr, and the balance is Fe.
[0006] Preferably, it contains, by weight percentage: 0.27% C, 0.90% Si, 0.80% Mn, 0.90% Cr, and the balance is Fe.
[0007] A heat treatment production method for temperature-controlled quenching of 30CrMnSi steel comprises the following steps:
[0008] (1) Forging billet: 30CrMnSi steel is smelted and cast into an ingot according to its composition, and the ingot is forged into a forging billet;
[0009] (2) Reheating: Cool the forging billet with air and then heat it in a furnace;
[0010] (3) Quenching: The forging blank is quenched to room temperature by oil cooling, water cooling and oil cooling;
[0011] (4) Tempering: Air cool the forging to room temperature.
[0012] Preferably, the ingot in step (1) is forged into a forging blank at 1200-1250°C.
[0013] Preferably, in step (2), the forging blank is air-cooled to 550°C±50°C, placed in a furnace and heated to 900±10°C, and kept at this temperature for half an hour.
[0014] Preferably, the oil-cooling-water-cooling-oil-cooling staged quenching process is: oil cooling to 600-650° C. in the first stage, water cooling to 350-400° C. in the second stage, and oil cooling to room temperature in the third stage.
[0015] Preferably, the oil cooling speed in the first stage and the third stage is controlled to be 10-15° C. / s.
[0016] Preferably, the water cooling rate of the second stage is controlled to be 40-50°C / s.
[0017] Preferably, the water-cooled quenching liquid is brine, and the oil-cooled quenching liquid is mineral oil.
[0018] Preferably, the forging blank in step (4) is kept at 570-630° C. for 2-3 hours and then air-cooled to room temperature.
[0019] The beneficial effects of the present invention are:
[0020] 1. Compared with the traditional reheating quenching process, the present invention shortens the offline secondary heating time of steel, reduces the energy consumption of heat treatment production by 40%, shortens the heat treatment production cycle by 40%, greatly improves the production efficiency, and achieves the effect of energy saving and consumption reduction. Compared with the direct quenching process after forging, the internal grain structure of the forging can be optimized before quenching, avoiding the coarse grain situation caused by direct quenching, and finally obtaining 30CrMnSi steel with good comprehensive mechanical properties;
[0021] 2. The quenching of the present invention adopts oil cooling and water cooling in stages. The oil cooling speed is slow and the water cooling speed is fast. Oil cooling to 600-650°C first can effectively avoid the huge quenching stress caused by excessive cooling speed. The temperature between 350-650°C is the most unstable area of supercooled austenite, so water cooling is performed for rapid cooling; below 350°C is the martensitic transformation area, oil cooling is performed for slow cooling, which reduces the organizational stress generated during the martensitic transformation.
[0022] 3. The present invention sets the tempering temperature to 570-630°C, which is high-temperature tempering, and can improve the low plasticity and low toughness problems caused by forging. Fine needle-shaped martensite and a small amount of ferrite are obtained by temperature-controlled quenching after forging. The tempering treatment can precipitate carbides to obtain fine tempered troostite + a small amount of ferrite, which reduces internal stress and increases the toughness of the material, and finally obtains 30CrMnSi steel with good comprehensive mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1This is a quenching metallographic structure diagram of 30CrMnSi steel of the present invention;
[0024] Figure 2 This is a tempering metallographic structure diagram of 30CrMnSi steel according to the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0026] The 30CrMnSi steel of the present invention comprises C, Si, Mn, Cr and Fe, as shown in Table 1 in terms of weight percentage:
[0027] Table 1
[0028]
[0029] One embodiment of the present invention is: heat treatment is directly performed on 30CrMnSi steel after forging, and the heat treatment method comprises the following steps:
[0030] (1) Forging billet: According to the composition of 30CrMnSi steel, it is smelted and cast into an ingot, and the ingot is forged into a forging billet at 1200-1250°C;
[0031] (2) Reheating: Cool the forging billet with air and then heat it in a furnace;
[0032] (3) Quenching: The forging blank is quenched to room temperature by oil cooling, water cooling and oil cooling;
[0033] (4) Tempering: Air cool the forging to room temperature.
[0034] Another embodiment of the present invention: reheating is to first air-cool the forging billet to 550°C±50°C, then charge the forging billet into a furnace and raise the temperature to 900±10°C, and keep the temperature for half an hour.
[0035] Another embodiment of the present invention: The process of oil cooling-water cooling-oil cooling segmented quenching is: in the first stage, oil cooling to 600-650°C, the cooling rate is controlled to 10-15°C / s, in the second stage, water cooling to 350-400°C, the cooling rate is controlled to 40-50°C / s, and in the third stage, oil cooling to room temperature, the cooling rate is controlled to 10-15°C / s.
[0036] The water-cooled quenching liquid is salt water, the oil-cooled quenching liquid is mineral oil, the water-cooled cooling speed is controlled at 40-50°C / s, and the oil-cooled cooling speed is 10-15°C / s.
[0037] Another embodiment of the present invention: during the tempering process, the forging blank is kept at 570-630° C. for 2-3 hours and then air-cooled to room temperature.
[0038] According to the method of directly heat treating 30CrMnSi steel after forging in the above embodiment, the 100 mm thick steel material was subjected to tensile test and impact test, and mechanical property test, as shown in Table 2:
[0039] Table 2
[0040]
[0041]
[0042]
[0043] Wherein, T in Table 2 is the thickness of the forging blank.
[0044] The present invention optimizes the internal grain structure of the forging before quenching to avoid the coarse grains caused by direct quenching. In addition, the quenching is processed in stages using oil cooling and water cooling, with a slow oil cooling rate and a faster water cooling rate. Oil cooling to 600-650°C is first performed to avoid excessive cooling rate and produce huge quenching stress; between 350-650°C is the most unstable area of supercooled austenite, so water cooling is performed for rapid cooling; below 350°C is the martensite transformation area, and oil cooling is performed for slow cooling, which reduces the organizational stress generated during martensite transformation. The tempering temperature is set to 570-630°C, which is high temperature tempering, which can improve the problems of low plasticity and low toughness caused by forging. Fine needle-shaped martensite + a small amount of ferrite is obtained by temperature-controlled quenching after forging. Tempering treatment can make carbides precipitate, obtain fine tempered troostite + a small amount of ferrite, reduce internal stress, increase the toughness of the material, and finally obtain 30CrMnSi steel with good comprehensive mechanical properties. Among them, the steel with the composition of 0.27% C, 0.90% Si, 0.80% Mn, 0.90% Cr and the balance of Fe has the best comprehensive performance. Figure 1 and 2 This is the quenched and tempered metallographic structure of the steel obtained with this component.
[0045] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed in the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A 30CrMnSi steel, characterized in that: It contains, by weight percentage: 0.27% to 0.34% C, 0.90% to 1.20% Si, 0.80% to 1.10% Mn, 0.80% to 1.10% Cr, and the balance is Fe.
2. A 30CrMnSi steel according to claim 1, characterized in that: Contains by weight: 0.27% C, 0.90% Si, 0.80% Mn, 0.90% Cr, and the balance is Fe.
3. A heat treatment production method for temperature controlled quenching of 30CrMnSi steel, used for heat treatment production of the 30CrMnSi steel according to any one of claims 1-2, characterized in that: The method comprises the following steps: (1) Forging billet: 30CrMnSi steel is smelted and cast into an ingot according to its composition, and the ingot is forged into a forging billet; (2) Reheating: Cool the forging billet with air and then heat it in a furnace; (3) Quenching: The forging blank is quenched in stages by oil cooling, water cooling, and oil cooling to room temperature; (4) Tempering: Air cool the forging to room temperature.
4. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 3, characterized in that: The ingot in step (1) is forged into a forging blank at 1200-1250°C.
5. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 3, characterized in that: In the step (2), the forging blank is air-cooled to 550°C±50°C, placed in a furnace and heated to 900±10°C, and kept at this temperature for half an hour.
6. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 3, characterized in that: The process of oil cooling-water cooling-oil cooling segmented quenching is as follows: oil cooling to 600-650° C. in the first stage, water cooling to 350-400° C. in the second stage, and oil cooling to room temperature in the third stage.
7. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 6, characterized in that: The oil cooling speed of the first stage and the third stage is controlled to be 10-15°C / s.
8. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 6, characterized in that: The water cooling rate of the second stage is controlled to be 40-50°C / s.
9. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 6, characterized in that: The water-cooled quenching liquid is salt water, and the oil-cooled quenching liquid is mineral oil.
10. The heat treatment production method for temperature-controlled quenching of 30CrMnSi steel according to claim 3, characterized in that: The forging blank in step (4) is kept at 570-630° C. for 2-3 hours and then air-cooled to room temperature.
Citation Information
Patent Citations
Improved 30CrMnSi steel
CN102660712A
Preparation method of improved 30CrMnSi steel
CN102703825A
Heat treatment method of low-carbon low-alloy steel
CN115874139A
Production method of high-strength alloy steel 30CrMnSi with thickness of 100-150 mm
CN118127415A
Heat treating technology of 30CrMnSi steel for higher toughness and antiwear nature
CN1363694A