Rotary abrasive flow polishing solution as well as preparation method and application thereof

Through specific combination and dispersion technology, the problem of insufficient dispersion stability of the rotary abrasive grain flow polishing liquid is solved, and uniform dispersion of the abrasive grains and uniform passivation of the tool edge are achieved, which extends the service life of the tool.

CN118996424APending Publication Date: 2024-11-22SHENYANG AEROSPACE UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076771.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The dispersion stability of the rotary abrasive grain flow polishing liquid is insufficient, resulting in agglomeration and settlement of abrasive grains, affecting the uniformity and wear resistance of the tool edge passivation.

Method used

Using a specific proportion of abrasive powder, suspended dispersant and preservatives and deionized water, a shear-thickened rotating abrasive stream polishing liquid is formed through mechanical stirring and ultrasonic dispersion technology to ensure uniform dispersion of abrasive particles and avoid agglomeration. .

Benefits of technology

It significantly improves the dispersion stability of abrasive particles, ensures the uniformity and wear resistance of the tool edge passivation, and extends the service life of the tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996424A_ABST
    Figure CN118996424A_ABST
Patent Text Reader

Abstract

The invention discloses a rotary abrasive flow polishing solution as well as a preparation method and application thereof, and belongs to the field of precision / ultra-precision machining. The rotating abrasive flow polishing solution is composed of the following components in percentage by mass: 0.01-20% of abrasive micro-powder; 0.01%-70% of a suspension dispersant and 0.01%-5% of a preservative; and 30%-70% of deionized water. The preparation method comprises the following steps: mixing the abrasive particle micro powder, the suspension dispersant and the preservative solid particles according to a preset percentage, and uniformly dispersing; and adding the dispersed solid particles into deionized water, and uniformly mixing to obtain the rotary abrasive flow polishing solution. The rotating abrasive particle flow polishing solution is a non-Newtonian fluid formed by mixing a high-molecular polymer and deionized water, when the rotating abrasive particle flow and a cutter move relatively, the shear thickening effect of the rotating abrasive particle flow is caused, the high-molecular polymer is promoted to wrap abrasive particles, and a flexible abrasive grinding tool is formed. The material of the cutting edge of the cutter is removed by utilizing the micro-cutting effect of the abrasive particles on the cutting edge of the cutter, so that the aim of passivating the cutting edge of the cutter is fulfilled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of precision / ultra-precision machining, and in particular to a rotating abrasive flow polishing liquid and a preparation method and application thereof. Background Art

[0002] Carbide tools have the advantages of high hardness, good wear resistance, sufficient strength and toughness, and are widely used in the processing of parts in the fields of aerospace, automobiles, electrical and electronic industries. With the rapid development of science and technology and the manufacturing industry, higher requirements are placed on the cutting performance and life of tools.

[0003] After grinding with a grinding wheel, the integral tool will have many microscopic defects, such as notches, microcracks, and micro-peaks. During the cutting process, these microscopic defects will continue to magnify, resulting in increased tool wear or tool edge collapse. Tool passivation is a process method that improves the contour and micromorphology of the tool edge by processing the tool edge. Through tool edge passivation, an appropriate edge contour can be obtained, microscopic defects can be removed, and an edge with fatigue resistance and compressive stress can be obtained, thereby improving the strength, wear resistance, and processing life of the tool. Among them, rotary abrasive flow passivation, as a flexible processing method, causes little damage to the tool body during material removal, and has good applicability to complex structure tools. It has great advantages in many tool passivation processes. However, if the dispersion stability of the rotary abrasive flow polishing liquid is not good, it will cause problems such as abrasive agglomeration and abrasive sedimentation, affecting the uniformity of the edge passivation. Therefore, the basic requirement for the polishing liquid is that the abrasive particles can be evenly suspended and dispersed in the polishing liquid and have sufficient distribution stability. At the same time, no secondary loss should be caused to the tool edge during the passivation process. Therefore, good dispersion stability and micro-defect removal effect are the biggest challenges facing rotating abrasive flow polishing fluids. Summary of the invention

[0004] In view of this, it is necessary to provide a rotating abrasive flow polishing liquid with good dispersion stability. In addition, the present invention also provides a preparation method and application of the rotating abrasive flow polishing liquid.

[0005] A rotating abrasive flow polishing liquid comprising the following components in mass fractions:

[0006] Abrasive powder: 0.01-20wt%;

[0007] Suspending dispersant: 0.01-70wt%;

[0008] Preservative: 0.01-5wt%;

[0009] Deionized water: 30-70wt%.

[0010] Furthermore, the abrasive micropowder is selected from one or more of diamond, aluminum oxide, brown corundum, white corundum, single crystal corundum, microcrystalline corundum, chrome corundum, zirconium corundum, praseodymium-rubidium corundum, black corundum, zirconium oxide, black silicon carbide, green silicon carbide, cubic silicon carbide, boron carbide, cerium silicon carbide, and cubic boron nitride with uniform particle size.

[0011] Furthermore, the type of the suspending dispersant is one or more of starch, corn starch, wheat starch, guar gum, gum arabic, xanthan gum, konjac gum, aloe vera gel, carrageenan, latex, polystyrene, polyvinyl chloride, polymethyl methacrylate, polyacrylamide, silicon dioxide, sodium alginate, agar, and hydroxyethyl cellulose.

[0012] Furthermore, the particle size of the abrasive powder is 0.05 μm-30 μm; the particle size of the suspending dispersant is 0.05-20 μm.

[0013] Furthermore, the preservative is one or more of sorbic acid, potassium sorbate, calcium sorbate, sodium sorbate, sodium benzoate, potassium benzoate, dehydroacetic acid, sodium dehydroacetate, sodium diacetate, propionic acid, sodium propionate, calcium propionate, sodium lactate, dehydrated acetic acid, and dehydrated sodium acetate.

[0014] Furthermore, the conductivity of the deionized water is 0.5 us / cm.

[0015] The rotating abrasive flow polishing liquid exhibits obvious shear thickening phenomenon. The initial viscosity of the rotating abrasive flow polishing liquid is 10-80 Pa, the peak viscosity is 10-100 Pa, and the critical shear rate is 0.3-10 s -1 .

[0016] A method for preparing a rotating abrasive flow polishing liquid comprises the following steps:

[0017] Prepare raw materials according to the following mass fractions: abrasive powder: 0.01-20wt%; suspending dispersant: 0.01-70wt%; preservative: 0.01-5wt%; deionized water: 30-70wt%, mix the abrasive powder, suspending dispersant and preservative and stir to disperse; add the dispersed solid particles into deionized water and stir to disperse, put the dispersed liquid into an ultrasonic cleaning machine for dispersion to remove bubbles, and the ultrasonic dispersion time is 5-60min to obtain a shear thickening polishing liquid.

[0018] Furthermore, the stirring speed of the stirring and dispersing is 50-1500 r / min, and the stirring time is 5-60 min.

[0019] An application of the rotating abrasive flow polishing liquid prepared by the method is used in polishing cemented carbide tools. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The shear rate-viscosity curve of the rotating abrasive flow polishing liquid prepared in Example 1;

[0021] Figure 2 Schematic diagram of the device for passivating the tool with a rotating abrasive flow polishing liquid;

[0022] Figure 3 Measure position map for carbide tool;

[0023] Figure 4 This is a graph showing the change in the radius of the tool edge passivated by the rotating abrasive flow polishing liquid prepared in Example 1 and Example 2;

[0024] Figure 5 The microscopic morphology of the tool edge passivated by the rotating abrasive flow polishing liquid prepared in Example 1 and Example 2. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not limit the present invention.

[0026] The rotating abrasive flow polishing liquid of the present invention comprises the following components in mass fractions:

[0027] Abrasive powder: 0.01 -20wt%;

[0028] Suspending dispersant: 0.01 -70wt%;

[0029] Preservatives: 0.01 -5wt%;

[0030] Deionized water: 30 -70wt%;

[0031] The abrasive micropowder in the rotating abrasive flow polishing liquid is selected from one or more of diamond, aluminum oxide, brown corundum, white corundum, single crystal corundum, microcrystalline corundum, chrome corundum, zirconium corundum, praseodymium rubidium corundum, black corundum, zirconium oxide, black silicon carbide, green silicon carbide, cubic silicon carbide, boron carbide, cerium silicon carbide, and cubic boron nitride with uniform particle size. The particle size of the abrasive micropowder is 0.05 μm-30 μm.

[0032] The type of the suspending dispersant in the rotating abrasive flow polishing liquid is one or more of starch, corn starch, wheat starch, guar gum, gum arabic, xanthan gum, konjac gum, aloe vera gel, carrageenan, latex, polystyrene, polyvinyl chloride, polymethyl methacrylate, polyacrylamide, silicon dioxide, sodium alginate, agar, and hydroxyethyl cellulose, and the particle size of the suspending dispersant is 0.05-20 μm.

[0033] The preservative in the rotating abrasive flow polishing liquid is one or more of sorbic acid, potassium sorbate, calcium sorbate, sodium sorbate, sodium benzoate, potassium benzoate, dehydroacetic acid, sodium dehydroacetate, sodium diacetate, propionic acid, sodium propionate, calcium propionate, sodium lactate, dehydrated acetic acid, and dehydrated sodium acetate.

[0034] The conductivity of the deionized water in the rotating abrasive flow polishing liquid is 0.5 us / cm.

[0035] The method for preparing the rotating abrasive flow polishing liquid comprises the following steps:

[0036] Abrasive particles, suspension dispersants, and preservative solid particles of a preset percentage are mixed and dispersed evenly to eliminate the agglomeration of abrasive micropowders and disperse the abrasive micropowder particles evenly, thereby avoiding uneven passivation during the passivation process. The dispersing method used is one or more of ultrasonic dispersion, magnetic stirring dispersion, electric stirring dispersion, and planetary ball mill dispersion.

[0037] The dispersed solid particles are added to deionized water and dispersed. The dispersion method used is one or more of ultrasonic dispersion, magnetic stirring dispersion, electric stirring dispersion, and planetary ball milling dispersion. Among them, the suspension dispersant will use the macromolecular long chain to entangle the abrasive particles, avoid the abrasive particles from contacting and agglomerating, and ensure that the abrasive particles are evenly distributed in the dispersion system. The preservative has a strong inhibitory effect on microorganisms in the polishing liquid, and it will not deteriorate after being left for a long time.

[0038] Example 1

[0039] The rotating abrasive flow polishing liquid is calculated as 100% by mass, and the components of the rotating abrasive flow polishing liquid are: 43wt% corn starch, 15wt% 15μm aluminum oxide abrasive, 0.2wt% xanthan gum, 2wt% sodium dehydroacetate, and 39.8wt% deionized water. The high molecular polymer corn starch mixed with deionized water can form a non-Newtonian fluid, produce a shear thickening phenomenon, and form a large number of polymer particles wrapped around the abrasive particle clusters. When the tool and the polishing liquid move relative to each other, the abrasive particles in the cluster can remove the material at the cutting edge, thereby achieving the purpose of passivating the cutting edge.

[0040] The steps of the preparation method of the rotating abrasive flow polishing liquid of this embodiment are as follows:

[0041] Alumina abrasive particles, corn starch, xanthan gum, and sodium dehydroacetate solid particles were placed in a mechanical stirrer for mechanical dispersion at a speed of 500 r / min for 20 minutes;

[0042] The dispersed solid particles were slowly added into a certain amount of deionized water and stirred continuously. After mixing, they were placed in a mechanical stirrer for mechanical dispersion at a speed of 80 r / min for 30 minutes.

[0043] The mechanically dispersed liquid was placed in an ultrasonic cleaning machine to disperse and remove bubbles. The dispersion time was 30 minutes to obtain a stable rotating abrasive flow polishing liquid.

[0044] The rheological curve of the rotating abrasive flow polishing liquid of this embodiment was tested, and the results are as follows: Figure 1 As shown. Figure 1 It can be seen that the polishing liquid mostly shows obvious shear thickening phenomenon, and the initial viscosity is 63.85Pa·s -1 , peak viscosity is 80.10Pa·s -1 , the critical shear rate is 3.162s -1 .

[0045] Example 2

[0046] Taking the mass fraction of the rotating abrasive flow polishing liquid as 100%, the shear thickening polishing liquid comprises: 43% corn starch, 15% 15 μm diamond abrasive grains, 0.2% xanthan gum, 2% sodium dehydroacetate, and 39.8% deionized water.

[0047] The steps of the preparation method of the rotating abrasive flow polishing liquid of this embodiment are as follows:

[0048] Diamond abrasive grains, corn starch, xanthan gum, and sodium dehydroacetate solid particles were placed in a mechanical stirrer for mechanical dispersion at a speed of 500 r / min for 20 minutes;

[0049] The dispersed solid particles were slowly added to a certain amount of deionized water and stirred continuously. After mixing, they were added to a mechanical stirrer for mechanical dispersion. The speed of the mechanical stirrer was 80 r / min and stirred for 30 minutes.

[0050] The dispersed liquid was placed in an ultrasonic cleaning machine to disperse and remove bubbles. The dispersion time was 30 minutes to obtain a stable rotating abrasive flow polishing liquid.

[0051] The initial viscosity of the rotating abrasive flow polishing liquid in this embodiment is 63.73 Pa·s -1 , peak viscosity is 78.56Pa·s -1 , the critical shear rate is 3.162s -1 .

[0052] Example 3

[0053] The components of the rotating abrasive flow polishing liquid of this embodiment are: 43% corn starch, 12% 15μm aluminum oxide abrasive particles, 5% 60μm aluminum oxide abrasive particles, 0.2% xanthan gum, 2% sodium dehydroacetate, and 37.8% deionized water.

[0054] The steps of the preparation method of the rotating abrasive flow polishing liquid of this embodiment are as follows:

[0055] Alumina abrasive particles, corn starch, xanthan gum, and sodium dehydroacetate solid particles were placed in a mechanical stirrer for mechanical dispersion at a speed of 500 r / min for 20 minutes;

[0056] The dispersed solid particles were slowly added to a certain amount of deionized water and stirred continuously. After mixing, they were added to a mechanical stirrer for mechanical dispersion. The speed of the mechanical stirrer was 70 r / min and stirred for 40 minutes.

[0057] The dispersed liquid was placed in an ultrasonic cleaning machine to disperse and remove bubbles. The dispersion time was 30 minutes to obtain a stable rotating abrasive flow polishing liquid.

[0058] The initial viscosity of the rotating abrasive flow polishing liquid in this embodiment is 65.32 Pa·s -1 , the peak viscosity is 86.54Pa·s -1 , the critical shear rate is 3.162s -1 .

[0059] Example 4

[0060] The components of the rotating abrasive flow polishing liquid of this embodiment are: 43% corn starch, 10% 15 μm diamond abrasive particles, 7% 60 μm diamond abrasive particles, 0.2% xanthan gum, 2% sodium dehydroacetate, and 37.8% deionized water.

[0061] The steps of the preparation method of the rotating abrasive flow polishing liquid of this embodiment are as follows:

[0062] Diamond abrasive grains, corn starch, xanthan gum, and sodium dehydroacetate solid particles were placed in a mechanical stirrer for mechanical dispersion at a speed of 400 r / min for 20 minutes;

[0063] The dispersed solid particles were slowly added to a certain amount of deionized water and stirred continuously. After mixing, they were added to a mechanical stirrer for mechanical dispersion. The speed of the mechanical stirrer was 70 r / min and stirred for 40 minutes.

[0064] The dispersed liquid was placed in an ultrasonic cleaning machine to disperse and remove bubbles. The dispersion time was 30 minutes to obtain a stable rotating abrasive flow polishing liquid.

[0065] The initial viscosity of the rotating abrasive flow polishing liquid in this embodiment is 64.93 Pa·s -1 , peak viscosity is 84.70Pa·s -1 , the critical shear rate is 3.162s -1 .

[0066] Example 5

[0067] The components of the rotating abrasive flow polishing liquid of this embodiment are: 41.2% corn starch, 20% 15 μm aluminum oxide abrasive, 0.1% carrageenan, 0.1% xanthan gum, 2% sodium dehydroacetate, and 36.6% deionized water.

[0068] The steps of the preparation method of the rotating abrasive flow polishing liquid of this embodiment are as follows:

[0069] Alumina abrasive particles, corn starch, carrageenan, xanthan gum, and sodium dehydroacetate solid particles were placed in a drum mixer for mechanical dispersion at a speed of 30 r / min for 60 minutes;

[0070] The dispersed solid particles were slowly added to a certain amount of deionized water and stirred continuously. After mixing, they were added to a mechanical stirrer for mechanical dispersion. The speed of the mechanical stirrer was 70 r / min and stirred for 40 minutes.

[0071] The dispersed liquid was placed in an ultrasonic cleaning machine to disperse and remove bubbles. The dispersion time was 30 minutes to obtain a stable rotating abrasive flow polishing liquid.

[0072] The initial viscosity of the rotating abrasive flow polishing liquid in this embodiment is 64.91 Pa·s -1 , peak viscosity is 86.01Pa·s -1 , the critical shear rate is 3.162s -1 .

[0073] Example 6

[0074] The components of the rotating abrasive flow polishing liquid of this embodiment are: 41.2% corn starch, 15% 5μm diamond abrasive particles, 5% 15μm diamond abrasive particles, 0.1% carrageenan, 0.1% xanthan gum, 2% potassium sorbate, and 36.6% deionized water.

[0075] The steps of the preparation method of the rotating abrasive flow polishing liquid of this embodiment are as follows:

[0076] Diamond abrasive grains, corn starch, xanthan gum, and potassium sorbate solid particles were placed in a drum mixer for mechanical dispersion at a speed of 30 r / min for 60 minutes;

[0077] The dispersed solid particles were slowly added to a certain amount of deionized water and stirred continuously. After mixing, they were added to a mechanical stirrer for mechanical dispersion. The speed of the mechanical stirrer was 70 r / min and stirred for 40 minutes.

[0078] The dispersed liquid was placed in an ultrasonic cleaning machine to disperse and remove bubbles. The dispersion time was 30 minutes to obtain a stable rotating abrasive flow polishing liquid.

[0079] The initial viscosity of the rotating abrasive flow polishing liquid in this embodiment is 64.61 Pa·s -1 , the peak viscosity is 83.44Pa·s -1 , the critical shear rate is 3.162s -1 .

[0080] Experimental part

[0081] In order to verify that the rotating abrasive flow polishing liquid prepared by the present invention can significantly remove microscopic defects on the cutting edge of cemented carbide tools and increase the cutting edge radius, the present invention also conducted the following tests:

[0082] Effect of Rotating Abrasive Flow Polishing Fluid on the Cutting Edge of Cemented Carbide Tools

[0083] The test selected the rotating abrasive flow polishing liquid prepared in Example 1 and Example 2, according to Figure 2 The passivation method shown in the figure is used to perform the passivation test. The edge radius measurement position is as follows: Figure 3 As shown in the figure, the tool edge radius change measurement results are as follows Figure 4 As shown in Figure 2, the tool microstructure is as follows: Figure 5 shown.

[0084] like Figure 4 As shown, the cutting edge radius of the tool edge passivated by Example 1 and Example 2 is significantly increased, and the cutting edge radius at each detection position changes evenly, indicating that the prepared rotating abrasive flow polishing liquid has good dispersion stability, and the abrasive particles can be evenly suspended and dispersed in the polishing liquid, and are not prone to abrasive agglomeration, abrasive particle sedimentation and other problems.

[0085] like Figure 5 (a) Figure 5 As shown in (b), the cutting edge of the unpassivated tool has obvious serrations and micro-notches. During the cutting process, the cutting force and cutting heat will first act on these defects, causing the cutting edge to break or aggravate wear. After passivation using the polishing liquid of Example 1, the microscopic defects are significantly removed, and the blunt radius of the cutting edge is significantly increased, as shown in FIG. Figure 5 After passivation with the polishing liquid of Example 2, the microscopic defects on the cutting edge surface are significantly removed, the blunt radius of the cutting edge is significantly increased, the cutting edge presents a smooth blunt shape, the grinding marks produced by the front and rear blade surfaces are removed, the surface finish is improved, and a better passivation effect is achieved. Figure 5 (d) as shown.

[0086] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the specification of the present application, or directly or indirectly applied in other related technical fields, are also included in the patent scope of the present application.

Claims

1. A rotating abrasive flow polishing liquid, It is characterized in that The following components are included in mass fraction: Abrasive powder: 0.01-20wt%; Suspending dispersant: 0.01-70wt%; Preservative: 0.01-5wt%; Deionized water: 30-70wt%.

2. A rotating abrasive flow polishing liquid according to claim 1, It is characterized in that The abrasive micropowder is selected from one or more of diamond, aluminum oxide, brown corundum, white corundum, single crystal corundum, microcrystalline corundum, chrome corundum, zirconium corundum, praseodymium-rubidium corundum, black corundum, zirconium oxide, black silicon carbide, green silicon carbide, cubic silicon carbide, boron carbide, cerium silicon carbide, and cubic boron nitride with uniform particle size.

3. A rotating abrasive flow polishing liquid according to claim 1, It is characterized in that The type of the suspending dispersant is one or more of starch, corn starch, wheat starch, guar gum, gum arabic, xanthan gum, konjac gum, aloe vera gel, carrageenan, latex, polystyrene, polyvinyl chloride, polymethyl methacrylate, polyacrylamide, silicon dioxide, sodium alginate, agar, and hydroxyethyl cellulose.

4. A rotating abrasive flow polishing liquid according to claim 1, It is characterized in that The particle size of the abrasive micropowder is 0.05 μm-30 μm; the particle size of the suspending dispersant is 0.05-20 μm.

5. The rotating abrasive flow polishing liquid according to claim 1, It is characterized in that The preservative is one or more of sorbic acid, potassium sorbate, calcium sorbate, sodium sorbate, sodium benzoate, potassium benzoate, dehydroacetic acid, sodium dehydroacetate, sodium diacetate, propionic acid, sodium propionate, calcium propionate, sodium lactate, dehydrated acetic acid, and dehydrated sodium acetate.

6. A rotating abrasive flow polishing liquid according to claim 1, It is characterized in that The conductivity of the deionized water is 0.5 us / cm.

7. The rotating abrasive flow polishing liquid according to claim 1, It is characterized in that The rotating abrasive flow polishing liquid exhibits obvious shear thickening phenomenon. The initial viscosity of the rotating abrasive flow polishing liquid is 10-80 Pa, the peak viscosity is 10-100 Pa, and the critical shear rate is 0.3-10 s -1 .

8. A method for preparing the rotating abrasive flow polishing liquid according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Prepare the raw materials according to the following mass fractions: abrasive powder: 0.01-20wt%; Suspending dispersant: 0.01-70wt%; preservative: 0.01-5wt%; deionized water: 30-70wt%, the abrasive micropowder, suspending dispersant and preservative are mixed and stirred for dispersion; the dispersed solid particles are added into deionized water for stirring and dispersion, the dispersed liquid is placed into an ultrasonic cleaning machine for dispersion and removal of bubbles, and the ultrasonic dispersion time is 5-60min to obtain a shear thickening polishing liquid.

9. The method for preparing the rotating abrasive flow polishing liquid according to claim 8, It is characterized in that The stirring speed of the stirring and dispersing is 50-1500 r / min, and the stirring time is 5-60 min.

10. Use of the rotating abrasive flow polishing liquid according to any one of claims 1 to 7, It is characterized in that The rotating abrasive flow polishing liquid is used for polishing hard alloy cutting tools.