Self-repairing anti-corrosion composite coating and preparation method thereof

By using sandwich structural design and coaxial electrospinning technology in the coating, the adhesion between the fiber membrane and the substrate is solved by preparing the intermediate layer of epoxy resin and polyvinyl alcohol/sodium polyacrylate@tanninic acid/tung oil fiber membrane. The problem of insufficient results has achieved self-repair and improved stability of the coating, and extended the service life of the substrate.

CN118996871APending Publication Date: 2024-11-22CHENGDU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411056447.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22

Smart Images

  • Figure CN118996871A_ABST
    Figure CN118996871A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of anti-corrosion coatings, and particularly relates to a self-repairing type anti-corrosion composite coating and a preparation method thereof. According to the invention, a coaxial nanofiber membrane with polyvinyl alcohol and sodium polyacrylate as a shell and tannic acid and tung oil as core liquid is prepared by adopting an electrostatic spinning technology. An epoxy resin coating is sprayed on an iron sheet in advance, the sprayed epoxy resin is subjected to low-temperature pretreatment to be in a semi-solidified state, a coaxial fiber membrane is attached to the pretreated epoxy resin coating, and finally the epoxy resin is sprayed on the fiber surface again to prepare the composite coating of a sandwich structure. According to the prepared composite coating, after the iron sheet coating is damaged, the anti-corrosion coating can rapidly release an anti-corrosion healing agent, the damaged part of the coating is rapidly repaired, and the composite coating has efficient self-repairing and anti-corrosion capacity and has good application prospects in the anti-corrosion field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of anti-corrosion coatings, and relates to a composite coating with self-repairing anti-corrosion properties and a preparation method thereof, and specifically relates to an epoxy resin and polyvinyl alcohol / sodium polyacrylate@tannic acid / tung oil fiber film composite coating, a preparation method thereof, and its application in the field of self-repairing anti-corrosion. Background Art

[0002] Common self-repairing coatings are mostly made by adding microcapsules and nanocontainers encapsulating metal corrosion inhibitors to epoxy resin and other coatings. When the coating is damaged, the corrosion inhibitor is released from the coating to repair the damaged area and extend the service life of the substrate. Among them, the self-repairing coating prepared based on coaxial electrospinning technology has the advantages of large loading amount of corrosion inhibitor, and when the coating is damaged, the corrosion inhibitor can be quickly and fully released through the vascular network.

[0003] At present, the fiber membrane made by coaxial electrospinning is coated on the surface of the substrate, and then epoxy resin is sprayed to make a composite coating. There is insufficient adhesion between the fiber membrane and the substrate. When the coating is damaged, seawater, river water and other liquids penetrate into the coating, and the fiber membrane and the substrate are separated, causing the coating to fall off the surface of the substrate. At the same time, after the coaxial fiber releases the corrosion inhibitor, hollow fibers are left, or after the fiber dissolves, interpenetrating holes are left inside the coating, which will reduce the mechanical properties of the coating. Summary of the invention

[0004] In view of this, the present invention discloses a self-repairing anti-corrosion composite coating and a preparation method thereof, to provide an anti-corrosion coating that can self-repair after the coating is damaged. The self-repairing anti-corrosion composite coating is a sandwich structure composite coating with self-repairing anti-corrosion properties, which ensures that the corrosion inhibitor of the coaxial fiber of the anti-corrosion layer is released during the process of being immersed in water while the fiber morphology is maintained, thereby enhancing the stability of the coating and achieving a long-term anti-corrosion effect.

[0005] It should be noted that the present invention adopts a sandwich structure design, and the coaxial nanofiber membrane loaded with a metal corrosion inhibitor is prepared between two layers of epoxy resin to avoid direct contact between the fiber membrane and the substrate surface, thereby ensuring the adhesion of the composite coating. At the same time, the coaxial fiber shell layer is prepared by adding polyvinyl alcohol with sodium polyacrylate. Sodium polyacrylate has the property of water absorption and swelling, which can make the shell layer swell, squeeze and release the metal corrosion inhibitor, fill the remaining cavity after release, and reduce the impact on the mechanical strength of the coating, thereby enhancing the self-repairing and anti-corrosion effect of the coating and extending the service life of the substrate.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The invention provides a self-repairing anti-corrosion composite coating, wherein the composite coating is a bottom epoxy resin, the middle layer is a core-shell electrostatic spinning nanofiber membrane with polyvinyl alcohol / sodium polyacrylate as an outer shell and tung oil / tannic acid as a core, and the upper layer is epoxy resin; the epoxy resin is sprayed on the surface of a Q235 steel sheet by a resin spraying technology; coaxial nanofibers with an outer shell of polyvinyl alcohol and sodium polyacrylate and a core liquid of tung oil and tannic acid are prepared by an electrostatic spinning technology; finally, the epoxy resin is sprayed on the fiber surface by a spraying technology to obtain the anti-corrosion composite coating.

[0008] Furthermore, the composite coating is an epoxy resin coating and a polyvinyl alcohol / sodium polyacrylate@tannic acid / tung oil fiber membrane composite coating. A first layer of epoxy resin coating with high viscosity and sealing effect is prepared by spraying technology, a second layer of coaxial nanofiber membrane wrapped with a corrosion inhibitor and having a swelling effect on the outer shell is prepared by coaxial electrospinning technology, and a third layer of epoxy resin coating with excellent adhesion and chemical corrosion resistance is prepared by spraying technology; thereby, a self-healing anti-corrosion composite coating with a sandwich structure is obtained.

[0009] The present invention also provides a method for preparing the self-repairing anti-corrosion composite coating as described above, which specifically comprises the following steps:

[0010] (1) Material selection: epoxy resin is selected as the polymer anti-corrosion coating, polyvinyl alcohol and sodium polyacrylate are used as the coaxial fiber shell, and tannic acid and tung oil are selected as the coaxial fiber core liquid;

[0011] (2) Electrospinning: polyvinyl alcohol, sodium polyacrylate and a cross-linking agent are mixed and dissolved in deionized water to prepare a shell electrospinning solution, and tannic acid and tung oil are mixed and dissolved in an organic solvent to prepare a core electrospinning solution; then, a coaxial nanofiber membrane is prepared by using a coaxial electrospinning technique;

[0012] (3) Fiber cross-linking: The coaxial nanofiber membrane was placed in an oven at 150 °C for two hours to make it swellable;

[0013] (4) Coating preparation: First, epoxy resin is sprayed on the iron sheet, then the coaxial nanofiber membrane is covered on the preheated epoxy resin, and another layer of epoxy resin is sprayed to form an anti-corrosion coating;

[0014] (5) Test preparation: The composite coating was scratched with a utility knife to reveal the iron sheet for subsequent testing.

[0015] Preferably, in step (1), epoxy resin (E44) and curing agent (D230) are used as epoxy resin coating materials; polyvinyl alcohol (PVA) and sodium polyacrylate (NaPAA) are used as shell materials of the anti-corrosion fiber coating, and tannic acid (TA) and tung oil are used as core materials of the anti-corrosion nanofiber membrane.

[0016] Preferably, in step (2), 1-5g PVA and 0.01-0.07g NaPAA are added to 9-50mL deionized water, and after the solution is cooled to room temperature, N, N'-methylenebisacrylamide (MBA) equivalent to 0.05wt% NaPAA is added; 1-5g TA and 0.2-1g tung oil are mixed evenly in an organic solvent. The coaxial spinning voltage is 17-19KV, the shell solution pushing speed is 0.1-0.5mL / h, the core solution pushing speed is 0.0001-0.0005mm / s, and a coaxial needle is used for electrostatic spinning. The distance between the iron plate receiver and the needle is 14±1cm. The electrostatic spinning process is maintained for 10-12h to prepare the coaxial nanofiber membrane, and ensure that the coaxial nanofiber membrane is completely covered on the surface of the iron sheet pretreated with epoxy resin.

[0017] Preferably, in step (3), the coaxial nanofiber membrane is placed in an oven, heated to 150° C. at a rate of 5° C. / min, and heat treated for two hours to completely crosslink it.

[0018] Preferably, in step (4), 1-5 g of E44 epoxy resin is added to 4-20 g of acetone solvent, and after the epoxy resin is completely dissolved, 0.33-2 g of D230 curing agent is added to prepare an epoxy resin solution, which is sprayed on the surface of the iron sheet, and then the iron sheet is placed in an oven at 80°C for heat treatment for 40 minutes; the electrospun membrane is covered on the surface of the epoxy resin, and after spraying the epoxy resin again, it is placed in an oven at 80°C for drying for four hours.

[0019] Furthermore, in step (4), the voltage of the electrospinning machine is 17-19 kV, the pushing speed of the shell solution is 0.1-0.5 mL / h, the pushing speed of the core solution is 0.0001-0.0005 mm / s, a coaxial needle is used for electrospinning, the distance between the iron plate receiver and the needle is 14±1 cm, and the electrospinning process is maintained for 10-12 hours.

[0020] Preferably, in step (5), the composite coating attached to the iron sheet is scratched with a utility knife to expose the iron sheet for corrosion resistance testing.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The composite anti-corrosion coating prepared by the present invention through coaxial electrospinning technology, epoxy resin spraying technology and sandwich structure design has the effect of self-repairing and anti-corrosion, and has broad application prospects in the field of metal substrate anti-corrosion.

[0023] Specifically, the present invention adopts coaxial electrospinning technology to prepare a coaxial nanofiber membrane with polyvinyl alcohol and sodium polyacrylate as the shell, and tannic acid and tung oil as the core liquid. The epoxy resin coating is pre-sprayed on the iron sheet, and the sprayed epoxy resin is pre-treated at low temperature to make it in a semi-solidified state, and the coaxial fiber membrane is attached to the pre-treated epoxy resin coating, and finally the epoxy resin is sprayed on the fiber surface again to form a composite coating with a sandwich structure. The prepared composite coating, after the iron sheet coating is damaged, the anti-corrosion coating will quickly release the anti-corrosion healing agent to quickly repair the damaged parts of the coating, and has a high-efficiency self-repairing anti-corrosion ability, and has good application prospects in the field of anti-corrosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0025] Figure 1 The microscopic morphology of the swelling effect of the coaxial nanofiber membrane before and after immersion; (a) is the microscopic morphology of the fiber membrane before immersion, and (b) is the microscopic morphology of the fiber membrane after immersion.

[0026] Figure 2 This is the microscopic morphology of the coaxial nanofiber membrane under a transmission electron microscope.

[0027] Figure 3 These are impedance diagrams of the composite anti-corrosion coating after scratches were made to expose iron sheets and then immersed in 3.5% NaCl; (a) is the impedance diagram of the blank coating, and (b) is the impedance diagram of the self-repairing anti-corrosion coating. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.

[0030] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.

[0031] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0032] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.

[0033] The present invention discloses a composite coating with self-repairing and anti-corrosion properties and a preparation method thereof, and specifically relates to an epoxy resin and polyvinyl alcohol / sodium polyacrylate@tannic acid / tung oil fiber film composite coating and a preparation method thereof and application thereof in the field of self-repairing and anti-corrosion.

[0034] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0035] Example 1

[0036] This embodiment 1 provides a method for preparing a polyvinyl alcohol / sodium polyacrylate@tannic acid / tung oil nanofiber membrane, which is as follows:

[0037] Dissolve 1g PVA in deionized water to prepare a 10w% PVA solution. Weigh 0.05g NaPAA and add it to the PVA solution, stir it thoroughly, wait for the solution to cool to 25°C, add 0.05mL of MBA aqueous solution NaPAA with a solubility of 0.5g / L, stir it again for 12 hours, and prepare the shell spinning solution. Weigh 1g TA and add it to the DMF solution. After it is fully dissolved, add 0.2g of tung oil and ultrasonicate for 2 hours to obtain the core spinning solution. Then place the obtained electrospinning solution in a 5mL medical syringe for coaxial electrospinning. The coaxial spinning voltage is 17KV, the shell solution push speed is 0.2mL / h, and the core solution push speed is 0.0002mm / s. Use a coaxial needle, the distance between the iron plate receiver and the needle is 14±1cm, and the electrospinning process is maintained for 12h. After spinning, the nanofiber membrane is placed in a 150°C oven for heat treatment for two hours.

[0038] Embodiment 2-3

[0039] Examples 2 to 3 provide different methods for preparing polyvinyl alcohol / sodium polyacrylate@tannic acid / tung oil nanofiber membranes, as follows:

[0040] The specific operation method is the same as that in Example 1, except that the mass of NaPAA added and the concentration of the MBA aqueous solution are different. In Example 2, 0.01 g NaPAA and 0.05 mL of an MBA aqueous solution with a solubility of 0.1 g / L are added; in Example 3, 0.07 g NaPAA and 0.05 mL of an MBA aqueous solution with a solubility of 0.7 g / L are added, and other parameters remain unchanged.

[0041] Example 4

[0042] This embodiment 4 provides a method for preparing a sandwich structure composite coating, which is as follows:

[0043] Weigh 1g of E44 epoxy resin and add it to 4g of acetone solvent. After it is completely dissolved, add 0.33g of D230 curing agent and stir thoroughly to obtain epoxy resin solution. After the steel sheet (Q235) is placed in an oven for heat treatment at 60°C for 1 hour, the configured epoxy resin solution is evenly sprayed on the surface of the iron sheet. After spraying, the steel sheet sprayed with epoxy resin is placed in an oven at 80°C for drying for 40 minutes. When the epoxy resin on the surface of the steel sheet is not completely solidified, the coaxial nanofiber membrane configured in Example 1 is completely covered on the surface of the epoxy resin, and the configured epoxy resin is evenly sprayed on the surface of the electrospinning membrane again. The prepared sandwich structure composite coating is placed in an oven at 80°C for drying for 4 hours.

[0044] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples and test examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.

[0045] Comparative Example 1

[0046] This comparative example 1 provides a method for preparing a blank coating without a self-repairing fiber membrane, which is as follows:

[0047] The specific operation method is the same as that of Example 4, except that no electrospinning membrane is added after the first layer of epoxy resin is sprayed on the steel sheet, and other parameters remain unchanged.

[0048] Test Example 1

[0049] This test example will characterize the microstructure of Examples 1 to 3 before and after immersion in water. The results are as follows: Figure 1 shown.

[0050] The composite nanofiber membranes prepared by electrospinning technology are uniform, continuous, and have a mesh structure with a large specific surface area ( Figure 1 a). The nanofiber membrane with 0.01g NaPAA added showed water absorption and dissolution. This is because the NaPAA content in the shell is small, the cross-linking degree between PVA and NaPAA is low, and the fiber dissolution occurs ( Figure 1 b). The nanofibers with 0.05g NaPAA added showed the best water absorption and swelling effect, because the abundant carboxyl groups in the molecular structure of NaPAA at this concentration will interact with water molecules through hydrogen bonds, causing NaPAA to absorb water and swell ( Figure 1 c). The nanofibers with 0.07 g NaPAA showed excessive water absorption and swelling due to the high concentration of NaPAA ( Figure 1 d).

[0051] Test Example 2

[0052] This test example will characterize the core-shell structure of the coaxial fiber of Example 1 under a transmission electron microscope. The results are as follows Figure 2 shown.

[0053] The composite nanofibrous membrane prepared using coaxial electrospinning technology is uniform, continuous and has a distinct core-shell nanofibrous structure.

[0054] Test Example 3

[0055] This test example uses electrochemical impedance spectroscopy to characterize the self-repairing anti-corrosion properties of the composite self-repairing anti-corrosion coating prepared in Example 4 and Comparative Example 1. The results are as follows: Figure 3 shown.

[0056] The prepared composite anti-corrosion coating was scratched with a utility knife to expose the iron sheet, and the scratched iron sheet was placed in a 3.5% NaCl solution and soaked for 15 days. Then the soaked iron sheet was electrochemically tested to obtain an impedance diagram, and the impedance was analyzed to obtain an impedance modulus diagram. The results are shown in Figure 3 shown.

[0057] like Figure 3 a is the impedance diagram of the blank coating. The impedance of the blank coating increased in the first few days of immersion because the scratches caused the iron exposed to the air to undergo oxidation reaction to form iron oxides such as Fe2O3 attached to the surface of the iron sheet. However, as the immersion time increased, the iron oxides gradually fell off, eventually resulting in a decrease in impedance.

[0058] like Figure 3b is the impedance diagram of the anti-corrosion composite coating containing the self-healing composite nanofiber membrane. The electrochemical impedance of the composite coating showed a small upward trend in the first 3 days. The reason for the increase was the occurrence of anodic dissolution. When the exposed carbon steel substrate was exposed to the corrosive solution, the solution penetrated into the gap to form metal oxides with the carbon steel, and the corrosion inhibitor in the nanofiber reacted with the metal oxide to form a TA film. As the immersion time increased, more and more corrosion inhibitors seeped out of the nanofibers. These water-soluble reaction products filled the bottom of the crack to form a TA protective film, causing the impedance to continue to increase after the third day.

[0059] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A self-repairing anti-corrosion composite coating, characterized in that: The composite coating is a bottom layer of epoxy resin, the middle layer is a core-shell type electrospun nanofiber membrane with polyvinyl alcohol / sodium polyacrylate as the shell and tung oil / tannic acid as the core, and the upper layer is epoxy resin; The epoxy resin is sprayed on the surface of the Q235 steel sheet by the resin spraying technology; the coaxial nanofiber with the shell of polyvinyl alcohol and sodium polyacrylate and the core liquid of tung oil and tannic acid is prepared by the electrospinning technology; finally, the epoxy resin is sprayed on the fiber surface by the spraying technology to obtain the anti-corrosion composite coating.

2. A method for preparing the self-repairing anti-corrosion composite coating according to claim 1, characterized in that: The method specifically comprises the following steps: (1) Preparation of spinning solution for nanofiber membrane: polyvinyl alcohol powder and sodium polyacrylate powder are dissolved in deionized water, and a cross-linking agent is added to prepare a polyvinyl alcohol / sodium polyacrylate spinning solution, i.e., a shell electrospinning solution; tannic acid and tung oil are dissolved in an organic solvent to prepare a tannic acid / tung oil spinning solution, i.e., a core electrospinning solution; and then a coaxial nanofiber membrane is prepared by coaxial electrospinning technology; (2) Preparation of epoxy resin coating: dissolving epoxy resin and curing agent in acetone to prepare epoxy resin solution; (3) fiber cross-linking: subjecting the nanofiber membrane to high temperature heat treatment to enable it to acquire responsiveness to water absorption and swelling; (4) Preparation of composite coating: The first layer of epoxy resin is sprayed on the surface of the iron sheet, and the coaxial nanofiber membrane is spun on the first layer of epoxy resin by electrospinning technology. Finally, epoxy resin is sprayed on the fiber surface again to form a sandwich structure composite coating, namely the self-healing anti-corrosion composite coating.

3. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2, characterized in that: In step (1), 1 to 5 g of polyvinyl alcohol (PVA) and 0.01 to 0.07 g of sodium polyacrylate (NaPAA) are first added to 9 to 50 mL of deionized water, and stirred at 80° C. for 12 hours. After the PVA and NaPAA are completely dissolved, the solution is cooled to room temperature, and then N, N'-methylenebisacrylamide (MBA) equivalent to 0.05 wt% of NaPAA is added to the solution, and stirred for 24 hours to finally prepare a uniformly mixed NaPAA / PVA electrospinning shell solution; 1-5 g of tannic acid (TA) and 0.2-1 g of tung oil were dissolved in 1-5 mL of N,N-dimethylformamide (DMF) solution, and ultrasonically dispersed at room temperature for 1 hour to form a uniformly mixed electrospinning core solution.

4. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2 or 3, characterized in that: In step (1), the coaxial spinning voltage is 17-19 KV, the pushing speed of the shell solution is 0.1-0.5 mL / h, the pushing speed of the core solution is 0.0001-0.0005 mm / s, and a coaxial needle is used for electrospinning. The distance between the iron plate receiver and the needle is 14±1 cm, and the electrospinning process is maintained for 10-12 hours.

5. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2, characterized in that: In step (2), 1-5 g of E44 epoxy resin is added to 4-20 g of acetone solvent and stirred for 1 hour. After the epoxy resin is completely dissolved, 0.33-2 g of D230 curing agent is added and stirred for 1 hour to obtain a uniformly mixed epoxy resin solution.

6. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2, characterized in that: In step (3), the high temperature heat treatment operation is: heating to 150°C at a rate of 5°C / min, and heat treating at 150°C for two hours.

7. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2, characterized in that: In step (4), epoxy resin is first sprayed on the surface of the Q235 steel sheet by spraying technology, the sprayed iron sheet is placed in an oven at 80°C for 40 minutes for pretreatment, and then the pretreated iron sheet sprayed with epoxy resin is fixed on the iron plate receiver of the electrospinning machine.

8. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2 or 7, characterized in that: In step (4), the voltage of the electrospinning machine is 17-19 kV, the pushing speed of the shell solution is 0.1-0.5 mL / h, the pushing speed of the core solution is 0.0001-0.0005 mm / s, and a coaxial needle is used for electrospinning. The distance between the iron plate receiver and the needle is 14±1 cm, and the electrospinning process is maintained for 10-12 hours.

9. The method for preparing a self-repairing anti-corrosion composite coating according to claim 2, characterized in that: In step (4), after spinning is completed, the iron sheet is placed in an oven for cross-linking and drying, and the dried iron sheet is sprayed with epoxy resin again and placed in an oven for drying at 80° C. for 4 hours.

Citation Information

Cited By

  • Swelling type hollow fiber container as well as preparation method and application thereof

    CN120443421A

  • Flame-retardant smoke-suppression anticorrosive fiber material, coating and preparation method thereof

    CN121826922A