Preparation method of pulp molding material with anti-counterfeiting function
By embedding modified cotton fibers in the pulp molding material, the anti-counterfeiting performance is improved by using multi-color luminescent characteristics, the problem of high anti-counterfeiting cost and low imitation difficulty of existing pulp molding products is solved, and efficient anti-counterfeiting effect is achieved.
Patent Information
- Application Number
- CN202411296746.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Existing pulp molding products have high cost and low imitation difficulty in anti-counterfeiting, and it is difficult to effectively prevent forgery.
By embedding red-blue, green-red, blue-green light modified cotton fibers into pulp molding materials, optical anti-counterfeiting fibers are prepared and dispersed in the pulp, and the anti-counterfeiting performance is improved by using multi-color luminescent characteristics. .
It significantly improves the anti-counterfeiting performance and difficulty of counterfeiting of pulp molding materials, enhances the anti-counterfeiting function of the materials, increases the imitation cost, and achieves the anti-counterfeiting effect of multi-color luminescence.
Smart Images

Figure CN118996907A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology and relates to a method for preparing pulp molding materials with anti-counterfeiting functions. Background Art
[0002] With the rapid development of society and the economy, product packaging is ubiquitous, and its role is becoming increasingly important. The most basic function of packaging is to protect products from wear and damage during transportation. Compared with traditional petroleum-based packaging materials, pulp molded products use green and renewable raw materials, and the fibers used can be recycled, making them increasingly important in the packaging field. Pulp molded products are a type of three-dimensional paper product made from paper pulp with the addition of water-retaining agents, reinforcing agents, and other additives, and then molded on a special die. With the widespread application of pulp molded products, how to easily and quickly prevent counterfeiting and achieve high-level anti-counterfeiting on the outer packaging of pulp molded products has become a key research issue. Currently, anti-counterfeiting of packaging materials mainly involves applying anti-counterfeiting ink to the surface of pulp molded products through printing and spraying. This is a post-processing anti-counterfeiting measure, but the cost and difficulty of counterfeiting this type of post-processing anti-counterfeiting are relatively low, making it difficult to achieve effective anti-counterfeiting. Moving the anti-counterfeiting process forward and embedding anti-counterfeiting particles inside the pulp molded product would significantly increase the cost and difficulty of counterfeiting. Summary of the Invention
[0003] The purpose of this invention is to provide a method for preparing pulp molding materials with anti-counterfeiting functions. This method prepares the material by embedding anti-counterfeiting particles inside the pulp molding product, thereby greatly improving the anti-counterfeiting performance of the material and increasing the difficulty and cost of counterfeiting.
[0004] The technical solution adopted in this invention is a method for preparing pulp molding material with anti-counterfeiting function, which specifically includes the following steps:
[0005] Step 1: Red-blue light modification of cotton fibers;
[0006] Step 2: Green-red light modification of cotton fibers;
[0007] Step 3: Perform blue-green light modification on cotton fibers;
[0008] Step 4: Prepare optical anti-counterfeiting fibers based on the products obtained in steps 1 to 3;
[0009] Step 5: Prepare pulp molding anti-counterfeiting materials based on the product obtained in Step 4.
[0010] The invention is further characterized by:
[0011] The specific process of step 1 is as follows:
[0012] Step 1.1: Take 3-6 cotton yarns, 1-2 meters long, with a specification of 60 / 4 count, and put them into 200-300 mL of dimethyl sulfoxide solution. Then add 20-40 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3-6 mL of triethylamine. Under a nitrogen atmosphere, raise the reaction temperature to 180-220℃. After the reaction is complete, wash 3 times with 300-600 mL of deionized water to obtain terpyridine modified cotton fiber.
[0013] Step 1.2: Place the terpyridine-modified cotton fiber obtained in Step 1.1 into 1-2L of deionized water, add 2-4g of reactive red R-2BF dye and 2-4g of sodium sulfate, raise the temperature to 40-60℃, react for 30-60min, then raise the temperature to 60-80℃, add 1.5-3g of sodium carbonate and react for 30min. After the reaction is complete, wash with soaping agent HM-900 until no pigment fades, and obtain red-blue modified cotton fiber.
[0014] The specific process of step 2 is as follows:
[0015] Step 2.1: Take 3-6 cotton yarns, 1-2 meters long, with a specification of 60 / 4 count, and put them into 200-300 mL of dimethyl sulfoxide solution. Then add 20-40 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3-6 mL of triethylamine. Under a nitrogen atmosphere, raise the reaction temperature to 180-220℃. After the reaction is complete, wash 3 times with 300-600 mL of deionized water to obtain terpyridine modified cotton fiber.
[0016] Step 2.2: Place the terpyridine-modified cotton fiber obtained in Step 2.1 into 1-2L of deionized water, add 2-4g of Direct Green BE dye and 2-4g of sodium sulfate, raise the temperature to 40-60℃, react for 30-60min, then raise the temperature to 60-80℃, add 1.5-3g of sodium carbonate, and react for 30-60min. After the reaction is complete, wash with soap detergent HM-900 until no pigment fades.
[0017] Step 2.3: Place the cotton fibers obtained after the treatment in step 2.2 into 100-200mL of deionized water, then add 3-6g of hexafluoroacetylacetone, 2-3g of europium chloride and 1-2mL of triethylamine in sequence, heat the temperature to 60-80℃ and react for 1-3h, wash three times with 300-600mL of deionized water to obtain green-red light modified cotton fibers.
[0018] The specific process of step 3 is as follows:
[0019] Step 3.1: Take 3-6 cotton yarns, 1-2 meters long, with a specification of 60 / 4 count, and put them into 200-300 mL of dimethyl sulfoxide solution. Then add 20-40 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3-6 mL of triethylamine. Under a nitrogen atmosphere, raise the reaction temperature to 180-220℃. After the reaction is complete, wash 3 times with 300-600 mL of deionized water to obtain terpyridine modified cotton fiber.
[0020] Step 3.2: Place the terpyridine-modified cotton fiber obtained in step 3.1 into 1-2L of deionized water, add 2-4g of reactive deep blue R-2GLN dye and 2-4g of sodium sulfate, raise the temperature to 40-60℃, react for 30-60min, then raise the temperature to 60-80℃, add 1.5-3g of sodium carbonate and react for 30-60min. After the reaction is complete, wash with soap detergent HM-900 until no pigment fades.
[0021] Step 3.3: Place the cotton fibers treated in step 3.2 into 100-200mL of deionized water, then add 3-6g of hexafluoroacetylacetone, 2-3g of terbium chloride and 1-2mL of triethylamine in sequence. Heat the water to 60-80℃ and react for 1-3 hours. Wash the cotton fibers three times with 300-600mL of deionized water to obtain green-red light modified cotton fibers.
[0022] The specific process of step 4 is as follows:
[0023] Step 4.1: Immerse 1-3 red-blue light modified cotton fibers, 1-3 green-red light modified cotton fibers, and 1-3 blue-green light modified cotton fibers in the UV adhesive solution for 2-10 seconds respectively.
[0024] Step 4.2: The cotton fibers impregnated with UV adhesive obtained in step 4.1 are spirally wound onto the surface of a circular cylinder with a diameter of 5-10cm, and then irradiated with a UV lamp for 20-40s to obtain optical anti-counterfeiting fibers.
[0025] In step 4.1, the UV adhesive is prepared by mixing 40-59g of ethylene glycol acrylate, 40-59g of butyl acrylate and 1-10g of azobisisobutyronitrile evenly.
[0026] The specific process of step 5 is as follows:
[0027] Step 5.1: Take 100-200g of pulp. Choose any one or more of the following: bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp. Break it up at 25℃ for 10-20 minutes and adjust the pulping concentration to 8-12%. After beating, the freeness should be 50-60°SR.
[0028] Step 5.2: Add 1-2g of cyclopropane acrylic resin, 2-3g of polyvinyl alcohol, 0.2-0.4g of polyacrylamide, and 0.5-1g of optical anti-counterfeiting fiber with a width of 0.1-1mm and a length of 1-3mm to the slurry obtained in step 5.1 to obtain a mixed slurry.
[0029] Step 5.3: The mixed slurry obtained in step 5.2 is introduced into the mold of a micro pulp molding machine and filtered until the water content is 55-60%. Then, it is extruded and molded at 5-6 MPa and demolded. Then, it is dried in a drying oven at 70-80℃ for 4-5 hours. Finally, it is transferred to a flat vulcanizing machine for hot pressing and shaping, with the temperature controlled at 100-110℃, the pressure at 5.5-6 MPa, and the time at 2-3 minutes, thus obtaining the pulp molded anti-counterfeiting material.
[0030] The beneficial effects of this invention are as follows:
[0031] 1. This invention designs fibrous anti-counterfeiting particles. A single fiber can achieve red, green, and blue color recognition with the naked eye. Furthermore, under 254nm excitation, it can emit blue, red, and green light. The length of the anti-counterfeiting fibers can be easily adjusted by arranging them as single, double, or triple fibers. Dispersing the anti-counterfeiting fibers in pulp and further preparing pulp molding products, the combination of the three colors and three light emission significantly improves the anti-counterfeiting performance.
[0032] 2. This invention constructs three colors of luminescent anti-counterfeiting fibers; most dyes have their own color and emit fluorescence when excited at 365nm, which has a great impact on the anti-counterfeiting color and luminescent anti-counterfeiting.
[0033] 3. The anti-counterfeiting fiber constructed in this invention has a fluorescence excitation of 254nm, avoiding the influence of ultraviolet excitation of pigments on luminescence performance. Simultaneously, the red, green, and blue colors match the blue, red, and green luminescence wavelengths, avoiding overlap between pigment absorption wavelengths and emission wavelengths, thus preventing impact on luminescence performance. The anti-counterfeiting fiber can be uniformly dispersed with the pulp, and the prepared pulp molding contains anti-counterfeiting particles, which differs from the surface printing process of traditional anti-counterfeiting particles, increasing the difficulty of counterfeiting. Attached Figure Description
[0034] Figure 1 This is a process diagram of the preparation of anti-counterfeiting fibers in the preparation method of the anti-counterfeiting pulp molding material of the present invention;
[0035] Figure 2 This is an example of the preparation method of the anti-counterfeiting pulp molding material of the present invention, showing the intensity of red-blue light modified cotton fiber, green-red light modified cotton fiber, and blue-green light modified cotton fiber at 254nm ultraviolet light. Detailed Implementation
[0036] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0037] The method for preparing the anti-counterfeiting molded pulp material of the present invention specifically includes the following steps:
[0038] Step 1, red-blue light modification of cotton fibers: Take 3-6 strands of cotton yarn, 1-2 meters long, with a specification of 60 / 4 metric count, and place them in 200-300 mL of dimethyl sulfoxide solution. Then add 20-40 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3-6 mL of triethylamine. Raise the reaction temperature to 180-220℃ under a nitrogen atmosphere. After the reaction is complete, wash three times with 300-600 mL of deionized water. Tripyridine-modified cotton fiber was obtained; the tripyridine-modified cotton fiber was further placed in 1-2L of deionized water, 2-4g of reactive red R-2BF dye and 2-4g of sodium sulfate were added, the temperature was raised to 40-60℃, and the reaction was carried out for 30-60min. Then the temperature was further raised to 60-80℃, 1.5-3g of sodium carbonate was added, and the reaction was carried out for 30min. After the reaction was completed, the cotton fiber was washed with soaping agent HM-900 until no pigment faded, thus obtaining red-blue modified cotton fiber.
[0039] Step 2, green-red light modification of cotton fibers, specifically: Take 3-6 strands of cotton yarn, 1-2 meters long, with a specification of 60 / 4 metric count, and place them in 200-300 mL of dimethyl sulfoxide solution. Then add 20-40 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3-6 mL of triethylamine. Raise the reaction temperature to 180-220℃ under a nitrogen atmosphere. After the reaction, wash three times with 300-600 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1-2 L of deionized water and add 2-4 g of direct green BE. Add 2-4g of dye and sodium sulfate, raise the temperature to 40-60℃, react for 30-60 minutes, then further heat to 60-80℃, add 1.5-3g of sodium carbonate, and react for another 30-60 minutes. After the reaction, wash with HM-900 soap until no pigment fades. Further, immerse the obtained cotton fibers in 100-200mL of deionized water, then add 3-6g of hexafluoroacetylacetone, 2-3g of europium chloride, and 1-2mL of triethylamine sequentially. Heat to 60-80℃ and react for 1-3 hours. Wash three times with 300-600mL of deionized water to obtain green-red modified cotton fibers.
[0040] Step 3, blue-green light modification of cotton fibers, specifically: Take 3-6 strands of cotton yarn, 1-2 meters long, with a specification of 60 / 4 metric count, and place them in 200-300 mL of dimethyl sulfoxide solution. Then add 20-40 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3-6 mL of triethylamine. Raise the reaction temperature to 180-220℃ under a nitrogen atmosphere. After the reaction, wash three times with 300-600 mL of deionized water to obtain terpyridine-modified cotton fibers. Further place the obtained terpyridine-modified cotton fibers in 1-2 L of deionized water and add 2-4 g of active deep blue R-2G. LN dye and 2-4g of sodium sulfate are reacted at 40-60℃ for 30-60 minutes, then further heated to 60-80℃. 1.5-3g of sodium carbonate is added, and the reaction continues for another 30-60 minutes. After the reaction, the mixture is washed with HM-900 soap until no pigment fading occurs. The resulting cotton fibers are then placed in 100-200mL of deionized water, followed by the sequential addition of 3-6g of hexafluoroacetylacetone, 2-3g of terbium chloride, and 1-2mL of triethylamine. The mixture is heated to 60-80℃ and reacted for 1-3 hours. The fibers are then washed three times with 300-600mL of deionized water to obtain blue-green modified cotton fibers.
[0041] Step 4, the preparation of optical anti-counterfeiting fibers, specifically as follows: Figure 1 As shown, 1-3 red-blue light-modified cotton fibers, 1-3 green-red light-modified cotton fibers, and 1-3 blue-green light-modified cotton fibers were respectively immersed in a UV adhesive solution for 2-10 seconds. The UV adhesive components were ethylene glycol acrylate (40-59g), butyl acrylate (40-59g), and azobisisobutyronitrile (1-10g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a cylindrical column with a diameter of 5-10cm, and irradiated with a 45W, 365nm UV lamp for 20-40 seconds. Finally, a laser cutting machine was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1-1mm and a length of 1-3mm.
[0042] Step 5, preparation of pulp molding anti-counterfeiting material, specifically: Take 100-200g of pulp, the pulp can be any one or more of bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp, and break it up at 25℃ for 10-20min, adjust the pulping concentration to 8-12%, and the freeness after beating is 50-60°SR. Then add cyclopropane acrylic resin (1-2g), polyvinyl alcohol (2-3g), polyacrylamide (0.2-0.4g), and optical anti-counterfeiting fibers with a width of 0.1-1mm and a length of 1-3mm (0.5-1g) to obtain a mixed pulp. The mixed slurry is then introduced into the mold of a micro pulp molding machine to filter water until the moisture content is 55-60%. After extrusion molding at 5-6 MPa, it is demolded and then dried in a drying oven at 70-80℃ for 4-5 hours. Finally, it is transferred to a flat vulcanizing machine for hot pressing and shaping, with the temperature controlled at 100-110℃, the pressure at 5.5-6 MPa, and the time at 2-3 minutes, to obtain pulp molded anti-counterfeiting material.
[0043] Example 1
[0044] Step 1, red-blue light modification of cotton fibers: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4 metric count, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180 °C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and 2 g of sodium sulfate, raise the temperature to 40 °C, and react for 30 min. Then, further raise the temperature to 60 °C, add 1.5 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0045] Step 2, green-red light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, place the terpyridine-modified cotton fibers in 1L of deionized water, add 2g of... Green BE dye and 2g of sodium sulfate were added, and the temperature was raised to 40℃. After reacting for 30 minutes, the temperature was further raised to 60℃, and 1.5g of sodium carbonate was added. The reaction was continued for 30 minutes. After the reaction was completed, the cotton fibers were washed with HM-900 soap until no pigment faded. The resulting cotton fibers were then placed in 100mL of deionized water, and then 3g of hexafluoroacetylacetone, 2g of europium chloride, and 1mL of triethylamine were added sequentially. The temperature was heated to 60℃ and reacted for 1 hour. The fibers were washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0046] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn (60 / 4 count) and place them in 200mL of dimethyl sulfoxide solution. Then add 20g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1L of deionized water and add 2g of active dark dye. Blue R-2GLN dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then further heated to 60℃. 1.5g of sodium carbonate was added and reacted for another 30 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of hexafluoroacetylacetone, 2g of terbium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0047] Step 4, the preparation of optical anti-counterfeiting fibers, specifically as follows: Figure 1As shown, one red-blue light-modified cotton fiber, one green-red light-modified cotton fiber, and one blue-green light-modified cotton fiber were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive consisted of ethylene glycol acrylate (40g), butyl acrylate (59g), and azobisisobutyronitrile (1g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a 5cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1mm and a length of 1mm.
[0048] Step 5, preparation of pulp molding anti-counterfeiting material, specifically: Take 100g of pulp, selecting any one or more of bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp. Break it up at 25℃ for 10 minutes, adjusting the pulping concentration to 8%. After beating, the freeness should be 50°SR. Then add 1g of cyclopropane acrylic resin, 2g of polyvinyl alcohol, 0.2g of polyacrylamide, and 0.5g of optical anti-counterfeiting fiber with a width of 0.1mm and a length of 1mm to obtain a mixed pulp. Then, pour the mixed pulp into the mold of a micro pulp molding machine, filter to a moisture content of 55%, then extrude and mold at 5MPa, demold, and dry in a drying oven at 70℃ for 4 hours. Finally, transfer to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 100℃, the pressure at 5.5MPa, and the time at 2 minutes to obtain the pulp molding anti-counterfeiting material.
[0049] Comparative Example 1 (Compared to Example 1, the beta-diketone ligand hexafluoroacetylacetone was replaced with 2-thiophenecarboxyltrifluoroacetone, the anti-counterfeiting fiber lacked green color and showed weak red light under 254 excitation)
[0050] Step 1, red-blue light modification of cotton fibers: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4 metric count, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180 °C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and 2 g of sodium sulfate, raise the temperature to 40 °C, and react for 30 min. Then, further raise the temperature to 60 °C, add 1.5 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0051] Step 2, green-red light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, place the terpyridine-modified cotton fibers in 1L of deionized water, add 2g of direct green light... BE dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then further heated to 60℃. 1.5g of sodium carbonate was added and reacted for another 30 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of 2-thiophenecarboxyltrifluoroacetone, 2g of europium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0052] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn (60 / 4 count) and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180°C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 1 L of deionized water and add 2 g of active deep blue R- 2g of 2GLN dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then further heated to 60℃. 1.5g of sodium carbonate was added and reacted for another 30 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of 2-thiophenecarboxyltrifluoroacetone, 2g of terbium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0053] Step 4, preparation of optical anti-counterfeiting fibers, specifically: One red-blue light modified cotton fiber, one green-red light modified cotton fiber, and one blue-green light modified cotton fiber were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive components were ethylene glycol acrylate (40g), butyl acrylate (59g), and azobisisobutyronitrile (1g). The cotton fibers impregnated with the UV adhesive were spirally wound onto the surface of a 5cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1mm and a length of 1mm.
[0054] Step 5, preparation of pulp molding anti-counterfeiting material, specifically: Take 100g of pulp, selecting any one or more of bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp, and break it down at 25℃ for 10 minutes, adjusting the pulping concentration to 8%, and achieving a freeness of 50°SR after beating. Then add cyclopropane acrylic resin (1g), polyvinyl alcohol (2g), polyacrylamide (0.2g), and optical anti-counterfeiting fiber (0.5g) with a width of 0.1mm and a length of 1mm to obtain a mixed pulp. Then, pour the mixed pulp into the mold of a micro pulp molding machine, filter water until the moisture content is 55%, then extrude it at 5MPa and demold it, then dry it in a drying oven at 70℃ for 4 hours, and finally transfer it to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 100℃, the pressure at 5.5MPa, and the time at 2 minutes to obtain the pulp molding anti-counterfeiting material.
[0055] Comparative Example 2 (Compared to Example 1, during the preparation of green-red light modified cotton fiber and blue-green light modified cotton fiber, Eu and Tb ion exchange occurred, the pulp molded anti-counterfeiting fiber did not have green light, and the position of red light changed)
[0056] Step 1, red-blue light modification of cotton fibers: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4 metric count, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180 °C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and 2 g of sodium sulfate, raise the temperature to 40 °C, and react for 30 min. Then, further raise the temperature to 60 °C, add 1.5 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0057] Step 2, green-red light modification of cotton fibers, specifically: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4 count, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1 L of deionized water and add 2 g of... Direct green BE dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then further heated to 60℃. 1.5g of sodium carbonate was added and reacted for another 30 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of hexafluoroacetylacetone, 2g of terbium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0058] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, obtain terpyridine-modified cotton fibers; place them in 1L of deionized water, add 2g of active... Deep blue R-2GLN dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then further heated to 60℃. 1.5g of sodium carbonate was added and reacted for another 30 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of hexafluoroacetylacetone, 2g of europium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0059] Step 4: One red-blue light-modified cotton fiber, one green-red light-modified cotton fiber, and one blue-green light-modified cotton fiber were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive consisted of ethylene glycol acrylate (40 parts), butyl acrylate (59 parts), and azobisisobutyronitrile (1 part). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a 5cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1mm and a length of 1mm.
[0060] Step 5: Take 100g of pulp. Choose one or more of the following pulp types: bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, or straw pulp. Break it up at 25℃ for 10 minutes, adjusting the beating concentration to 8%. After beating, the freeness should be 50°SR. Then add 1g of cyclopropane acrylic resin, 2g of polyvinyl alcohol, 0.2g of polyacrylamide, and 0.5g of optical anti-counterfeiting fiber with a width of 0.1mm and a length of 1mm to obtain a mixed pulp. Pulp is then introduced into the mold of a micro pulp molding machine and filtered until the moisture content is 55%. It is then extruded at 5MPa and demolded. Afterward, it is dried in a drying oven at 70℃ for 4 hours. Finally, it is transferred to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 100℃, the pressure at 5.5MPa, and the time at 2 minutes to obtain the pulp molded anti-counterfeiting material.
[0061] Comparative Example 3 (Compared to Example 1, in the preparation of red-blue and blue-green modified cotton fibers, the red and blue dyes were exchanged, the pulp molded anti-counterfeiting fibers did not have blue light, and the positions of blue and red were interchanged)
[0062] Step 1, red-blue light modification of cotton fibers: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1L of deionized water, add 2g of reactive deep blue R-2GLN dye and 2g of sodium sulfate, raise the temperature to 40℃, react for 30min, then further heat to 60℃, add 1.5g of sodium carbonate, and react for 30min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0063] Step 2, green-red light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, place the terpyridine-modified cotton fibers in 1L of deionized water, add 2g of... Green BE dye and 2g of sodium sulfate were added, and the temperature was raised to 40℃. After reacting for 30 minutes, the temperature was further raised to 60℃, and 1.5g of sodium carbonate was added. The reaction was continued for 30 minutes. After the reaction was completed, the cotton fibers were washed with HM-900 soap until no pigment faded. The resulting cotton fibers were then placed in 100mL of deionized water, and then 3g of hexafluoroacetylacetone, 2g of europium chloride, and 1mL of triethylamine were added sequentially. The temperature was heated to 60℃ and reacted for 1 hour. The fibers were washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0064] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn (60 / 4 count) and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180°C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water. Further, place the cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and sulfur... 2g of sodium carbonate was added, and the temperature was raised to 40℃. After reacting for 30 minutes, the temperature was further raised to 60℃, and 1.5g of sodium carbonate was added. The reaction was continued for another 30 minutes. After the reaction was completed, the cotton fibers were washed with HM-900 soap until no pigment faded. The resulting cotton fibers were then placed in 100mL of deionized water, and then 3g of hexafluoroacetylacetone, 2g of terbium chloride, and 1mL of triethylamine were added sequentially. The temperature was heated to 60℃ and reacted for 1 hour. The fibers were washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0065] Step 4: One red-blue light-modified cotton fiber, one green-red light-modified cotton fiber, and one blue-green light-modified cotton fiber were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive consisted of ethylene glycol acrylate (40g), butyl acrylate (59g), and azobisisobutyronitrile (1g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a 5cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1mm and a length of 1mm.
[0066] Step 5: Take 100g of pulp from any one or more of the following: bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp. Break it up at 25℃ for 10 minutes, adjusting the beating concentration to 8%. After beating, the freeness should be 50°SR. Then add 1g of cyclopropane acrylic resin, 2g of polyvinyl alcohol, 0.2g of polyacrylamide, and 0.5g of optical anti-counterfeiting fiber with a width of 0.1mm and a length of 1mm to obtain a mixed pulp. Pulp is then introduced into a mold of a micro pulp molding machine and filtered until the moisture content is 55%. It is then extruded at 5MPa, demolded, and dried in a drying oven at 70℃ for 4 hours. Finally, it is transferred to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 100℃, the pressure at 5.5MPa, and the time at 2 minutes to obtain the pulp molded anti-counterfeiting material.
[0067] Comparative Example 4 (Compared to Example 1, the water-retaining agent cyclopropane acrylic resin was replaced with sodium alginate, and the multi-color luminescence of the anti-counterfeiting fiber was changed to single blue light)
[0068] Step 1, red-blue light modification of cotton fibers: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further place the terpyridine-modified cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and 2 g of sodium sulfate, raise the temperature to 40℃, and react for 30 min. Then, further heat to 60℃, add 1.5 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0069] Step 2, green-red light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, place the terpyridine-modified cotton fibers in 1L of deionized water, add 2g of... Green BE dye and 2g of sodium sulfate were added, and the temperature was raised to 40℃. After reacting for 30 minutes, the temperature was further raised to 60℃, and 1.5g of sodium carbonate was added. The reaction was continued for 30 minutes. After the reaction was completed, the cotton fibers were washed with HM-900 soap until no pigment faded. The resulting cotton fibers were then placed in 100mL of deionized water, and then 3g of hexafluoroacetylacetone, 2g of europium chloride, and 1mL of triethylamine were added sequentially. The temperature was heated to 60℃ and reacted for 1 hour. The fibers were washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0070] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn (60 / 4 count) and place them in 200mL of dimethyl sulfoxide solution. Then add 20g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 1L of deionized water and add 2g of active deep blue dye. R-2GLN dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then the temperature was further increased to 60℃, and 1.5g of sodium carbonate was added, followed by another 30 minutes of reaction. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of hexafluoroacetylacetone, 2g of terbium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0071] Step 4: One red-blue light-modified cotton fiber, one green-red light-modified cotton fiber, and one blue-green light-modified cotton fiber were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive consisted of ethylene glycol acrylate (40g), butyl acrylate (59g), and azobisisobutyronitrile (1g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a 5cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1mm and a length of 1mm.
[0072] Step 5: Take 100g of pulp, selecting one or more of the following: bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp. Break it up at 25℃ for 10 minutes, adjusting the beating concentration to 8%. After beating, the freeness should be 50°SR. Then add sodium alginate (1g), polyvinyl alcohol (2g), polyacrylamide (0.2g), and optical anti-counterfeiting fiber (0.5g) with a width of 0.1mm and a length of 1mm to obtain a mixed pulp. Pulp is then introduced into the mold of a micro pulp molding machine and filtered until the moisture content is 55%. It is then extruded at 5MPa and demolded. Afterward, it is dried in a drying oven at 70℃ for 4 hours. Finally, it is transferred to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 100℃, the pressure at 5.5MPa, and the time at 2 minutes to obtain the pulp molded anti-counterfeiting material.
[0073] Comparative Example 5 (Compared to Example 1, the reinforcing agent polyvinyl alcohol was replaced with carboxymethyl cellulose, and the multi-color luminescence of the anti-counterfeiting fiber was changed to single blue light)
[0074] Step 1, red-blue light modification of cotton fibers: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4 metric count, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180 °C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and 2 g of sodium sulfate, raise the temperature to 40 °C, and react for 30 min. Then, further raise the temperature to 60 °C, add 1.5 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0075] Step 2, green-red light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, place the terpyridine-modified cotton fibers in 1L of deionized water, add 2g of... Green BE dye and 2g of sodium sulfate were added, and the temperature was raised to 40℃. After reacting for 30 minutes, the temperature was further raised to 60℃, and 1.5g of sodium carbonate was added. The reaction was continued for 30 minutes. After the reaction was completed, the cotton fibers were washed with HM-900 soap until no pigment faded. The resulting cotton fibers were then placed in 100mL of deionized water, and then 3g of hexafluoroacetylacetone, 2g of europium chloride, and 1mL of triethylamine were added sequentially. The temperature was heated to 60℃ and reacted for 1 hour. The fibers were washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0076] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn (60 / 4 count) and place them in 200mL of dimethyl sulfoxide solution. Then add 20g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 1L of deionized water and add 2g of active deep blue dye. R-2GLN dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then the temperature was further increased to 60℃, and 1.5g of sodium carbonate was added, followed by another 30 minutes of reaction. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of hexafluoroacetylacetone, 2g of terbium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0077] Step 4: One red-blue light-modified cotton fiber, one green-red light-modified cotton fiber, and one blue-green light-modified cotton fiber (1) were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive consisted of ethylene glycol acrylate (40 parts), butyl acrylate (59 parts), and azobisisobutyronitrile (1 part). The UV-adhesive-impregnated cotton fiber was spirally wound onto the surface of a cylindrical column with a diameter of cm, and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fiber to obtain an optical anti-counterfeiting fiber with a width of 0.1mm and a length of 1mm.
[0078] Step 5: Take 100g of pulp. The pulp can be any one or more of the following: bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, or straw pulp. Break it up at 25℃ for 10 minutes, adjusting the beating concentration to 8%. After beating, the freeness should be 50°SR. Then add 1g of cyclopropane acrylic resin, 2g of carboxymethyl cellulose, 0.2g of polyacrylamide, and 0.5g of optical anti-counterfeiting fiber with a width of 0.1mm and a length of 1mm to obtain a mixed pulp. Then, pour the mixed pulp into the mold of a micro pulp molding machine, filter to a moisture content of 55%, and then extrude it at 5MPa. After demolding, dry it in a drying oven at 70℃ for 4 hours. Finally, transfer it to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 100℃, the pressure at 5.5MPa, and the time at 2 minutes to obtain the pulp molded anti-counterfeiting material.
[0079] Comparative Example 6 (Compared to Example 1, in the preparation process of optical anti-counterfeiting fibers, ethylene glycol acrylate was not added to the UV binder, and the prepared anti-counterfeiting fibers could not be dispersed in pulp molding)
[0080] Step 1, red-blue light modification of cotton fibers: Take 3 cotton yarns, each 1 meter long and of specification 60 / 4 metric count, and place them in 200 mL of dimethyl sulfoxide solution. Then add 20 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3 mL of triethylamine. Raise the reaction temperature to 180 °C under a nitrogen atmosphere. After the reaction, wash three times with 300 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1 L of deionized water, add 2 g of reactive red R-2BF dye and 2 g of sodium sulfate, raise the temperature to 40 °C, and react for 30 min. Then, further raise the temperature to 60 °C, add 1.5 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0081] Step 2, green-red light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn with a specification of 60 / 4 count, place them in 200mL of dimethyl sulfoxide solution, then add 20g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers; further, place the terpyridine-modified cotton fibers in 1L of deionized water, add 2g of... Green BE dye and 2g of sodium sulfate were added, and the temperature was raised to 40℃. After reacting for 30 minutes, the temperature was further raised to 60℃, and 1.5g of sodium carbonate was added. The reaction was continued for 30 minutes. After the reaction was completed, the cotton fibers were washed with HM-900 soap until no pigment faded. The resulting cotton fibers were then placed in 100mL of deionized water, and then 3g of hexafluoroacetylacetone, 2g of europium chloride, and 1mL of triethylamine were added sequentially. The temperature was heated to 60℃ and reacted for 1 hour. The fibers were washed three times with 300mL of deionized water to obtain green-red modified cotton fibers.
[0082] Step 3, blue-green light modification of cotton fibers, specifically: Take 3 strands of 1-meter-long cotton yarn (60 / 4 count) and place them in 200mL of dimethyl sulfoxide solution. Then add 20g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 3mL of triethylamine. Raise the reaction temperature to 180℃ under a nitrogen atmosphere. After the reaction, wash three times with 300mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1L of deionized water and add 2g of active dark dye. Blue R-2GLN dye and 2g of sodium sulfate were reacted at 40℃ for 30 minutes, then further heated to 60℃. 1.5g of sodium carbonate was added and reacted for another 30 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 100mL of deionized water, followed by the addition of 3g of hexafluoroacetylacetone, 2g of terbium chloride, and 1mL of triethylamine. The mixture was heated to 60℃ and reacted for 1 hour. The fibers were then washed three times with 300mL of deionized water to obtain blue-green modified cotton fibers.
[0083] Step 4, preparation of optical anti-counterfeiting fibers, specifically: One red-blue light modified cotton fiber, one green-red light modified cotton fiber, and one blue-green light modified cotton fiber were each immersed in a UV adhesive solution for 10 seconds. The UV adhesive components were butyl acrylate (99g) and azobisisobutyronitrile (1g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a cylindrical column with a diameter of cm, and irradiated with a 45W, 365nm UV lamp for 20 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.1mm and a length of 1mm.
[0084] Results Discussion
[0085] like Figure 1 As shown, the preparation process of anti-counterfeiting fibers mainly involves adhesive impregnation, spiral winding, UV curing, and laser cutting. It can be achieved by arranging one red-blue light-modified cotton fiber, one green-red light-modified cotton fiber, and one blue-green light-modified cotton fiber to form single red, green, and blue fibers, whose colors are visible to the naked eye and whose blue, red, and green light emission can be seen under 254nm ultraviolet light. Similarly, two red-blue light-modified cotton fibers, two green-red light-modified cotton fibers, and two blue-green light-modified cotton fibers can be arranged sequentially to form a double red, green, and blue fiber arrangement; or three red-blue light-modified cotton fibers, three green-red light-modified cotton fibers, and three blue-green light-modified cotton fibers can be arranged sequentially to form a triple red, green, and blue fiber arrangement. The fiber colors and color arrangements can be used as an anti-counterfeiting code.
[0086] like Figure 2 As shown, the red-blue light modified cotton fiber, green-red light modified cotton fiber, and blue-green light modified cotton fiber prepared in Example 1 can be detected with blue light emission at 430 nm, red light emission at 613 nm, and green light emission at 547 nm under 254 nm ultraviolet light irradiation. The broad peak at 430 nm in the red-blue light modified cotton fiber is the fluorescence emission peak of the terpyridine functional group. The red light emission at 613 nm in the green-red light modified cotton fiber is a narrow linear spectrum, clearly indicating the presence of rare earth ions (Eu). 3+ The characteristic luminescence of the blue-green modified cotton fiber is also a narrow linear spectrum, which can be attributed to the characteristic luminescence of rare earth Tb3+ ions. It should be noted that the pigment used in the dyeing of the yarn itself also luminesces under 365nm ultraviolet light excitation, enhancing the fluorescent anti-counterfeiting properties of the fiber. This invention uses conjugated small hexafluoroacetylacetone as the main ligand, which, under 254nm ultraviolet excitation, can simultaneously sensitize both Tb and Eu ions, while also reducing the impact of pigment luminescence on the fluorescent anti-counterfeiting performance.
[0087] Table 1. Color and luminescence of anti-counterfeiting fibers in pulp molding under natural light and UV 254 irradiation.
[0088]
[0089] As shown in Table 1, the anti-counterfeiting fibers inside the pulp molding in Example 1 exhibit red, green, and blue colors under natural light, with the three colors arranged in the same order. Furthermore, under 254nm illumination, blue, red, and green light emission at 430, 613, and 547nm can be observed.
[0090] In Comparative Example 1, during the preparation of green-red and blue-green modified cotton fibers, the beta-diketone ligand hexafluoroacetylacetone was replaced with 2-thiophenecarboxyltrifluoroacetone. The anti-counterfeiting fibers within the molded pulp lacked green color and exhibited weak red light under 254nm excitation. This is because 2-thiophenecarboxyltrifluoroacetone has high conjugation, and its optimal wavelength for exciting Eu3+ ions is 365nm. Therefore, when using 254nm UV secondary excitation, the red light of the green-red modified cotton fibers was weak. Furthermore, due to energy level matching, 2-thiophenecarboxyltrifluoroacetone could not effectively sensitize Tb ions, resulting in the blue-green modified cotton fibers emitting no green light and only the residual blue light of the terpyridine ligand. However, the blue dye in the blue-green modified cotton fibers strongly absorbs blue light, making luminescence unobservable.
[0091] In Comparative Example 2, during the preparation of green-red and blue-green cotton fibers, Eu and Tb ions were exchanged. The resulting anti-counterfeiting fibers showed no green light, and the position of the red light changed. This is because after the Eu and Tb ion exchange, the Tb ions in the green-red cotton fibers could emit green light, but this was affected by the absorption of the green pigment, making the green light unobservable. However, the blue-green cotton fibers emitted red light from the Eu ions, unaffected by the blue dye, and the red light was observable. Therefore, in pulp molding, three color segments (red, green, and blue) can be observed. Under 254nm ultraviolet excitation, the emission wavelengths are 430nm (no green light) and 613nm, respectively.
[0092] In Comparative Example 3, during the preparation of red-blue and blue-green modified cotton fibers, the pulp molded anti-counterfeiting fibers did not emit blue light when the red and blue dyes were exchanged, and the positions of the blue and red dyes were interchanged. Due to the exchange of red and blue dyes, their color positions changed under natural light, becoming three segments of blue, green, and red (although the red, green, and blue segments of the anti-counterfeiting fibers in the pulp molded fibers are the same as the blue, green, and red segments without change, it is impossible to determine the color position change, but the position color change can be determined by the arrangement of the luminescence sequence of the anti-counterfeiting fibers).
[0093] Replacing the water-retaining agent, polyacrylic acid cyclopropane resin, with sodium alginate in Comparative Example 4, and replacing the reinforcing agent, polyvinyl alcohol, with carboxymethyl cellulose in Comparative Example 5, resulted in a large number of carboxyl functional groups within the molded pulp. Due to the strong coordination reaction between rare earth ions Eu3+ and Tb3+ and carboxyl groups, the coordination structure between rare earth elements and hexafluoroacetylacetone was disrupted, leading to quenching of luminescence. Therefore, in Comparative Examples 4 and 5, luminescence of rare earth ions could not be observed under 254 nm UV excitation; only luminescence of the terpyridine group was observed. The three luminescent segments of the anti-counterfeiting fiber within the molded pulp were all at 430, 430, and 430 nm.
[0094] In Comparative Example 6, no ethylene glycol acrylate was added to the UV binder during the preparation of the anti-counterfeiting fiber. The surface of the prepared anti-counterfeiting fiber was coated with hydrophobic polybutyl acrylate, which could not be dispersed in the pulp molding slurry aqueous solution and ultimately could not be dispersed in the pulp molding process.
[0095] Example 2
[0096] Step 1, red-blue light modification of cotton fibers: Take 4 cotton yarns, each 1.5 meters long and of specification 60 / 4, and place them in 250 mL of dimethyl sulfoxide solution. Then add 30 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 4 mL of triethylamine. Raise the reaction temperature to 200 °C under a nitrogen atmosphere. After the reaction, wash three times with 400 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 1.5 L of deionized water, add 3 g of reactive red R-2BF dye and 3 g of sodium sulfate, raise the temperature to 50 °C, and react for 40 min. Then, further raise the temperature to 70 °C, add 2 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0097] Step 2, green-red light modification of cotton fibers, specifically: Take four 1.5-meter-long cotton yarns of specification 60 / 4 metric count and place them in 250 mL of dimethyl sulfoxide solution. Then add 30 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 4 mL of triethylamine. Raise the reaction temperature to 200℃ under a nitrogen atmosphere. After the reaction, wash three times with 400 mL of deionized water to obtain terpyridine-modified cotton fibers. Further place the terpyridine-modified cotton fibers in 1.5 L of deionized water and add 3 g of... Direct green BE dye and 3g of sodium sulfate were reacted at 50℃ for 40 minutes, then further heated to 70℃. 2g of sodium carbonate was added and the reaction was continued for another 40 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 150mL of deionized water, followed by the addition of 4g of hexafluoroacetylacetone, 2.5g of europium chloride, and 1.5mL of triethylamine. The mixture was heated to 70℃ and reacted for 2 hours. The fibers were then washed three times with 400mL of deionized water to obtain green-red modified cotton fibers.
[0098] Step 3, blue-green light modification of cotton fibers, specifically: Take four 1.5-meter-long cotton yarns of specification 60 / 4 metric count and place them in 250 mL of dimethyl sulfoxide solution. Then add 30 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 4 mL of triethylamine. Raise the reaction temperature to 200℃ under a nitrogen atmosphere. After the reaction, wash three times with 400 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 1.5 L of deionized water and add 3 g of active deep-dyeing agent. Blue R-2GLN dye and 3g of sodium sulfate were reacted at 50℃ for 40 minutes, then further heated to 70℃. 2g of sodium carbonate was added, and the reaction was continued for another 40 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading occurred. The resulting cotton fibers were then placed in 150mL of deionized water, followed by the addition of 4g of hexafluoroacetylacetone, 2.5g of terbium chloride, and 1.5mL of triethylamine. The mixture was heated to 70℃ and reacted for 1.5 hours. The fibers were then washed three times with 400mL of deionized water to obtain green-red modified cotton fibers.
[0099] Step 4, preparation of optical anti-counterfeiting fibers, specifically: Two red-blue light modified cotton fibers, two green-red light modified cotton fibers, and two blue-green light modified cotton fibers were each immersed in a UV adhesive solution for 8 seconds. The UV adhesive components were ethylene glycol acrylate (50g), butyl acrylate (45g), and azobisisobutyronitrile (5g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of an 8cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 30 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 0.8mm and a length of 2mm.
[0100] Step 5, preparation of pulp molding anti-counterfeiting material, specifically: Take 100g of pulp, the pulp can be any one or more of bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp, and break it up at 25℃ for 15min, adjust the pulping concentration to 10%, and after beating, the freeness is 55°SR. Then add acrylic cyclopropane resin (1.5g), polyvinyl alcohol (2.5g), polyacrylamide (0.3g), and optical anti-counterfeiting fiber with a width of 0.8mm and a length of 2mm (0.8g) to obtain a mixed pulp. The mixed slurry was then introduced into the mold of a micro pulp molding machine to filter water until the moisture content was 58%. After extrusion molding at 5.5 MPa, it was demolded and then dried in a drying oven at 75°C for 4.5 hours. Finally, it was transferred to a flat vulcanizing machine for hot pressing and shaping, with the temperature controlled at 105°C, the pressure at 5.8 MPa, and the time at 2.5 minutes, to obtain the pulp molded anti-counterfeiting material.
[0101] Example 3
[0102] Step 1, red-blue light modification of cotton fibers: Take 6 cotton yarns, each 2 meters long and of specification 60 / 4, and place them in 300 mL of dimethyl sulfoxide solution. Then add 40 g of 4'-chloro-2,2':6',2”-terpyridine and dropwise add 6 mL of triethylamine. Raise the reaction temperature to 220 °C under a nitrogen atmosphere. After the reaction, wash three times with 600 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 2 L of deionized water, add 4 g of reactive red R-2BF dye and 4 g of sodium sulfate, raise the temperature to 60 °C, and react for 60 min. Then, further raise the temperature to 80 °C, add 3 g of sodium carbonate, and react for 30 min. After the reaction, wash with soap detergent HM-900 until no pigment fades to obtain red-blue light modified cotton fibers.
[0103] Step 2, green-red light modification of cotton fibers, specifically: Take 6 cotton yarns, each 2 meters long and of specification 60 / 4, and place them in 300 mL of dimethyl sulfoxide solution. Then add 40 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 6 mL of triethylamine. Raise the reaction temperature to 220℃ under a nitrogen atmosphere. After the reaction, wash three times with 600 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the terpyridine-modified cotton fibers in 2 L of deionized water and add 4 g of... Direct green BE dye and 4g of sodium sulfate were reacted at 60℃ for 60 minutes, then further heated to 80℃, and 3g of sodium carbonate were added, reacting for another 60 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading occurred. The resulting cotton fibers were then placed in 200mL of deionized water, followed by the addition of 6g of hexafluoroacetylacetone, 3g of europium chloride, and 2mL of triethylamine. The mixture was heated to 80℃ and reacted for 3 hours. The fibers were then washed three times with 600mL of deionized water to obtain green-red modified cotton fibers.
[0104] Step 3, blue-green light modification of cotton fibers, specifically: Take 6 cotton yarns, each 2 meters long and of specification 60 / 4, and place them in 300 mL of dimethyl sulfoxide solution. Then add 40 g of 4'-chloro-2,2':6',2”-terpyridine, and dropwise add 6 mL of triethylamine. Raise the reaction temperature to 220 °C under a nitrogen atmosphere. After the reaction, wash three times with 600 mL of deionized water to obtain terpyridine-modified cotton fibers. Further, place the obtained terpyridine-modified cotton fibers in 2 L of deionized water and add 4 g of active... Deep blue R-2GLN dye and 4g of sodium sulfate were reacted at 60℃ for 60 minutes, then further heated to 80℃. 3g of sodium carbonate was added and the reaction continued for another 60 minutes. After the reaction, the mixture was washed with HM-900 soap until no pigment fading was observed. The resulting cotton fibers were then placed in 200mL of deionized water, followed by the addition of 6g of hexafluoroacetylacetone, 3g of terbium chloride, and 2mL of triethylamine. The mixture was heated to 80℃ and reacted for 3 hours. The fibers were then washed three times with 600mL of deionized water to obtain green-red modified cotton fibers.
[0105] Step 4, preparation of optical anti-counterfeiting fibers, specifically: Three red-blue light modified cotton fibers, three green-red light modified cotton fibers, and three blue-green light modified cotton fibers were each immersed in a UV adhesive solution for 8 seconds. The UV adhesive components were ethylene glycol acrylate (59g), butyl acrylate (40g), and azobisisobutyronitrile (10g). The UV-adhesive-impregnated cotton fibers were spirally wound onto the surface of a 10cm diameter cylindrical column and irradiated with a 45W, 365nm UV lamp for 40 seconds. Finally, a laser cutter was used to cut the fibers to obtain optical anti-counterfeiting fibers with a width of 1mm and a length of 3mm.
[0106] Step 5, preparation of pulp molded anti-counterfeiting material: Take 100g of pulp, selecting any one or more of bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp, and straw pulp. Break it up at 25℃ for 20 minutes, adjusting the pulp concentration to 12%. After beating, the freeness should be 60°SR. Then add 2g of cyclopropane acrylic resin, 3g of polyvinyl alcohol, 0.4g of polyacrylamide, and 1g of optical anti-counterfeiting fiber with a width of 1mm and a length of 3mm to obtain a mixed pulp. Then, pour the mixed pulp into the mold of a micro pulp molding machine, filter to a moisture content of 60%, extrude at 6MPa, demold, and dry in a drying oven at 80℃ for 5 hours. Finally, transfer to a flat vulcanizing machine for hot pressing and shaping, controlling the temperature at 110℃, the pressure at 6MPa, and the time at 3 minutes to obtain the pulp molded anti-counterfeiting material.
Claims
1. A method for preparing a pulp molding material with anti-counterfeiting function, characterized in that: The specific steps include: Step 1, red-blue light modification of cotton fibers; Step 2, green-red light modification of cotton fibers; Step 3, modifying the cotton fiber with blue-green light; Step 4, preparing an optical anti-counterfeiting fiber according to the products obtained in steps 1 to 3; Step 5, preparing a pulp molded anti-counterfeiting material according to the product obtained in step 4.
2. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 1, characterized in that: The specific process of step 1 is as follows: Step 1.1, take 3-6 cotton yarns with a length of 1-2 meters and a specification of 60 / 4 male yarn, put them into 200-300 mL of dimethyl sulfoxide solution, then add 20-40 g of 4'-chloro-2,2':6',2"-terpyridine, add 3-6 mL of triethylamine dropwise, raise the reaction temperature to 180-220° C. under a nitrogen atmosphere, and wash them with 300-600 mL of deionized water 3 times after the reaction to obtain terpyridine-modified cotton fibers; Step 1.2, the terpyridine modified cotton fiber obtained in step 1.1 is placed in 1-2L deionized water, 2-4g of reactive red R-2BF dye and 2-4g of sodium sulfate are added, the temperature is raised to 40-60°C, and after reacting for 30-60min, the temperature is raised to 60-80°C, 1.5-3g of sodium carbonate is added and reacted for 30min, and after the reaction is completed, it is washed with soaping agent HM-900 until no pigment fades, thereby obtaining red-blue light modified cotton fiber.
3. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 1, characterized in that: The specific process of step 2 is as follows: Step 2.1, take 3-6 cotton yarns with a length of 1-2 meters and a specification of 60 / 4 male yarn, put them into 200-300 mL of dimethyl sulfoxide solution, then add 20-40 g of 4'-chloro-2,2':6',2"-terpyridine, add 3-6 mL of triethylamine dropwise, raise the reaction temperature to 180-220° C. under a nitrogen atmosphere, and wash them with 300-600 mL of deionized water 3 times after the reaction to obtain terpyridine-modified cotton fibers; Step 2.2, putting the terpyridine modified cotton fiber obtained in step 2.1 into 1-2L deionized water, adding 2-4g of direct green BE dye and 2-4g of sodium sulfate, raising the temperature to 40-60°C, reacting for 30-60min, raising the temperature to 60-80°C, adding 1.5-3g of sodium carbonate and reacting for 30-60min, and washing with soaping agent HM-900 after the reaction is completed until no pigment fades; Step 2.3, put the cotton fiber obtained after the treatment in step 2.2 into 100-200 mL of deionized water, then add 3-6 g of hexafluoroacetylacetone, 2-3 g of europium chloride and 1-2 mL of triethylamine in sequence, heat the temperature to 60-80 ° C for 1-3 hours, wash three times with 300-600 mL of deionized water to obtain green-red light modified cotton fiber.
4. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 1, characterized in that: The specific process of step 3 is as follows: Step 3.1, take 3-6 cotton yarns with a length of 1-2 meters and a specification of 60 / 4 male yarn, put them into 200-300 mL of dimethyl sulfoxide solution, then add 20-40 g of 4'-chloro-2,2':6',2"-terpyridine, add 3-6 mL of triethylamine dropwise, raise the reaction temperature to 180-220° C. under a nitrogen atmosphere, and wash them three times with 300-600 mL of deionized water after the reaction is completed to obtain terpyridine-modified cotton fibers; Step 3.2, putting the terpyridine modified cotton fiber obtained in step 3.1 into 1-2L deionized water, adding 2-4g of active dark blue R-2GLN dye and 2-4g of sodium sulfate, raising the temperature to 40-60°C, reacting for 30-60min, raising the temperature to 60-80°C, adding 1.5-3g of sodium carbonate and reacting for 30-60min, and washing with soaping agent HM-900 after the reaction is completed until no pigment fades; Step 3.3, put the cotton fiber treated in step 3.2 into 100-200 mL of deionized water, then add 3-6 g of hexafluoroacetylacetone, 2-3 g of terbium chloride and 1-2 mL of triethylamine in sequence, heat the temperature to 60-80 ° C and react for 1-3 hours, wash three times with 300-600 mL of deionized water to obtain blue-green light modified cotton fiber.
5. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 1, characterized in that: The specific process of step 4 is as follows: Step 4.1, immersing 1-3 red-blue light modified cotton fibers, 1-3 green-red light modified cotton fibers, and 1-3 blue-green light modified cotton fibers in a UV adhesive solution for 2-10 seconds respectively; Step 4.2, winding the cotton fiber impregnated with UV adhesive obtained in step 4.1 on the surface of a circular column with a diameter of 5-10 cm in a spiral winding form, and irradiating it with ultraviolet light for 20-40 seconds to obtain an optical anti-counterfeiting fiber.
6. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 5, characterized in that: In the step 4.1, the preparation process of the UV adhesive is as follows: 40-59 g of ethylene glycol acrylate, 40-59 g of butyl acrylate and 1-10 g of azobisisobutyronitrile are uniformly mixed to obtain the UV adhesive.
7. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 1, characterized in that: The specific process of step 5 is as follows: Step 5.1, taking 100-200 g of pulp, breaking it at 25° C. for 10-20 min, adjusting the pulping concentration to 8-12%, and the beating degree after pulping to 50-60° SR; Step 5.2, adding 1-2 g of cyclopropane acrylic acid resin, 2-3 g of polyvinyl alcohol, 0.2-0.4 g of polyacrylamide and 0.5-1 g of optical anti-counterfeiting fiber having a width of 0.1-1 mm and a length of 1-3 mm to the slurry obtained in step 5.1 to obtain a mixed slurry; Step 5.3, introduce the mixed slurry obtained in step 5.2 into the mold of a micro pulp molding machine and filter the water to a moisture content of 55-60%, then demold after extrusion molding at 5-6 MPa, and then dry in a drying oven at 70-80°C for 4-5 hours, and finally transfer to a flat vulcanizer for hot pressing and shaping, controlling the temperature to 100-110°C, the pressure to 5.5-6 MPa, and the time to 2-3 minutes to obtain a pulp molded anti-counterfeiting material.
8. The method for preparing a pulp molding material with anti-counterfeiting function according to claim 7, characterized in that: The pulp can be any one or more of bamboo pulp, sugarcane pulp, wood pulp, waste corrugated paper pulp, newspaper pulp and straw pulp.
Citation Information
Patent Citations
Pigmentation method for paper-pulp moulding product
CN101245569A
Positioning distributed fiber anti-counterfeiting paper and manufacturing method thereof
CN102182114A
Molded pulp product with anti-counterfeiting function and preparation method thereof
CN103031782A
Preparation method of degradable plastic filling material taking waste bank note paper as substrate
CN104893241A
Method for producing 20 tons of molded pulp products per day
CN105568777A