Exhaust pipeline prepared from basalt fibers and manufacturing method of exhaust pipeline

Through the combination of basalt fiber material and modified epoxy resin, the problems of large weight and poor corrosion resistance of traditional metal exhaust pipes are solved, and the high temperature and corrosion resistance of exhaust pipes are improved, thus achieving lightweight and efficient exhaust Pipe design.

CN118997903APending Publication Date: 2024-11-22BEIJING LIHAOJIAYUAN BUILDING MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411099820.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional metal exhaust pipes have large weight and poor corrosion resistance. The high-temperature resistant paint layer is prone to fall off and leads to rust, which cannot effectively resist the chemical corrosion of sulfides and phosphides.

Method used

The basalt fiber material is used to wove and modify the flexible chain segment epoxy resin to form a basalt fiber braided layer and a tube wall reinforcement layer, combined with a high-temperature resistant paint layer, to improve the high temperature resistance, corrosion resistance and strength of the exhaust pipes.

Benefits of technology

It has achieved high temperature and corrosion performance improvements in the exhaust pipe, reduced weight, and ensured corrosion resistance. Even if the high-temperature resistant paint layer falls off, it will not affect use, and has high market potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118997903A_ABST
    Figure CN118997903A_ABST
Patent Text Reader

Abstract

The exhaust pipeline comprises a basalt fiber braid layer, a pipe wall reinforcing layer and a high-temperature-resistant paint layer, the basalt fiber braid layer is formed by conducting high-density winding and weaving on basalt fiber spun yarn according to the diameter of the pipeline and then conducting impregnation and curing, the thickness of the basalt fiber braid layer is 1-1.5 mm, and the diameter of the pipe wall reinforcing layer is 1-1.5 mm. The pipe wall reinforcing layers are distributed on the inner side and the outer side of the basalt fiber woven layer, the pipe wall reinforcing layers are formed by curing after being coated with modified epoxy resin, the thickness of the pipe wall reinforcing layers is 0.5-1 mm, and the inner side and the outer side of each pipe wall reinforcing layer are sprayed with high-temperature-resistant paint layers; the basalt fiber material is used as a base material for weaving and modifying the epoxy resin containing the flexible chain segment, so that the base material of the exhaust pipeline has good high-temperature resistance and corrosion resistance, even if a high-temperature-resistant paint layer sprayed outside falls off due to long-time use, the high-temperature-resistant paint layer is still excellent in high-temperature resistance and corrosion resistance, and the service life of the exhaust pipeline is prolonged. And the corrosion resistance of the manufactured exhaust pipeline is improved while the self weight is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile exhaust pipes, and in particular to an exhaust pipe made of basalt fiber and a manufacturing method thereof. Background Art

[0002] Exhaust pipes are widely used in automobiles, ships, airplanes and other fields. Exhaust pipes are important components connecting engines and mufflers, and their performance directly affects the emission performance and noise level of automobiles. Since the exhaust gas emitted by automobiles contains sulfides and phosphides, these substances will remain in the automobile exhaust pipes and cause chemical corrosion and electrochemical corrosion, damaging the exhaust pipes. Therefore, the exhaust pipes are required to have good high temperature resistance, corrosion resistance, light weight and high strength.

[0003] Traditional metal exhaust pipes have the problem of being heavy, and although a corrosion-resistant coating is sprayed on the surface of the exhaust pipe, the corrosion-resistant coating will fall off after long-term use, exposing the internal metal, which will rust when encountering residual substances, resulting in poor corrosion resistance. This is also a fatal problem of existing metal exhaust pipes. Therefore, the present invention proposes an exhaust pipe made of basalt fiber and a manufacturing method thereof to solve the problems existing in the prior art. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to propose an exhaust duct made of basalt fiber and a manufacturing method thereof. The exhaust duct made of basalt fiber and the manufacturing method thereof are woven by basalt fiber material as a base material and modified with a flexible segment epoxy resin, so that the substrate of the exhaust duct itself has good high temperature resistance and corrosion resistance. Even if the high temperature resistant paint layer sprayed on the outside falls off due to long-term use, it will not affect the use of the exhaust duct, and its high temperature resistance and corrosion resistance are still excellent. At the same time, the flexible segment epoxy resin modified by basalt fiber chopped yarn can greatly increase the strength of the exhaust duct after curing. The manufactured exhaust duct has improved corrosion resistance while reducing its own weight.

[0005] To achieve the purpose of the present invention, the present invention is implemented through the following technical scheme: an exhaust pipe prepared by basalt fiber, comprising a basalt fiber braided layer, a pipe wall reinforcement layer and a high-temperature resistant paint layer, wherein the basalt fiber braided layer is made by spinning basalt fibers according to the pipe diameter, winding and braiding at a high density, and then dipping and curing, the thickness of the basalt fiber braided layer is 1-1.5mm, the pipe wall reinforcement layer is distributed on the inside and outside of the basalt fiber braided layer, the pipe wall reinforcement layer is formed by coating with a modified epoxy resin and then curing, the thickness of the pipe wall reinforcement layer is 0.5-1mm, and the inside and outside of the pipe wall reinforcement layer are sprayed with a high-temperature resistant paint layer.

[0006] Further improvements are as follows: the basalt fiber braided layer is impregnated with an epoxy resin containing a flexible segment; the modified epoxy resin is made of basalt fiber chopped yarn and a corrosion-resistant filler modified with an epoxy resin containing a flexible segment; the corrosion-resistant filler is one of nano-scale silicon dioxide and titanium dioxide.

[0007] A method for manufacturing an exhaust pipe made of basalt fiber comprises the following steps:

[0008] Step 1, preparation of epoxy resin raw materials: using toluene diisocyanate and polypropylene glycol to react to prepare isocyanate-terminated polyether, and then mixing the isocyanate-terminated polyether with epoxy resin to prepare epoxy resin containing flexible segments;

[0009] Step 2: Preparation of basalt fiber braided layer: Using a pipe smaller than the diameter of the exhaust pipe as a base frame, high-density woven basalt fiber spinning is performed on the base frame, and then the yarn is immersed in epoxy resin containing flexible segments and taken out for curing treatment, and finally the basalt fiber braided layer is obtained by removing the yarn from the pipe;

[0010] Step 3, preparation of modified epoxy resin: adding chopped basalt fiber yarn and corrosion-resistant filler into epoxy resin containing flexible chain segments, and then fully stirring the epoxy resin to obtain modified epoxy resin;

[0011] Step 4: Coating the pipe wall reinforcement layer: uniformly coat the modified epoxy resin prepared in step 3 on the inner and outer surfaces of the basalt fiber braided layer and then cure it. Repeat the coating and curing for 3-5 times to obtain a semi-finished exhaust pipe.

[0012] Step 5. Post-processing of semi-finished products: Smoothly grind and polish the inner and outer surfaces of the semi-finished exhaust pipe, and finally spray a layer of high-temperature resistant paint on the inner and outer surfaces. After drying, the exhaust pipe is obtained.

[0013] The further improvement is that the specific preparation process in step 1 is:

[0014] S1. First, toluene diisocyanate is heated to 70°C under nitrogen protection, and then polypropylene glycol is slowly added dropwise with stirring, and the reaction is allowed to proceed for 3 hours to obtain an isocyanate-terminated polyether;

[0015] S2, then heating the epoxy resin to 70° C. under nitrogen protection, adding the terminal isocyanate polyether thereto, and adding a catalyst to react for 2 hours to obtain a high-purity epoxy resin containing a flexible segment;

[0016] S3. Finally, the high-purity epoxy resin containing flexible segments is mixed with a curing agent and diluted with a diluent to obtain an epoxy resin containing flexible segments.

[0017] Further improvements are as follows: the reaction mass ratio of toluene diisocyanate and polypropylene glycol in S1 is 2:1; the catalyst is dibutyltin dilaurate, and its addition amount is 0.1% of the total mixed amount of terminal isocyanate polyether and epoxy resin; the mass ratio of high-purity flexible segment epoxy resin, curing agent and diluent in S3 is 70:10:20, wherein the curing agent is modified fatty amine epoxy resin curing agent, and the diluent is benzyl glycidyl ether.

[0018] Further improvements are as follows: the outer diameter of the pipe used as the base frame in step 2 is 0.5-1 mm smaller than the inner diameter of the exhaust pipe to be produced; a layer of release agent is applied to the outer side of the pipe of the base frame before spinning the basalt fibers; and the curing treatment conditions in step 2 and step 4 are curing at 80°C for 3 hours.

[0019] Further improvements are: in step three, the mass ratio of the flexible segment epoxy resin, the basalt fiber chopped yarn and the corrosion-resistant filler is 75:15:10; in step four, the single coating layer is controlled between 0.2-0.4 mm.

[0020] The further improvement lies in that: in the step five, 600-mesh sandpaper is first used for coarse grinding, and then 2000-mesh sandpaper and 3000-mesh sandpaper are used for fine grinding respectively, and finally 5000-mesh sandpaper is used for polishing; after grinding and polishing, the pipeline is cleaned and dried, and then a high-temperature resistant paint made of a mixture of polytitanate, graphite, zinc powder, silicone resin, black pigment, curing agent and solvent is sprayed on the surface of the pipeline after grinding and polishing; wherein the mass ratio of polytitanate, graphite, zinc powder, silicone resin, black pigment, curing agent and solvent is 60:8:5:15:5:4:3.

[0021] The beneficial effects of the present invention are as follows: the present invention uses basalt fiber material as a base material for weaving and modifying the epoxy resin containing a flexible chain segment, so that the substrate of the exhaust pipe itself has excellent high temperature resistance and corrosion resistance. Even if the high temperature resistant paint layer sprayed on the outside falls off due to long-term use, it will not affect the use of the exhaust pipe, and its high temperature resistance and corrosion resistance are still excellent. At the same time, the epoxy resin containing a flexible chain segment modified by the basalt fiber chopped yarn can greatly increase the strength of the exhaust pipe after curing. The manufactured exhaust pipe has improved corrosion resistance while reducing its own weight. It has a high market potential in the fields of automobile engines and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a cross-sectional structural diagram of the pipeline of the present invention.

[0023] Figure 2 This is a flow chart of the production method of Example 1 of the present invention.

[0024] Figure 3This is a flow chart of the production method of Example 2 of the present invention. DETAILED DESCRIPTION

[0025] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0026] Example 1

[0027] according to Figure 1 As shown, this embodiment provides an exhaust pipe made of basalt fiber, including a basalt fiber braided layer, a pipe wall reinforcement layer and a high-temperature resistant paint layer. The basalt fiber braided layer is made by spinning basalt fibers according to the pipe diameter, winding and braiding them at a high density, and then dipping and curing them. The thickness of the basalt fiber braided layer is 1-1.5mm, and the pipe wall reinforcement layer is distributed on the inside and outside of the basalt fiber braided layer. The pipe wall reinforcement layer is formed by coating modified epoxy resin and then curing it. The thickness of the pipe wall reinforcement layer is 0.5-1mm, and the inside and outside of the pipe wall reinforcement layer are sprayed with a high-temperature resistant paint layer.

[0028] The basalt fiber braided layer is impregnated with epoxy resin containing flexible segments; the modified epoxy resin is made of basalt fiber chopped yarn and corrosion-resistant filler modified with epoxy resin containing flexible segments; the corrosion-resistant filler is nano-scale silicon dioxide.

[0029] according to Figure 2 As shown, this embodiment provides a method for manufacturing an exhaust pipe made of basalt fiber, which is characterized by comprising the following steps:

[0030] Step 1, preparation of epoxy resin raw materials: using toluene diisocyanate and polypropylene glycol to react to prepare isocyanate-terminated polyether, and then mixing the isocyanate-terminated polyether with epoxy resin to prepare epoxy resin containing flexible segments;

[0031] The specific preparation process is:

[0032] S1. First, toluene diisocyanate is heated to 70°C under nitrogen protection, and then polypropylene glycol is slowly added dropwise and stirred. The reaction is allowed to proceed for 3 hours to obtain an isocyanate-terminated polyether, wherein the reaction mass ratio of toluene diisocyanate to polypropylene glycol is 2:1.

[0033] S2, then heating the epoxy resin to 70° C. under nitrogen protection, adding the isocyanate-terminated polyether thereto, and adding 0.1% of dibutyltin dilaurate catalyst based on the total amount of the isocyanate-terminated polyether and the epoxy resin to react for 2 hours to obtain a high-purity epoxy resin containing a flexible segment;

[0034] S3, finally mixing the high-purity epoxy resin containing the flexible segment with the curing agent and diluting with a diluent to obtain the epoxy resin containing the flexible segment;

[0035] The mass ratio of high-purity epoxy resin containing flexible segments, curing agent and diluent is 70:10:20, wherein the curing agent is modified fatty amine epoxy resin curing agent, and the diluent is benzyl glycidyl ether.

[0036] Step 2: Preparation of basalt fiber braided layer: a pipe smaller than the diameter of the exhaust pipe is used as a base frame and a layer of release agent is coated on the outside of the pipe, basalt fiber spinning is woven on the base frame at a high density, and then it is immersed in epoxy resin containing flexible chain segments and taken out for curing treatment, and finally removed from the pipe to obtain the basalt fiber braided layer;

[0037] The outer diameter of the pipe used as the base frame is 0.5-1 mm smaller than the inner diameter of the exhaust pipe to be manufactured; the curing treatment condition is curing at 80° C. for 3 hours.

[0038] Step 3, preparation of modified epoxy resin: adding chopped basalt fiber yarn and nano-scale silica to the epoxy resin containing the flexible chain segment, and then fully stirring the epoxy resin to obtain the modified epoxy resin;

[0039] The mass ratio of the flexible segment epoxy resin, basalt fiber chopped yarn and nano-silicon dioxide is 75:15:10.

[0040] Step 4: Coating of the pipe wall reinforcement layer: evenly coat the modified epoxy resin prepared in step 3 on the inner and outer surfaces of the basalt fiber braided layer and then cure it. Repeat the coating and curing for 3-5 times to obtain a semi-finished exhaust pipe. The single coating layer is controlled between 0.2-0.4mm, and the curing condition is to cure at 80°C for 3h.

[0041] Step 5, post-processing of semi-finished products: Smoothly grind and polish the inner and outer surfaces of the semi-finished exhaust pipe, and finally spray a layer of high-temperature resistant paint on the inner and outer surfaces, and obtain the exhaust pipe after drying;

[0042] The specific grinding and polishing process is to use 600-grit sandpaper for rough grinding, then use 2000-grit sandpaper and 3000-grit sandpaper for fine grinding, and finally use 5000-grit sandpaper for polishing, and then clean and dry the pipe;

[0043] The sprayed high temperature resistant paint layer is made of polytitanate, graphite, zinc powder, silicone resin, black pigment, curing agent and solvent in a mass ratio of 60:8:5:15:5:4:3.

[0044] Example 2

[0045] The present embodiment provides an exhaust pipe made of basalt fiber, including a basalt fiber braided layer, a pipe wall reinforcement layer and a high-temperature resistant paint layer. The basalt fiber braided layer is made by spinning basalt fibers at a high density, winding and braiding according to the pipe diameter, and then dipping and curing. The thickness of the basalt fiber braided layer is 1-1.5 mm. The pipe wall reinforcement layer is distributed on the inside and outside of the basalt fiber braided layer. The pipe wall reinforcement layer is formed by coating modified epoxy resin and then curing. The thickness of the pipe wall reinforcement layer is 0.5-1 mm. The inside and outside of the pipe wall reinforcement layer are sprayed with a high-temperature resistant paint layer.

[0046] The basalt fiber braided layer is impregnated with high temperature resistant epoxy resin; the modified epoxy resin is made of basalt fiber chopped yarn and corrosion resistant filler modified high temperature resistant epoxy resin; the corrosion resistant filler is nano-grade titanium dioxide.

[0047] according to Figure 2 As shown, this embodiment provides a method for manufacturing an exhaust pipe made of basalt fiber, which is characterized by comprising the following steps:

[0048] Step 1, preparation of epoxy resin raw materials, using epoxy resin and high temperature resistant curing agent to mix and stir to obtain high temperature resistant epoxy resin; wherein the mass ratio of epoxy resin to high temperature resistant curing agent is 80:20, wherein the high temperature resistant curing agent is made by mixing aromatic polyamine, hydroxyl, 70 acid anhydride and terminal carboxyl liquid nitrile rubber in a mass ratio of 20:10:15:55.

[0049] Step 2: Making a basalt fiber braided layer: using a pipe smaller than the exhaust pipe diameter as a base frame and coating the outside of the pipe with a layer of release agent, weaving basalt fiber spinning at a high density on the base frame, then immersing it in a high temperature resistant epoxy resin and taking it out for curing treatment, and finally removing it from the pipe to obtain the basalt fiber braided layer;

[0050] The outer diameter of the pipe used as the base frame is 0.5-1 mm smaller than the inner diameter of the exhaust pipe to be manufactured; the curing treatment condition is curing at 80° C. for 3 hours.

[0051] Step 3, preparation of modified epoxy resin, adding chopped basalt fiber yarn and nano-sized titanium dioxide into high temperature resistant epoxy resin, and then fully stirring the mixture to obtain modified epoxy resin;

[0052] The mass ratio of high temperature resistant epoxy resin, basalt fiber chopped yarn and nano-grade titanium dioxide is 75:15:10.

[0053] Step 4: coating the pipe wall reinforcement layer. The modified epoxy resin prepared in step 3 is evenly coated on the inner and outer surfaces of the basalt fiber braided layer and then cured. After repeated coating and curing for 3-5 times, a semi-finished exhaust pipe is obtained. The single coating layer is controlled between 0.2-0.4mm, and the curing treatment condition is to cure at 80°C for 3h.

[0054] Step 5: Post-processing of the semi-finished product: smoothing and polishing the inner and outer surfaces of the semi-finished exhaust pipe, and finally spraying a layer of high-temperature resistant paint on the inner and outer surfaces, and obtaining the exhaust pipe after drying;

[0055] The specific grinding and polishing process is to use 600-grit sandpaper for rough grinding, then use 2000-grit sandpaper and 3000-grit sandpaper for fine grinding, and finally use 5000-grit sandpaper for polishing, and then clean and dry the pipe;

[0056] The sprayed high temperature resistant paint layer is made of polytitanate, graphite, zinc powder, silicone resin, black pigment, curing agent and solvent in a mass ratio of 60:8:5:15:5:4:3.

[0057] In order to verify the performance of the exhaust pipes prepared in Examples 1 and 2 of the present application and the traditional metal exhaust pipes, high temperature tests, corrosion resistance tests and weight tests were performed on the three exhaust pipes. During the high temperature test, the exhaust pipes were heat-baked to observe whether they were softened. During the corrosion resistance test, a piece of the corrosion-resistant and high-temperature coating on the surfaces of the three exhaust pipes was scraped off, and a corrosive agent was dropped on the scraped-off coating and left to stand to observe the degree of corrosion. During the weight test, the three exhaust pipes were directly weighed, and the test results are shown in the following table.

[0058] Three types of exhaust pipe inspection test table

[0059] Example 1 Exhaust duct Example 2 Exhaust duct Metal exhaust pipe High temperature testing No softening Slight softening No softening Corrosion resistance test No erosion points No erosion points More corrosion spots Weight detection (kg / m) 1.63 1.66 2.83

[0060] As can be seen from the above table, the high temperature test of the exhaust pipe prepared in Example 1 of the present application is good, while the high temperature resistance of the exhaust pipe prepared in Example 2 is slightly inferior to that of the exhaust pipe in Example 1. It can be seen that the heat resistance of the epoxy resin mixed with the high temperature resistant curing agent cannot meet the standard, and the heat resistance of the epoxy resin containing the flexible segment directly prepared by changing the epoxy resin structure by chemical synthesis is better than that of the epoxy resin mixed with the high temperature resistant curing agent;

[0061] At the same time, the addition of corrosion-resistant fillers makes the exhaust pipe made of basalt fiber epoxy resin more corrosion-resistant than metal exhaust pipes, and its weight is more lightweight than that of metal exhaust pipes.

[0062] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. An exhaust pipe made of basalt fiber, characterized in that: It includes a basalt fiber braided layer, a pipe wall reinforcement layer and a high-temperature resistant paint layer. The basalt fiber braided layer is made by spinning basalt fibers according to the pipe diameter, winding and braiding them at a high density, and then dipping and curing them. The thickness of the basalt fiber braided layer is 1-1.5mm. The pipe wall reinforcement layer is distributed inside and outside the basalt fiber braided layer. The pipe wall reinforcement layer is formed by coating modified epoxy resin and then curing. The thickness of the pipe wall reinforcement layer is 0.5-1mm. The inside and outside of the pipe wall reinforcement layer are sprayed with a high-temperature resistant paint layer.

2. The exhaust pipe made of basalt fiber according to claim 1, characterized in that: The basalt fiber braided layer is impregnated with epoxy resin containing flexible segments; the modified epoxy resin is made of basalt fiber chopped yarn and corrosion-resistant filler modified epoxy resin containing flexible segments; the corrosion-resistant filler is one of nano-scale silicon dioxide and titanium dioxide.

3. A method for manufacturing an exhaust pipe made of basalt fiber, characterized in that: The following steps are involved: Step 1: preparing epoxy resin raw materials, using toluene diisocyanate and polypropylene glycol to react to prepare terminal isocyanate polyether, and then mixing the isocyanate polyether with epoxy resin to prepare epoxy resin containing flexible segments; Step 2: Making a basalt fiber braided layer: using a pipe smaller than the diameter of the exhaust pipe as a base frame, weaving basalt fiber spinning at a high density on the base frame, then immersing it in an epoxy resin containing a flexible chain segment and taking it out for curing treatment, and finally removing it from the pipe to obtain the basalt fiber braided layer; Step 3, preparation of modified epoxy resin, adding basalt fiber chopped yarn and corrosion-resistant filler into epoxy resin containing flexible segments, and then fully stirring the epoxy resin to obtain modified epoxy resin; Step 4: coating the pipe wall reinforcement layer. The modified epoxy resin prepared in step 3 is evenly coated on the inner and outer surfaces of the basalt fiber braided layer and then cured. The semi-finished exhaust pipe is obtained after repeated coating and curing for 3-5 times. Step 5: Post-processing of the semi-finished product: Smoothly grind and polish the inner and outer surfaces of the semi-finished exhaust pipe, and finally spray a layer of high-temperature resistant paint on the inner and outer surfaces. After drying, the exhaust pipe is obtained.

4. The method for manufacturing an exhaust pipe made of basalt fiber according to claim 3, characterized in that: The specific preparation process in step 1 is as follows: S1. First, toluene diisocyanate is heated to 70°C under nitrogen protection, and then polypropylene glycol is slowly added dropwise with stirring, and the reaction is allowed to proceed for 3 hours to obtain an isocyanate-terminated polyether; S2, then heating the epoxy resin to 70° C. under nitrogen protection, adding the terminal isocyanate polyether thereto, and adding a catalyst to react for 2 hours to obtain a high-purity epoxy resin containing a flexible segment; S3. Finally, the high-purity epoxy resin containing flexible segments is mixed with a curing agent and diluted with a diluent to obtain an epoxy resin containing flexible segments.

5. The method for manufacturing an exhaust pipe made of basalt fiber according to claim 4, characterized in that: The reaction mass ratio of toluene diisocyanate and polypropylene glycol in S1 is 2:1; the catalyst is dibutyltin dilaurate, and its addition amount is 0.1% of the total mixed amount of terminal isocyanate polyether and epoxy resin; the mass ratio of high-purity epoxy resin containing flexible segments, curing agent and diluent in S3 is 70:10:20, wherein the curing agent is modified fatty amine epoxy resin curing agent, and the diluent is benzyl glycidyl ether.

6. The method for manufacturing an exhaust pipe made of basalt fiber according to claim 3, characterized in that: The outer diameter of the pipe used as the base frame in step 2 is 0.5-1 mm smaller than the inner diameter of the exhaust pipe to be manufactured; a layer of release agent is applied to the outer side of the pipe of the base frame before spinning the basalt fibers; the curing treatment conditions in step 2 and step 4 are curing at 80° C. for 3 hours.

7. The method for manufacturing an exhaust pipe made of basalt fiber according to claim 3, characterized in that: In the step three, the mass ratio of the flexible segment epoxy resin, the basalt fiber chopped yarn and the corrosion-resistant filler is 75:15:10; in the step four, the single coating layer is controlled between 0.2-0.4 mm.

8. The method for manufacturing an exhaust pipe made of basalt fiber according to claim 3, characterized in that: In the step 5, 600-mesh sandpaper is first used for coarse grinding, and then 2000-mesh sandpaper and 3000-mesh sandpaper are used for fine grinding, and finally 5000-mesh sandpaper is used for polishing; after grinding and polishing, the pipeline is cleaned and dried, and then a high-temperature resistant paint mixed with polytitanate, graphite, zinc powder, silicone resin, black pigment, curing agent and solvent is sprayed on the surface of the pipeline after grinding and polishing; wherein the mass ratio of polytitanate, graphite, zinc powder, silicone resin, black pigment, curing agent and solvent is 60:8:5:15:5:4:3.

Citation Information

Cited By

  • Composite pipeline material as well as preparation method and application thereof

    CN119659098A