A method for manufacturing a stepped substrate with a cavity
By optimizing the bonding process and the method of dissolving uncured material at the bottom of the dissolution tank, the problem of adhesive overflow in bonding materials was solved, thus achieving stability and reliability of chip packaging.
Patent Information
- Application Number
- CN202410941853.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-07-15
AI Technical Summary
During chip packaging, bonding material overflows into deep trenches, causing the overflow at the bottom of the trench to affect chip mounting and wire bonding, a problem that is difficult to solve effectively with existing technologies.
By optimizing the bonding process, low-temperature and low-pressure bonding layers and window plates are used to dissolve the uncured bonding material at the bottom of the bonding tank after bonding, forming a cavity substrate to avoid adhesive overflow. A vacuum laminator is used to ensure tight bonding.
This effectively reduces adhesive overflow from bonding materials, ensuring proper chip mounting and wire bonding, and improving the reliability and stability of the package.
Smart Images

Figure CN119008419B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of semiconductor packaging technology, and specifically relates to a method for manufacturing a stepped substrate with a cavity. Background Technology
[0002] Among various packaging structures, one type of chip packaging requires creating a deep trench structure on the substrate surface. The chip is then attached and wire-bonded within the cavity formed by the trench. However, the space within the deep trench is limited, hindering the development of... Figure 1 As shown, the bonding materials used for bonding the top and bottom plates of the bonding slot are squeezed into the slot during the bonding process, forming excess adhesive. In mild cases, this can encroach on the deep slot space, cover the electrodes in the slot, and affect chip mounting and wire bonding; in severe cases, the overflowing adhesive can fill the deep slot, rendering the deep slot unusable. Summary of the Invention
[0003] Therefore, the technical problem to be solved by this application is to provide a method for manufacturing a stepped substrate with a cavity, which reduces the overflow of bonding material into the groove by specially optimizing the process conditions, and removes the overflow of bonding material at the bottom of the groove by dissolving the bonding material at the bottom of the groove before the bonding layer is cured, thus avoiding the inability of chip mounting and wire bonding caused by the overflow of bonding material at the bottom of the groove.
[0004] To address the aforementioned problems, this application provides a method for manufacturing a stepped substrate with a cavity, comprising:
[0005] Bonding layers are laminated onto the substrate;
[0006] A window panel is laminated on the side of the bonding layer away from the substrate;
[0007] Dissolve the bonding material on the bonding layer at the position relative to the window of the windowed plate;
[0008] Curing bonding layer.
[0009] Optionally, the bonding material can be a dry model photosensitive resin or a thermosetting resin.
[0010] Optionally, the bonding temperature of the bonding layer and the window plate is lower than the conventional bonding temperature of the bonding layer and the window plate, which is 60℃~80℃.
[0011] The bonding pressure of the bonding layer and the window plate is greater than the conventional bonding pressure of the bonding layer and the window plate, which is 0.2MPa to 0.6MPa.
[0012] Optionally, the bonding layer and the window panel can be bonded together using a vacuum laminator.
[0013] Optionally, when dissolving the bonding material on the bonding layer at the position relative to the window of the windowed plate, the window of the windowed plate is set to face downward.
[0014] Optionally, the curing temperature of the bonding layer is 150℃~250℃, and the curing time of the bonding layer is 30min~120min.
[0015] Optionally, the method further includes:
[0016] Drill through holes in the stepped substrate with cavities along the vertical direction;
[0017] Through-hole metallization to form solder pads.
[0018] Optionally, the method further includes:
[0019] A solder resist layer is fabricated on the top and bottom surfaces of a stepped substrate with a cavity, in the area outside the pad projection.
[0020] Optionally, the method further includes:
[0021] Coating is applied to the surface of the solder pads.
[0022] Optionally, the method further includes:
[0023] Balls are placed on the surface of the solder pads.
[0024] Beneficial effects
[0025] The cavity-based stepped substrate manufacturing method provided in the embodiments of the present invention, through optimized bonding process, effectively reduces adhesive overflow in the window opening after the window plate is bonded, and before the bonding layer is cured, dissolves the uncured bonding material at the bottom of the tank, thereby removing the bonding material and overflowing adhesive at the bottom of the tank, and avoiding adhesive overflow at the bottom of the tank that would prevent the chip from being mounted and wire bonded. Attached Figure Description
[0026] Figure 1 A schematic diagram of a stepped substrate with a cavity, produced using traditional manufacturing methods;
[0027] Figure 2 A flowchart illustrating a method for manufacturing a stepped substrate with a cavity, according to an optional embodiment of this application;
[0028] Figure 3 A flowchart illustrating a method for manufacturing a stepped substrate with a cavity, according to another optional embodiment of this application;
[0029] Figure 4 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0030] Figure 5 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0031] Figure 6This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0032] Figure 7 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0033] Figure 8 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0034] Figure 9 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0035] Figure 10 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0036] Figure 11 This is a schematic flowchart of one step in the fabrication of a stepped substrate with a cavity according to this application.
[0037] The reference numerals in the attached figures are as follows:
[0038] 1. Substrate; 2. Bonding layer; 3. Window panel; 4. Pad; 5. Solder resist layer. Detailed Implementation
[0039] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting the present invention.
[0040] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.
[0041] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0042] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0043] See also Figures 2 to 11 As shown, according to an embodiment of this application, a method for manufacturing a stepped substrate with a cavity is provided. By dissolving the uncured bonding material at the bottom of the groove after the window plate 3 is bonded and before the bonding layer 2 is cured, the overflow adhesive at the bottom of the groove can be removed, thus avoiding the inability of chip mounting and wire bonding caused by the overflow adhesive at the bottom of the groove.
[0044] Method for manufacturing stepped substrates with cavities:
[0045] First, see Figure 4 As shown, step S1: bonding layer 2 is pressed onto substrate 1.
[0046] The substrate 1 can be a single-layer circuit board or a multi-layer circuit board, whichever is appropriate for the specific situation. This embodiment does not impose further limitations. It is understood that single-layer circuit boards are suitable for use in simpler electronic devices, such as some small electronic toys; multi-layer circuit boards are suitable for use in devices that require the integration of numerous functional modules and high-performance chips to achieve complex circuit layouts and signal transmissions, such as smartphones.
[0047] The bonding layer 2 can be a photosensitive resin sheet. The bonding layer 2 is pressed onto the substrate 1 and acts as an adhesive to establish a connection between the substrate 1 and other components, forming a stable multilayer structure, so that the substrate 1 and other components can maintain a stable connection when subjected to external forces such as vibration and impact.
[0048] Then, see Figure 5 As shown, step S2: Press the window plate 3 onto the side of the bonding layer 2 away from the substrate 1.
[0049] The window panel 3 has a through groove that runs through it. The cross-section of the through groove can be cylindrical or rectangular, etc., and this embodiment does not impose further limitations.
[0050] Specifically, the cavity formed by the through slot is used to mount the chip. By creating the through slot, a chip packaging space is formed.
[0051] In one embodiment, the window plate 3 is a double-sided copper-clad board, which protects the chip; in another embodiment, the window plate 3 is a circuit board, which supports the chip and also connects the circuit.
[0052] Specifically, the window plate 3 is located on the side of the bonding layer 2 away from the substrate 1. The window plate 3 is pressed onto the bonding layer 2. One side of the bonding layer 2 is used to bond the substrate 1, and the other side is used to bond the window plate 3.
[0053] Secondly, see Figure 6 As shown, step S3: dissolve the bonding material on the bonding layer 2 at the position relative to the window of the window plate 3.
[0054] Among them, the bonding material at the position of the bonding layer 2 relative to the window of the window plate 3 is the bonding material at the bottom of the through groove.
[0055] The dissolving bonding material at the bottom of the through-slot can, on the one hand, expose the electrodes at the bottom of the through-slot, making it easier for the chip to bond with the electrode leads; on the other hand, it can create better installation conditions for chip mounting, which is beneficial for chip placement.
[0056] Specifically, the windowed plate of the stepped substrate with cavity is placed face down, and in the developing equipment, the bonding material at the bottom of the developing tank is dissolved by spraying developing solution or organic solvent from bottom to top onto the bottom of the developing tank.
[0057] Finally, step S4: cure the bonding layer 2.
[0058] The bonding layer 2 can be cured by baking, so that the bonding layer 2 is tightly bonded to the substrate 1 and the window plate 3 respectively, forming a stepped substrate with a cavity.
[0059] In the above embodiments, the bonding material is a dry model photosensitive resin or a thermosetting resin.
[0060] When the bonding material is a dry model photosensitive resin, the bonding layer 2 can be a photosensitive resin sheet; when the bonding material is a thermosetting resin, the bonding layer 2 can be a thermosetting resin sheet.
[0061] Specifically, when the bonding material is a dry model photosensitive resin, the bonding material at the bottom of the through-slot can be removed by spraying with a water-soluble alkaline solution such as sodium carbonate solution; when the bonding material is a thermosetting resin, the bonding material at the bottom of the through-slot can be removed by spraying with organic solvents such as acetone, ethanol, toluene, or xylene.
[0062] When the bonding material is a thermosetting resin, the thermosetting resin is a pure adhesive resin film that does not contain fiberglass cloth.
[0063] In the above embodiments, the bonding temperature of the bonding layer 2 and the window plate 3 is lower than the conventional bonding temperature of the bonding layer 2 and the window plate 3, which is 60℃~80℃; the bonding pressure of the bonding layer 2 and the window plate 3 is higher than the conventional bonding pressure of the bonding layer 2 and the window plate 3, which is 0.2MPa~0.6MPa. By setting the bonding temperature of the bonding layer 2 and the window plate 3 to be lower than the conventional bonding temperature, the viscosity of the bonding material can be increased, thereby reducing the fluidity of the bonding material and reducing the amount of adhesive overflow at the bottom of the through-slot; at the same time, by setting the bonding pressure of the bonding layer 2 and the window plate 3 to be higher than the conventional bonding pressure, it can be ensured that the bonding layer 2 has good circuit filling performance.
[0064] The bonding temperature of the bonding layer 2 and the window plate 3 can be 10℃ to 20℃ lower than the conventional bonding temperature of the bonding layer 2 and the window plate 3.
[0065] Specifically, when the conventional bonding temperature of bonding layer 2 and window plate 3 is 80℃, the set value of the bonding temperature of bonding layer 2 and window plate 3 can be 60℃~70℃; when the conventional bonding temperature of bonding layer 2 and window plate 3 is 70℃, the set value of the bonding temperature of bonding layer 2 and window plate 3 can be 50℃~60℃. It should be noted that when the conventional bonding temperature of bonding layer 2 and window plate 3 is 60℃, the set value of the bonding temperature of bonding layer 2 and window plate 3 can only be 50℃. If the set value of the bonding temperature of bonding layer 2 and window plate 3 is less than 50℃, the substrate 1 and window plate 3 cannot be bonded.
[0066] The bonding pressure of the bonding layer 2 and the window plate 3 can be 5% to 15% higher than the conventional bonding pressure of the bonding layer 2 and the window plate 3.
[0067] Specifically, when the conventional pressing pressure of the bonding layer 2 and the window plate 3 is 0.6 MPa, the setting value of the pressing pressure of the bonding layer 2 and the window plate 3 can be 0.63 MPa to 0.69 MPa; when the conventional pressing pressure of the bonding layer 2 and the window plate 3 is 0.4 MPa, the setting value of the pressing pressure of the bonding layer 2 and the window plate 3 can be 0.42 MPa to 0.46 MPa; when the conventional pressing pressure of the bonding layer 2 and the window plate 3 is 0.2 MPa, the setting value of the pressing pressure of the bonding layer 2 and the window plate 3 can be 0.21 MPa to 0.23 MPa.
[0068] In the above embodiments, the bonding layer 2 and the window plate 3 are bonded together using a vacuum laminator. By using a vacuum laminator to bond the bonding layer 2 and the window plate 3, air bubbles can be avoided in the bonding area, ensuring that the bonding layer 2 can be tightly bonded to the substrate 1 and the window plate 3.
[0069] In this embodiment, the substrate 1, bonding layer 2, and window plate 3 can be placed in a hollow laminator for lamination.
[0070] In the above embodiments, when dissolving the bonding material on the bonding layer 2 at the position relative to the window of the window plate 3, the window of the window plate 3 is set to face downwards, so that the water-soluble alkaline solution or organic solvent is sprayed upwards, which can reduce the residence time of the water-soluble alkaline solution or organic solvent at the bottom of the through tank and prevent the bonding material outside the bottom area of the through tank from being dissolved.
[0071] The downward direction can be the vertically downward direction.
[0072] In the above embodiments, the curing temperature of the bonding layer 2 is 150℃~250℃, and the curing time of the bonding layer 2 is 30min~120min.
[0073] For example, the curing temperature of bonding layer 2 is 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃, or 250℃. It is understood that the curing temperature of bonding layer 2 can also be any value other than those mentioned above, as long as the curing temperature of bonding layer 2 is between 150℃ and 250℃.
[0074] Specifically, in this embodiment, the curing temperature of the bonding layer 2, i.e. the baking temperature of the bonding layer 2, is preferably 200°C.
[0075] For example, the curing time of the bonding layer 2 can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, or 120 min. It is understood that the curing time of the bonding layer 2 can also be any value other than those mentioned above, as long as the curing time of the bonding layer 2 is between 30 min and 120 min.
[0076] Specifically, in this embodiment, the curing time of the bonding layer 2, i.e. the baking time of the bonding layer 2, is preferably 60 minutes.
[0077] In some possible implementations provided in this application, see [link to relevant documentation]. Figure 7 As shown, the method for manufacturing a stepped substrate with a cavity further includes:
[0078] Step S5: Drill through holes in the stepped substrate with cavities along the vertical direction.
[0079] This process involves mechanically drilling through-holes in a stepped substrate with cavities, then metallizing the vias to create conductive channels between different layers, allowing current and signals to be transmitted between them. Multiple vias can be drilled, providing more path options for circuit layout and optimizing circuit design.
[0080] In some possible implementations provided in this application, see [link to relevant documentation]. Figure 8 As shown, the method for manufacturing a stepped substrate with a cavity further includes:
[0081] Step S6: Metallize the via to form pad 4.
[0082] Through-hole metallization can include: desmearing, removing resinous drilling debris and slag generated on the hole walls during drilling, which can be done using chemical methods such as strong oxidants or plasma treatment; hole wall activation, making the hole wall surface active so that it can subsequently adsorb metal; chemical copper plating, depositing a thin copper layer on the hole walls using chemical plating methods. This usually involves a series of chemical reactions to reduce copper ions to metallic copper and attach it to the hole walls; and electroplating to thicken the copper layer, further increasing the thickness of the copper layer based on chemical copper plating to meet conductivity and reliability requirements.
[0083] Specifically, after through-hole metallization, the lines between different layers of the circuit board can be interconnected through the through-holes, ensuring smooth transmission of current and signals, providing a good conductive path, reducing contact resistance and signal loss, and improving the stability and reliability of the circuit. At the same time, the metal filling the through-holes can increase the overall strength of the substrate, enabling it to withstand the stress during subsequent processing and use.
[0084] The through-hole metallization also includes forming pad 4, which can serve as a pin for circuit connection.
[0085] Specifically, the shape and size of the metal layer can be precisely controlled through processes such as photolithography or etching to form pads of specific shapes and sizes.
[0086] In some possible implementations provided in this application, see [link to relevant documentation]. Figure 9 As shown, the method for manufacturing a stepped substrate with a cavity further includes:
[0087] Step S7: Fabricate solder resist layers on the top and bottom surfaces of the stepped substrate with cavity, and create solder resist openings in the pad 4 area.
[0088] Understandably, by creating a solder mask layer 5 on the top and bottom surfaces of a stepped substrate with cavities, outside the projection area of the pad 4, solder can be prevented from spreading in areas where soldering is not required, thus avoiding short circuits between adjacent lines due to solder connections. For example, in high-density wiring circuit boards, the solder mask layer 5 can precisely limit the flow range of solder, ensuring the independence of each line.
[0089] The solder resist layer 5 can be made of liquid solder resist ink and dry film solder resist material.
[0090] In some possible implementations provided in this application, see [link to relevant documentation]. Figure 10 As shown, the method for manufacturing a stepped substrate with a cavity further includes:
[0091] Step S8: Coating the surface of pad 4.
[0092] Tin plating or nickel-gold plating can be applied to the surface of pad 4.
[0093] Specifically, by coating the surface of pad 4, the solder can better adhere to the surface of pad 4, forming good solder joints and ensuring soldering quality; at the same time, a protective film can be formed on the surface of pad 4 to prevent it from being oxidized during storage and use, thereby ensuring conductivity during soldering.
[0094] In some possible implementations provided in this application, see [link to relevant documentation]. Figure 11 As shown, the method for manufacturing a stepped substrate with a cavity further includes:
[0095] Step S9: Ball placement on pad 4.
[0096] Among them, the template ball planting method, vacuum ball planting method or spray ball method can be used to plant balls on the surface of pad 4.
[0097] Specifically, by placing balls on the surface of pad 4, more connection points can be achieved in a limited space, making it suitable for highly integrated electronic devices; at the same time, compared with traditional pin connections, ball-shaped connection points can provide better electrical performance and reduce signal transmission delay and loss.
[0098] The method for manufacturing a stepped substrate with a cavity provided in the embodiments of this application uses a photosensitive resin sheet or a thermosetting resin sheet as the bonding material between the substrate 1 and the window plate 3. After the window plate 3 is bonded, before the photosensitive resin sheet or thermosetting resin sheet is cured, the window of the window plate 3 is turned downwards, and a developer or solvent is sprayed upwards to dissolve and remove the uncured photosensitive resin sheet or thermosetting resin sheet at the bottom of the tank. Since the photosensitive resin sheet or thermosetting resin sheet covered by the window plate 3 cannot come into contact with the developer or solvent, the photosensitive resin sheet or thermosetting resin sheet under the window plate 3 is retained. After the photosensitive resin sheet or thermosetting resin sheet at the bottom of the through-hole is completely removed, the stepped substrate with the photosensitive resin sheet or thermosetting resin sheet at the bottom of the through-hole is heated to form a permanent bond between the substrate 1 and the window plate 3.
[0099] It will be readily understood by those skilled in the art that the aforementioned advantageous methods can be freely combined and superimposed without conflict.
[0100] The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application. The above are merely preferred embodiments of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of this application, and these improvements and modifications should also be considered within the protection scope of this application.
Claims
1. A method for manufacturing a stepped substrate with a cavity, characterized in that, include: A bonding layer (2) is pressed onto the substrate (1); A windowed plate (3) with a pre-opened window is pressed onto the side of the bonding layer (2) away from the substrate (1). The window of the window panel (3) is set to face downwards, and the uncured bonding material on the bonding layer (2) at the position relative to the window of the window panel (3) is dissolved by spraying. After the uncured bonded material has dissolved, the bonded layer (2) is cured.
2. The method for manufacturing a stepped substrate with a cavity according to claim 1, characterized in that, The bonding material is a dry model photosensitive resin or a thermosetting resin.
3. The method for manufacturing a stepped substrate with a cavity according to claim 1, characterized in that, The bonding temperature of the bonding layer (2) and the window plate (3) is lower than the conventional bonding temperature of the bonding layer (2) and the window plate (3). The conventional bonding temperature of the bonding layer (2) and the window plate (3) is 60℃~80℃. The bonding pressure of the bonding layer (2) and the window plate (3) is greater than the conventional bonding pressure of the bonding layer (2) and the window plate (3). The conventional bonding pressure of the bonding layer (2) and the window plate (3) is 0.2MPa~0.6MPa.
4. The method for manufacturing a stepped substrate with a cavity according to claim 1, characterized in that, The bonding layer (2) and the window plate (3) are bonded together using a vacuum laminator.
5. The method for manufacturing a stepped substrate with a cavity according to claim 1, characterized in that, The curing temperature of the bonding layer (2) is 150℃~250℃, and the curing time of the bonding layer (2) is 30min~120min.
6. The method for manufacturing a stepped substrate with a cavity according to claim 1, characterized in that, The method further includes: Drill through holes in the stepped substrate with cavities along the vertical direction; Through-hole metallization to form pads (4).
7. The method for manufacturing a stepped substrate with a cavity according to claim 6, characterized in that, The method further includes: A solder resist layer (5) is fabricated in the area outside the projection of the pad (4) on the top and bottom surfaces of the stepped substrate with cavity.
8. The method for manufacturing a stepped substrate with a cavity according to claim 6, characterized in that, The method further includes: Coating of the surface of the pad (4).
9. The method for manufacturing a stepped substrate with a cavity according to claim 6, characterized in that, The method further includes: Balls are placed on the surface of the pad (4).
Citation Information
Patent Citations
Adhesive film and its use and method for producing semiconductor device
JP2002265888A
Multilayer wiring board
JP2009065009A
Method of manufacturing circuit board and chip package and circuit board prepared by the same