Surface-modified negative electrode active material particles, negative electrode composite material, lithium ion battery, and method for producing negative electrode composite material
By modifying fluoroalkyl groups on the negative active material particles of lithium-ion batteries and combining them with fluorine-containing adhesives, the problem of large battery resistance is solved, and the battery performance is improved, especially in automotive battery applications. efficiency and endurance.
Patent Information
- Application Number
- CN202410092464.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-01-23
- Publication Date
- 2024-11-22
AI Technical Summary
The negative active substance particles of existing lithium-ion batteries have large resistance, which affects the performance of the battery. Especially in automotive battery applications, the resistance needs to be reduced to improve efficiency and endurance.
By modifying the surface of silicon particles to increase fluoroalkyl groups, forming silicon-oxygen-silicon-carbon bonds, and combining them with fluorine-containing adhesives, surface modified negative electrode active material particles with small resistance are prepared for manufacturing negative electrode composite materials. and lithium-ion batteries.
It effectively reduces the internal resistance of the battery, improves the charging uniformity of the battery and the overall performance of the battery, enhances the bonding strength between the negative electrode active material layer and the current collector layer, and reduces the risk of cracking of the battery.
Smart Images

Figure CN119008871A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to surface modified negative electrode active material particles, negative electrode composite materials, lithium ion batteries and a method for producing the negative electrode composite materials. Background Art
[0002] In recent years, the development of batteries has been in full swing. For example, in the automotive industry, the development of batteries for pure electric vehicles (battery electric vehicles) or hybrid electric vehicles (hybrid electric vehicles) is underway. In addition, silicon is known as a negative electrode active material for batteries.
[0003] Japanese Patent Application Laid-Open No. 2018-120866 discloses a negative electrode active material, characterized in that it contains a carbon-based negative electrode active material and a porous SiO x Particles (0≤x<2), the porous SiO x The particles contain an oxide film layer coated on the surface. x The particles are porous silicon particles, the thickness of the oxide film layer is 40 nm or more and 200 nm or less, and the porous SiO x The specific surface area of the particles is 5m 2 / g to 50m 2 / g. Summary of the invention
[0004] For lithium-ion batteries, it is desirable to reduce the resistance.
[0005] The object of the present invention is to provide surface-modified negative electrode active material particles with low resistance, a negative electrode composite material containing such surface-modified negative electrode active material particles, a lithium ion battery containing such surface-modified negative electrode active material particles, and a method for producing such surface-modified negative electrode active material particles.
[0006] The inventors of the present application have found that the above-mentioned problems can be solved by the following means.
[0007] Method 1
[0008] A surface-modified negative electrode active material particle comprises a silicon particle and a fluoroalkyl group modifying the surface of the silicon particle.
[0009] Method 2
[0010] The surface-modified negative electrode active material particle according to Embodiment 1 has a silicon-oxygen-silicon-carbon bond, wherein the silicon not bonded to the carbon is silicon of the silicon particle, and the carbon is carbon of a fluoroalkyl group.
[0011] Method 3
[0012] The surface-modified negative electrode active material particle according to aspect 1, wherein the fluoroalkyl group has 3 or more and 12 or less carbon atoms.
[0013] Method 4
[0014] A negative electrode composite material comprising the surface-modified negative electrode active material particles according to any one of Embodiments 1 to 3 and a fluorine-containing binder.
[0015] Method 5
[0016] The negative electrode composite material according to embodiment 4, wherein the fluorine-containing binder is a polyvinylidene fluoride-based binder.
[0017] Method 6
[0018] A lithium ion battery having a negative electrode active material layer, wherein the negative electrode active material layer contains the negative electrode composite material according to embodiment 4 or 5.
[0019] Method 7
[0020] A method for producing surface-modified negative electrode active material particles comprises modifying the surface of silicon particles with a fluoroalkyl group.
[0021] Method 8
[0022] The method according to Embodiment 7, wherein the surface of the silicon particle is modified with the fluoroalkyl group by dehydration condensation of the silanol groups on the surface of the silicon particle with the silanol groups generated by hydrolyzing the hydrolyzable group-containing silane having a fluoroalkyl group.
[0023] According to the present invention, it is possible to provide surface-modified negative electrode active material particles with low resistance, a negative electrode composite material containing such surface-modified negative electrode active material particles, a lithium ion battery containing such surface-modified negative electrode active material particles, and a method for producing such surface-modified negative electrode active material particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Features, advantages, and technical and industrial significance of exemplary embodiments of the present invention are described below with reference to the accompanying drawings, wherein like symbols represent like elements.
[0025] Figure 1 It is the result of XPS measurement of Comparative Synthesis Examples 1 to 3 and Synthesis Examples 1 and 2 (Si(2p)).
[0026] Figure 2 It is the result of XPS measurement of Comparative Synthesis Examples 1 to 3 and Synthesis Examples 1 and 2 (F(1s)). DETAILED DESCRIPTION
[0027] Hereinafter, embodiments of the present invention will be described in detail. It should be noted that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the disclosed gist.
[0028] Surface modification of negative electrode active material particles
[0029] The surface-modified negative electrode active material particles of the present invention comprise silicon particles and a fluoroalkyl group modifying the surface of the silicon particles.
[0030] The inventor of the present application has found that the resistance of a lithium ion battery containing silicon particles whose surface is modified by fluoroalkyl as a negative electrode active material is small. As the reason, it is not intended to be bound by any theory, and it is speculated as follows. That is, it is believed that by modifying the surface of the silicon particles, the affinity of the silicon particles in the negative electrode composite material and the fluorine-containing binder is improved. And it is believed that the battery made using the negative electrode composite material is easy to charge evenly, so the resistance becomes small.
[0031] Silicon particles
[0032] The surface-modified negative electrode active material particles of the present invention include silicon particles.
[0033] The composition of the silicon particles is not particularly limited. The ratio of silicon element to all elements contained in the silicon particles may be, for example, 50 mol % or more, 70 mol % or more, or 90 mol % or more.
[0034] The silicon particles may contain other elements besides Si element, such as Li element. Other elements include Sn element, Fe element, Co element, Ni element, Ti element, Cr element, B element, P element, etc. besides Li element.
[0035] The silicon particles may contain impurities such as oxides.
[0036] The silicon particles may be amorphous or crystalline. The crystal phase contained in the silicon particles is not particularly limited.
[0037] The shape and size of the silicon particles are not particularly limited. The average particle size of the silicon particles can be, for example, more than 30 nm, more than 50 nm, more than 100 nm or more than 150 nm, and can be less than 10 μm, less than 5 μm, less than 3 μm, less than 2 μm or less than 1 μm. It should be noted that the average particle size can be obtained by observation using an electron microscope such as SEM, for example, it can be obtained as the average value of the maximum Feret diameter of each of two or more particles. The number of samples is preferably large, for example, more than 20, more than 50, or more than 100. The average particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the silicon particles described later or performing a classification process.
[0038] The silicon particles contained in the surface-modified negative electrode active material particles may be porous silicon particles. The porous silicon particles contain silicon having two or more voids. The form of the voids in the porous silicon particles is not particularly limited.
[0039] The porous silicon particles may be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having two or more pores having a pore diameter of nanometer order (less than 1000 nm, preferably 100 nm or less).
[0040] Fluorinated alkyl
[0041] The surface-modified negative electrode active material particles of the present invention have a fluoroalkyl group modifying the surface of the silicon particles.
[0042] The number of carbon atoms in the fluoroalkyl group may be 3 or more and 15 or less. In addition, the number of carbon atoms may be 4 or more, 5 or more, 6 or more, 7 or more, or 8 or less, 14 or less, 13 or less, 12 or less, 11 or less, or 10 or less. The fluoroalkyl group may have a linear, branched, or cyclic structure, and is preferably a linear fluoroalkyl group. In addition, the fluoroalkyl group may be a perfluoroalkyl group, or an alkyl group in which a portion of hydrogen is replaced by fluorine (e.g., -(CH2)2(CF2) n CF3 (n is an integer from 0 to 12), preferably -(CH2)2(CF2) n A fluorinated alkyl group represented by CF3 (n is an integer of 0 to 12).
[0043] The surface modified negative electrode active material particles of the present invention may have a silicon-oxygen-silicon-carbon bond, the silicon not bonded to the carbon is the silicon of the silicon particle, and the carbon is the carbon of a fluoroalkyl group. That is, the carbon of the fluoroalkyl group may be bonded to the silicon on the surface of the silicon particle via oxygen and silicon.
[0044] Method for producing surface-modified negative electrode active material particles
[0045] The method of the present invention for producing surface-modified negative electrode active material particles includes the step of modifying the surface of silicon particles with a fluoroalkyl group.
[0046] The surface of the silicon particle can be modified with a fluoroalkyl group by dehydration condensation between the silanol groups on the surface of the silicon particle and the silanol groups generated by hydrolyzing the hydrolyzable group-containing silane having a fluoroalkyl group.
[0047] As the hydrolyzable group-containing silane, a hydrolyzable group-containing silane having a corresponding structure can be used with reference to the above description related to the fluoroalkyl group of the present invention.
[0048] Anode composite materials
[0049] The negative electrode composite material of the present invention comprises surface-modified negative electrode active material particles and a fluorine-containing binder. The surface-modified negative electrode active material particles contained in the negative electrode composite material of the present invention comprise silicon particles and a fluoroalkyl group modifying the surface of the silicon particles.
[0050] Without intending to be bound by any theory, it is believed that by making both the surface modification group and the binder fluorine-based, the silicon particles and the binder are firmly bonded via the surface modification group, the peel strength between the negative electrode active material layer and the negative electrode collector layer is improved, and thus cracking of the negative electrode active material layer is suppressed, resulting in reduced resistance.
[0051] It should be noted that, with respect to the present invention, "negative electrode composite material" refers to a composition that can directly constitute a negative active material layer or can constitute a negative active material layer by further containing other components. In addition, with respect to the present invention, "negative electrode composite material slurry" refers to a slurry that contains a dispersion medium on the basis of a "negative electrode composite material" and is coated and dried using the dispersion medium to form a negative electrode active material layer.
[0052] Surface modification of negative electrode active material particles
[0053] The negative electrode composite material of the present invention contains surface-modified negative electrode active material particles. Regarding the surface-modified negative electrode active material particles, the above description related to the surface-modified negative electrode active material particles of the present invention can be referred to.
[0054] Fluorinated adhesive
[0055] The negative electrode composite material of the present invention contains a fluorine-containing binder. Examples of the fluorine-containing binder include polyvinylidene fluoride (PVdF)-based binders and polytetrafluoroethylene (PTFE)-based binders. The fluorine-containing binder is preferably a PVdF-based binder. The PVdF-based binder may be a copolymer having units derived from a monomer other than VdF.
[0056] In addition, the negative electrode composite material of the present invention optionally contains an electrolyte, a conductive aid, and a binder other than the fluorine-containing binder.
[0057] Electrolytes
[0058] The material of the solid electrolyte is not particularly limited, and a material that can be used as a solid electrolyte used in a lithium ion battery can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.
[0059] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5 (Li7P3S 11, Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 (Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x PS 6-x Cl x etc., or combinations thereof, but are not limited thereto.
[0060] The sulfide solid electrolyte may be glass or crystallized glass (glass ceramic).
[0061] It should be noted that when the negative electrode composite material contains a solid electrolyte, the mass ratio of the surface modified negative electrode active material particles to the solid electrolyte in the negative electrode composite material (mass of the surface modified negative electrode active material particles: mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0062] The electrolyte preferably contains a supporting salt and a solvent.
[0063] As supporting salts (lithium salts) of electrolytes having lithium ion conductivity, for example, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3 can be listed.
[0064] Examples of the solvent used in the electrolyte include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolyte preferably contains two or more solvents.
[0065] Conductive additives
[0066] The conductive additive is not particularly limited, and may be, for example, vapor grown carbon fiber (VGCF), acetylene black (AB), Ketjen black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.
[0067] Adhesives other than fluorinated adhesives
[0068] There is no particular limitation on the adhesive other than the fluorine-containing adhesive. For example, the adhesive may be a material such as butadiene rubber (BR) or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto. The mass of the adhesive other than the fluorine-containing adhesive relative to the total mass of the adhesive may be less than 50 mass %, less than 40 mass %, less than 30 mass %, less than 20 mass % or less than 10 mass %, or may be 0 mass %.
[0069] Lithium-ion battery
[0070] The lithium ion battery of the present invention has a negative electrode active material layer, and the negative electrode active material layer contains the negative electrode composite material of the present invention. The lithium ion battery of the present invention may sequentially have a negative electrode collector layer, a negative electrode active material layer containing the negative electrode composite material of the present invention, a solid electrolyte layer, a positive electrode active material layer and a positive electrode collector layer.
[0071] The lithium-ion battery of the present invention may be a liquid battery containing an electrolyte as an electrolyte layer, or may be a solid-state battery having a solid electrolyte layer as an electrolyte layer. It should be noted that, with respect to the present invention, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore, a solid-state battery may also use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. In addition, the solid-state battery of the present invention may also be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.
[0072] Lithium-ion batteries can be either primary or secondary batteries.
[0073] Examples of the shape of the lithium ion battery include a coin shape, a laminate shape, a cylindrical shape, and a square shape.
[0074] Negative electrode collector layer
[0075] The material used for the negative electrode collector layer is not particularly limited, and any material that can be used as a negative electrode collector for a battery may be appropriately used, such as copper, copper alloys, and copper plated or vapor-deposited with nickel, chromium, carbon, etc., but is not limited thereto.
[0076] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among them, a foil shape is preferred.
[0077] Negative electrode active material layer
[0078] The negative electrode active material layer of the present invention contains the negative electrode composite material of the present invention. Regarding the negative electrode composite material, the above description related to the negative electrode composite material of the present invention can be referred to.
[0079] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0080] Electrolyte layer
[0081] The electrolyte layer contains at least an electrolyte. In addition, the electrolyte layer may contain a binder as needed in addition to the electrolyte. Regarding the electrolyte, reference may be made to the above-mentioned description related to the negative electrode composite material of the present invention. As a binder, for example, it may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR) or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.
[0082] The thickness of the electrolyte layer is, for example, 0.1 μm to 300 μm, and preferably 0.1 μm to 100 μm.
[0083] Positive electrode active material layer
[0084] The positive electrode active material layer is a layer containing a positive electrode active material and, optionally, an electrolyte, a conductive aid, a binder, and the like.
[0085] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material can be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、Li 1+x Mn 2-x-y MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni and Zn) is a kind of Li-Mn spinel, lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co and Ni), etc., but is not limited to these.
[0086] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material having lithium ion conductivity, low reactivity with the positive electrode active material and the solid electrolyte, and maintaining the form of a coating layer that does not flow even when in contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but not limited to these.
[0087] As the shape of the positive electrode active material, for example, a particle shape can be cited. The average particle size (D50) of the positive electrode active material is not particularly limited, and is, for example, greater than 10 nm, and can be greater than 100 nm. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, less than 50 μm, and can be less than 20 μm. The average particle size (D50) can be calculated, for example, by measurement using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0088] Regarding the electrolyte and the conductive aid, reference may be made to the above description related to the negative electrode composite material of the present invention. Regarding the binder, reference may be made to the above description related to the electrolyte layer of the present invention.
[0089] It should be noted that when the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.
[0090] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0091] Positive electrode collector layer
[0092] The material used for the positive electrode collector layer is not particularly limited. Materials that can be used as positive electrode collectors for batteries can be appropriately used, such as SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium and zinc, as well as materials plated or vapor-deposited with nickel, chromium, carbon, etc. on these metals, but are not limited to these.
[0093] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among them, a foil shape is preferred.
[0094] Preparation of surface modified negative electrode active material particles
[0095] Preparation of silicon particles
[0096] Comparative Synthesis Example 1
[0097] As a silicon (Si) source, silicon particles were prepared. The silicon particles and metal lithium (Li) were weighed at a molar ratio of Li / Si=4.0, and the weighed silicon particles and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere to obtain porous silicon particles.
[0098] Modification using fluoroalkyl groups
[0099] Synthesis example 1
[0100] In an argon (Ar) replacement glove box, 2g of porous silicon particles, 20g of super dehydrated ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.15g of trimethoxy (1H, 1H, 2H, 2H-tridecafluorooctyl) silane (manufactured by Tokyo Chemical Industry) as a silane coupling agent with a fluoroalkyl group (-C2H4(CF2)5CF3) were weighed, placed in a closed reaction vessel, and stirred at 50°C for 16 hours to dehydrate and condense the silanol groups on the surface of the silicon particles with the silanol groups generated by the hydrolysis of the silane coupling agent with a fluoroalkyl group. The solution after the reaction was filtered, washed and filtered with 30mL of ethanol, and the above operation was repeated 5 times. The obtained solid was vacuum dried at 100°C for 12 hours to obtain surface-modified negative electrode active material particles whose surfaces were modified with -C2H4(CF2)5CF3 on the surface of the silicon particles.
[0101] Synthesis example 2
[0102] The silane coupling agent was changed to 0.18 g of trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane (manufactured by Tokyo Chemical Industry) having a fluoroalkyl group (-C2H4(CF2)7CF3). The same operation as in Synthesis Example 1 was performed except that the surface of the silicon particles was modified with -C2H4(CF2)7CF3 to produce surface-modified negative electrode active material particles.
[0103] Comparative Synthesis Example 2
[0104] The silane coupling agent was changed to 0.06 g of hexyltrimethoxysilane (manufactured by Tokyo Chemical Industry) having an alkyl group (-(CH2)5CH3) but not having a fluoroalkyl group. The same operation as in Synthesis Example 1 was performed to produce surface-modified negative electrode active material particles in which the surface of the silicon particles was modified with -(CH2)5CH3.
[0105] Comparative Synthesis Example 3
[0106] The silane coupling agent was changed to 0.08 g of trimethoxy-n-octylsilane (manufactured by Tokyo Chemical Industry) having an alkyl group (-(CH2)7CH3) but not having a fluoroalkyl group. The same operation as in Synthesis Example 1 was performed to produce surface-modified negative electrode active material particles in which the surface of the silicon particles was modified with -(CH2)7CH3.
[0107] Battery production
[0108] Preparation of cathode composite materials
[0109] In a polypropylene (PP) container, butyl butyrate, a 5 wt% butyl butyrate solution of a polyvinylidene fluoride (PVDF)-based binder, LiNi as a positive electrode active material, and a 1 / 3 Co 1 / 3 Mn 1 / 3O2 (average particle size: 6 μm), Li2S-P2S5 glass ceramics as sulfide solid electrolyte, and vapor-grown carbon fiber (VGCF) as a conductive additive were added to the container and stirred for 30 seconds using an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the container was vibrated for 3 minutes using a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.) and stirred for 30 seconds using an ultrasonic dispersion device. Further, the vibrator was vibrated for 3 minutes to obtain a slurry-like positive electrode composite material (positive electrode composite material slurry).
[0110] Formation of positive electrode active material layer
[0111] The obtained slurry was applied to an aluminum (Al) foil (manufactured by Showa Denko) as a positive electrode current collector layer using a doctor blade method using an applicator. The applied slurry was dried on a hot plate at 100° C. for 30 minutes. Thus, a positive electrode active material layer was formed on the positive electrode current collector layer.
[0112] Preparation of negative electrode composite materials
[0113] Comparative Examples 1 to 3 and Examples 1 and 2
[0114] In a polypropylene (PP) container, diisobutyl ketone, a 5 wt% diisobutyl ketone solution of a PVDF-based binder (KF8300 manufactured by KUREHA), VGCF as a conductive aid, Li2S-P2S5 glass ceramics as a solid electrolyte, and any one of the silicon particles of Comparative Synthesis Examples 1 to 3 and Synthesis Examples 1 and 2 as negative electrode active materials are added to the container and stirred for 30 seconds using an ultrasonic dispersion device (UH-50 manufactured by SMT). Further, the container is vibrated for 30 minutes with a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.) to obtain a slurry-like negative electrode composite material (negative electrode composite material slurry) of Comparative Examples 1 to 3 and Examples 1 and 2.
[0115] Comparative Examples 4 and 5
[0116] Negative electrode composite material slurries of Comparative Examples 4 and 5 were prepared in the same manner as in Examples 1 and 2 except that the binder was changed to a 5 wt % diisobutyl ketone solution of a styrene-butadiene rubber (SBR)-based binder.
[0117] Formation of negative electrode active material layer
[0118] The obtained slurry was applied onto a nickel (Ni) foil as a negative electrode current collector using a doctor blade method using an applicator, and the applied slurry was dried on a hot plate at 100° C. for 30 minutes. Thus, a negative electrode active material layer was formed on the negative electrode current collector layer.
[0119] Formation of solid electrolyte layer
[0120] Heptane, a 5 wt% heptane solution of an SBR-based adhesive, and a Li2S-P2S5-based glass ceramic as a solid electrolyte were added to a polypropylene (PP) container and stirred for 30 seconds using an ultrasonic dispersion device (UH-50 manufactured by SMT). Further, the container was vibrated for 30 minutes with a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.) to obtain a solid electrolyte slurry. The obtained slurry was applied to an Al foil by a scraper method using an applicator. The applied slurry was dried on a hot plate at 100°C for 30 minutes. Thus, a solid electrolyte layer was formed. Three solid electrolyte layers were made.
[0121] Battery Assembly
[0122] The positive electrode current collector layer, the positive electrode active material layer and the first solid electrolyte layer were stacked in order, and the stack was placed in a roll press and pressed at a first pressing step of 100 kN / cm and 165° C. to obtain a positive electrode stack.
[0123] The negative electrode current collector layer, the negative electrode active material layer and the second solid electrolyte layer were stacked in this order, and the stack was placed in a roll press and pressed at a second pressing step of 60 kN / cm and 25° C. to obtain a negative electrode stack.
[0124] The negative electrode stack and the positive electrode stack were produced so that the area of the negative electrode stack was larger than that of the positive electrode stack.
[0125] Furthermore, the Al foil as a peeling sheet, the intermediate solid electrolyte layer formed on the Al foil, and the negative electrode stack are stacked in such a way that the solid electrolyte layers are in contact with each other. The stack is placed in a flat uniaxial press and temporarily pressed for 10 seconds under the conditions of a pressing pressure of 100 MPa and a pressing temperature of 25°C. The Al foil is peeled off from the intermediate solid electrolyte layer of the stack to obtain a negative electrode stack further stacked with an intermediate solid electrolyte layer.
[0126] The positive electrode stack and the negative electrode stack further stacked with the intermediate solid electrolyte layer are stacked in such a way that the solid electrolyte layers are in contact with each other. The stack is placed in a flat uniaxial press and pressurized for 1 minute under the conditions of a pressurizing pressure of 200 MPa and a pressurizing temperature of 120° C. in the third pressurizing step. Thus, an all-solid-state battery is obtained.
[0127] evaluate
[0128] Analysis of the surface properties of silicon particles
[0129] The carbon content of the silicon particles of the synthesis examples and comparative synthesis examples was measured by high-frequency combustion infrared absorption method (apparatus used: CSLS600 of LECO). In addition, the fluorine content of the silicon particles of each example was measured by combustion ion chromatography (apparatus used: ICS-1500 ion chromatograph manufactured by Thermo Fisher Scientific, AQF-100 automatic sample combustion apparatus manufactured by Nitto Seiko Analytic).
[0130] Furthermore, the surface of the silicon particles of each example was analyzed by X-ray photoelectron spectroscopy (XPS) (using the device: PHI5000VersaprobeII manufactured by ULVAC-PHI). The measurement was performed under the conditions of X-ray source: AlKα, 15kV, 3mA, energy step: 0.1eV, and number of scans: 4 times. For the peak area of XPS, the XPS analysis software (MultiPak manufactured by ULVAC-PHI) was used to draw a baseline for each peak and obtain the integrated intensity (area) of each peak. The area ratio of F(1s) / Si(2p) was calculated using the obtained area (F(1s): 684eV to 692eV, Si(2p): 95eV to 107eV).
[0131] Determination of DCIR
[0132] The manufactured battery was constrained with a constraining fixture at a specified constraining pressure, and after constant current-constant voltage charging (1 / 100C cut-off) at 1 / 10C until 4.55V, it was discharged at 1C to 3.0V. Then, constant current-constant voltage charging (1 / 100C cut-off) was performed at 1 / 3C until 4.35V, and constant current-constant voltage discharge (1 / 100C cut-off) was performed at 1 / 3C until 3.00V. Furthermore, after constant current-constant voltage charging (1 / 100C cut-off) was performed at 1 / 3C until 4.35V, constant current-constant voltage discharge (1 / 100C cut-off) was performed at 1 / 3C until 3.14V. Then, a current was applied at a constant current of 5C for 10s, and the DC internal resistance (DCIR) was measured.
[0133] result
[0134] Analysis of the surface properties of silicon particles
[0135] The results of quantitative analysis of the carbon content and fluorine content of the silicon particles of the comparative synthesis example and the synthesis example are shown in Table 1. In addition, the XPS analysis results of each silicon particle are shown in Tables 1 and 2. Figure 1 and 2 middle.
[0136] Table 1
[0137]
[0138] As shown in Table 1, the silicon particles of the synthesis example have a larger amount of carbon and fluorine on the particle surface and a value of F(1s) / Si(2p) than the silicon particles of the comparative synthesis example 1. It is therefore believed that the surface of the silicon particles of the embodiment has been modified with a fluoroalkyl group. It should be noted that the silicon particles of comparative synthesis examples 2 and 3 have a larger amount of carbon on the particle surface than the silicon particles of comparative synthesis example 1, and therefore it is believed that the surface of these silicon particles has been modified with an alkyl group.
[0139] Determination of DCIR
[0140] The results of DCIR measurement of the battery of each example are shown in Table 2. The DCIR value of each example is shown as a relative value when the measurement result of Comparative Example 1 is set to 1.00.
[0141] Table 2
[0142] Surface modification groups Adhesives DCIR(Relative value) Comparative Example 1 - PVdF-HFP 1.00 Comparative Example 2 <![CDATA[-(CH2)5CH3]]> PVdF-HFP 1.05 Comparative Example 3 <![CDATA[-(CH2)7CH3]]> PVdF-HFP 1.04 Example 1 <![CDATA[-C2H4(CF2)5CF3]]> PVdF-HFP 0.74 Example 2 <![CDATA[-C2H4(CF2)7CF3]]> PVdF-HFP 0.84 Comparative Example 4 <![CDATA[-C2H4(CF2)5CF3]]> SBR 0.99 Comparative Example 5 <![CDATA[-C2H4(CF2)7CF3]]> SBR 1.03
[0143] As shown in Table 2, the DCIR value of the battery of the embodiment in which both the surface modification group and the binder are fluorine-based is small. In contrast, the DCIR values of the batteries of Comparative Examples 2 to 5 in which either the surface modification group or the binder is other than fluorine-based are equivalent to that of Comparative Example 1 using unmodified silicon particles.
Claims
1. A surface-modified negative electrode active material particle comprising a silicon particle and a fluoroalkyl group modifying the surface of the silicon particle.
2. The surface-modified negative electrode active material particle according to claim 1, in, It has a bond of silicon-oxygen-silicon-carbon, the silicon not bonded to the carbon is the silicon of the silicon particle, and the carbon is the carbon of a fluoroalkyl group.
3. The surface-modified negative electrode active material particle according to claim 1, in, The fluoroalkyl group has 3 or more and 12 or less carbon atoms. 4 . A negative electrode composite material comprising the surface-modified negative electrode active material particles according to claim 1 and a fluorine-containing binder.
5. The negative electrode composite material according to claim 4, in, The fluorine-containing adhesive is a polyvinylidene fluoride adhesive. 6 . A lithium ion battery comprising a negative electrode active material layer, wherein the negative electrode active material layer contains the negative electrode composite material according to claim 4 or 5 .
7. A method for producing surface-modified negative electrode active material particles, comprising the step of modifying the surface of silicon particles with a fluoroalkyl group.
8. The method according to claim 7, in, The surface of the silicon particle is modified with the fluoroalkyl group by dehydration condensation between the silanol groups on the surface of the silicon particle and the silanol groups generated by hydrolyzing the hydrolyzable group-containing silane having the fluoroalkyl group.
Citation Information
Patent Citations
Porous silicon-based anode active material, method for preparing the same, and lithium secondary battery comprising the same