Lithium-rich manganese-based positive electrode material prepared by agar-assisted sol-gel method
The preparation of lithium-rich manganese-based positive electrode material through the agar-assisted sol gel method has solved the problems of inefficiency and instability of the material, achieved the goal of performance improvement and environmental protection, and promoted the commercial development of the material.
Patent Information
- Application Number
- CN202310565906.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
The lithium-rich manganese-based positive electrode material has problems such as low efficiency, poor cycle stability and poor rate performance in the first circle, which hinders its commercial development.
The lithium-rich manganese-based positive electrode material Li1.2Ni0.15Co0.15Mn0.5O2 was prepared by sol-gel method, which simplified the preparation process and improved the cycle stability and rate performance of the material.
The cycle stability and rate performance of lithium-rich manganese-based positive electrode material is significantly improved, and the specific capacity for the first discharge is also high, which is green and environmentally friendly.
Smart Images

Figure HSA0000296973430000011 
Figure HSA0000296973430000012 
Figure HSA0000296973430000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium-rich manganese-based positive electrode material prepared by an agar-assisted sol-gel method. Background Art
[0002] With the rapid development of science and technology and the progress of society, human beings have an increasing demand for energy and higher requirements for energy. In recent years, the contradiction between economic development and energy constraints has become particularly obvious. Traditional energy sources such as coal, oil, and natural gas are non-renewable energy sources with limited reserves, and over-exploitation and abuse will cause a series of environmental problems. Therefore, the development and utilization of renewable energy is an effective way to resolve the contradiction between economic development and energy constraints. Solar energy, wind energy, tidal energy, etc. are all green and environmentally friendly renewable energy sources. However, they are affected by factors such as weather and region, and cannot be used directly, requiring energy storage equipment to store them.
[0003] So far, there are many types of energy storage devices, and lithium-ion batteries stand out among many energy storage devices due to their own advantages. In the composition of lithium-ion batteries, the positive electrode material is a very important part. It not only participates in the electrochemical reaction in the battery, but also provides a lithium ion source for the lithium-ion battery. Among them, the layered lithium-rich manganese-based positive electrode material is considered to be the most promising lithium-ion battery positive electrode material due to its high capacity, low cost, and green environmental protection. Compared with traditional commercial positive electrode materials, the discharge specific capacity of lithium-rich manganese-based positive electrode materials is almost twice that of them. However, there are many problems with lithium-rich manganese-based materials themselves, such as low first-cycle coulomb efficiency, poor cycle stability, and poor rate performance, which hinder their commercial development. Researchers have solved the problems of lithium-rich manganese-based positive electrode materials themselves and improved the electrochemical properties of lithium-rich manganese-based positive electrode materials through surface coating, ion doping, morphology control and other modification methods.
[0004] Based on the sol-gel method, the present invention uses agar as an auxiliary agent to synthesize the lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.15 Co 0.15 Mn 0.5 O2. Its preparation method is simple and can effectively improve the cycle stability and rate performance of lithium-rich manganese-based positive electrode materials. Summary of the invention
[0005] Purpose of the invention: In view of the problems existing in lithium-rich manganese-based positive electrode materials, the present invention uses agar as an auxiliary agent and adopts an agar-assisted sol-gel method to prepare lithium-rich manganese-based positive electrode materials. The preparation method is simple, green and environmentally friendly, and the cycle and rate performance of lithium-rich manganese-based positive electrode materials are significantly improved.
[0006] Technical solution: The present invention adopts agar-assisted sol-gel method to prepare lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.15 Co 0.15 Mn 0.5 O2.
[0007] The present invention adopts the control experiment method, and the specific synthesis steps are as follows:
[0008] S1: Use a balance to weigh a certain amount of nickel acetate, cobalt acetate and manganese acetate, and completely dissolve them in 100 ml of deionized water, which is recorded as solution A.
[0009] S2: Weigh a certain amount of citric acid and lithium acetate, and completely dissolve them in 100 ml of deionized water, which is recorded as solution B.
[0010] S3: Add solution A to solution B drop by drop and stir continuously.
[0011] S4: The pH of the AB mixed solution was adjusted to neutral with aqueous ammonia, and then stirred continuously in a water bath at 100°C.
[0012] S5: After a while, add agar powder (the mass ratio of agar powder to transition metal salt is 0% and 10% respectively), and stir continuously until the agar powder is completely dissolved.
[0013] S6: Then, the mixture is continuously stirred in a water bath at 80°C until a gel state is formed.
[0014] S7: Put it in the oven and dry it thoroughly.
[0015] S8: After grinding, calcining in a tube furnace. After cooling, taking out, grinding and sieving, 0% and 10% agar-assisted synthesis of Li 1.2 Ni 0.15 Co 0.15 Mn 0.5 O2 material.
[0016] The above two materials were used as positive electrodes of lithium-ion batteries for electrochemical performance tests.
[0017] Beneficial effects: Compared with other modification methods of lithium-rich manganese-based positive electrode materials, the method of the present invention is simpler and more environmentally friendly. The present invention found through comparative experiments that the cycle stability and rate performance of the lithium-rich manganese-based positive electrode material prepared with the assistance of agar are significantly improved, and the first discharge specific capacity is also very high. This has practical significance for the development of lithium-rich manganese-based positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The XRD patterns of the synthetic materials of the present invention and the comparative examples are shown in FIG.
[0019] Figure 2 The cycle performance diagram of the synthetic material of the embodiment of the present invention and the synthetic material of the comparative example is shown in FIG.
[0020] Figure 3 The rate performance diagram of the synthetic material of the embodiment of the present invention and the synthetic material of the comparative example DETAILED DESCRIPTION
[0021] The technical scheme of the present invention will be clearly and completely described below in combination with the embodiments and comparative examples of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative labor conditions belong to the scope of protection of the present invention.
[0022] Example:
[0023] Weigh Ni(CH3COO)2·4H2O, Co(CH3COO)2·4H2O and Mn(CH3COO)2·4H2O according to the stoichiometric ratio and dissolve them in 100ml of deionized water, which is recorded as solution A. Weigh CH3COOLi·2H2O and C6H8O7·H2O according to the molar ratio of 6:5 and dissolve them in 100ml of deionized water, which is recorded as solution B. Add solution A dropwise into solution B and stir evenly. Adjust the pH of the AB mixed solution to 7 with ammonia water. After fully stirring, move it into a water bath, set the temperature to 100℃, and stir continuously. After a while, add agar powder (the mass ratio of agar powder to transition metal salt is 10%) and stir continuously until the agar powder is completely dissolved. Then, keep stirring under 80℃ water bath conditions until a purple-red gel state is formed. Put it in an oven and dry it at 140℃ for 24h. After grinding, the mixture was pre-calcined at 450°C for 5 h and calcined at 850°C for 14 h under air conditions. After cooling, the mixture was taken out, ground and sieved to obtain 10% agar-assisted synthesized Li 1.2 Ni 0.15 Co 0.15 Mn 0.5 O2 material.
[0024] Comparative Example:
[0025] Weigh Ni(CH3COO)2·4H2O, Co(CH3COO)2·4H2O and Mn(CH3COO)2·4H2O according to the stoichiometric ratio and dissolve them in 100ml deionized water, which is recorded as solution A. Weigh CH3COOLi·2H2O and C6H8O7·H2O according to the molar ratio of 6:5 and dissolve them in 100ml deionized water, which is recorded as solution B. Add solution A dropwise into solution B and stir evenly. Adjust the pH of the AB mixed solution to 7 with ammonia water. After fully stirring, move it into a water bath, set the temperature to 100℃, and stir continuously. After a while, keep stirring under 80℃ water bath conditions until a gel state is formed. Put it in an oven and dry it at 140℃ for 24h. After grinding, pre-calculate at 450℃ for 5h and calcine at 850℃ for 14h in air. After cooling, take out, grind and sieve to obtain the comparative example material.
[0026] The two materials of the embodiment and the comparative example were assembled with a metal lithium sheet into a button cell and the electrochemical performance was tested. Cyclic performance test: The voltage window of the test was 2.0-4.8V, and the current of the first 4 cycles was 0.1C (1C = 250mAh·g -1 ), the current for 5-100 cycles is 0.5C. Rate performance test: The voltage window of the test is 2.0-4.8V, and the currents are 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 0.1C (4 cycles each). The cycle performance of the example materials and the comparative example materials is shown in Figure 2 At 0.1C current, the first cycle discharge capacity of the example material is 260.2 mAh g -1 After 100 cycles of charge and discharge at 0.5C current, the discharge specific capacities of the comparative material and the example material were 92.8 mAh·g -1 、145.3mAh·g -1 The capacity retention rate of the example material is as high as 70.0%, which is 25.4% higher than that of the comparative example material. Figure 3 As can be seen from the figure, the rate performance of the example material is more excellent. Through comparative experiments, it is found that the cycle and rate performance of the lithium-rich manganese-based positive electrode material prepared by the agar-assisted sol-gel method are significantly improved.
Claims
1. A lithium-rich manganese-based positive electrode material prepared by an agar-assisted sol-gel method, characterized in that: Agar was used as an auxiliary agent to prepare lithium-rich manganese-based cathode material Li 1.2 Ni 0.15 Co 0.15 Mn 0.5 O2. Its preparation method is simple, green and environmentally friendly, which significantly improves the cycle and rate performance of lithium-rich manganese-based positive electrode materials.
2. The lithium-rich manganese-based positive electrode material prepared by the agar-assisted sol-gel method according to claim 1, characterized in that: The preparation method is simple and green.
3. The lithium-rich manganese-based positive electrode material prepared by the agar-assisted sol-gel method according to claim 1, characterized in that: Adding an appropriate amount of agar as an auxiliary agent makes the synthesized lithium-rich manganese-based cathode material Li 1.2 Ni 0.15 Co 0.15 Mn 0.5 O2 performance improvement.
4. The lithium-rich manganese-based positive electrode material prepared by the agar-assisted sol-gel method according to claim 1, characterized in that: The initial water bath temperature is 100°C. After agar powder is added and completely dissolved, the water bath temperature is 80°C.