Imidazolium cation comb cross-linked polybenzimidazole gel state proton exchange membrane and preparation method thereof
By preparing an imidazolium cationic comb-shaped cross-linked polybenzimidazole gel proton exchange membrane, the "trade-off" problem between proton conductivity and mechanical strength was solved, achieving high proton conductivity and stability at low acid doping levels and improving the durability of fuel cells.
Patent Information
- Application Number
- CN202411127934.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
Existing proton exchange membranes exhibit a "trade-off" effect between proton conductivity and mechanical strength and chemical stability in high-temperature proton exchange membrane fuel cells. Furthermore, excessive phosphoric acid doping leads to membrane mechanical failure and phosphoric acid leakage, affecting the durability of the fuel cell.
An imidazolium cationic comb-shaped crosslinked polybenzimidazole gel proton exchange membrane was prepared by phase inversion method. By forming an imidazolium cationic comb-shaped crosslinked network structure, the proton transport channels are enhanced, and phosphoric acid leakage is reduced through strong acid-base interaction, thereby improving the membrane's PA retention capacity and mechanical properties.
At lower acid doping levels, proton exchange membranes exhibit high proton conductivity and stability, improving creep resistance and mechanical strength, and extending the lifespan of fuel cells.
Smart Images

Figure CN119009039A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cell proton exchange membranes, and in particular to an imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane and a preparation method thereof. The proton exchange membrane still has high proton conductivity at a relatively low acid doping level. Background Art
[0002] Proton exchange membrane fuel cell (PEMFC) is an energy conversion device that converts hydrogen energy into electrical energy. It has the advantages of being noiseless, safe, and efficient, and has a wide range of applications. As the core component of fuel cells, high-temperature proton exchange membranes (HT-PEMs) have received increasing attention. Since the first report of phosphoric acid-doped polybenzimidazole (PA / PBI) membranes for HT-PEMFC in 1995, PBI membranes have been widely studied as one of the most promising HT-PEMs.
[0003] The traditional method of producing PBI is through multi-step solution casting. The dense PBI membrane prepared has excellent mechanical properties and low gas permeability. However, due to the dense structure inside the membrane and the small free volume space, only a small amount of phosphoric acid can be doped, and a high proton conductivity cannot be achieved, so protons cannot be efficiently transmitted, and the overall performance and efficiency of practical fuel cell applications need to be improved.
[0004] In recent years, the polyphosphoric acid (PPA) sol-gel method has shown great potential in the preparation of high molecular weight PBI gel membranes. PA / PBI gel membranes have excellent proton conductivity due to excessive PA doping. However, due to the plasticization of phosphoric acid and the dissolution of the polymer matrix, a higher PA doping content easily leads to mechanical failure of the membrane. From the perspective of the trade-off effect between proton conductivity and structural stability, increasing proton conductivity usually reduces the mechanical strength and chemical stability of the membrane. In addition, during the operation of the fuel cell, excessive PA easily escapes from the HT-PEM. These problems will reduce the durability of HT-PEMFC and limit its application. Therefore, it is urgent to develop proton exchange membranes with high proton conductivity at lower acid doping levels in the field of HT-PEMFC.
[0005] The present invention proposes a gel-state PBI proton exchange membrane prepared by a phase inversion method, and a PBI proton membrane with an imidazolium cation comb-like cross-linked network structure formed in the membrane is prepared by a post-modification method combining nucleophilic substitution with free radical polymerization. (1) The new imidazolium cation proton transport channel formed promotes proton transport, thereby enhancing proton conductivity. (2) The formed quaternary ammonium salt alkaline site has a strong acid-base interaction with PA, which can effectively reduce the leakage of PA and improve the PA retention capacity in the membrane. (3) The creep resistance and mechanical properties of the sol-gel PBI membrane are improved by increasing the connection density of the gel network by introducing a comb-like cross-linked network. Because the above-mentioned preparation still has high proton conductivity at a lower acid doping level, there is a mutually restrictive relationship between different performance indicators when designing and optimizing the proton exchange membrane used in fuel cells. The present invention overcomes the "trade-off" effect of traditional proton exchange membranes in "acid doping level-proton conductivity performance", is a technical innovation in this field, and shows commercial application value in PEMFC systems. Summary of the invention
[0006] In view of the shortcomings of existing proton exchange membranes, the present invention provides an imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane with high proton conductivity at a low acid doping level and a preparation method thereof.
[0007] The technical solution of the present invention is as follows:
[0008] An imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane, comprising imidazolium cation comb-shaped cross-linked polybenzimidazole, anion H2PO4 - (to balance the charge), phosphoric acid and water;
[0009] The structural formula of imidazolium cationic comb-shaped cross-linked polybenzimidazole is as follows:
[0010]
[0011] Where: x = 1 to 3, y = 1 to 3, m = 10 to 5000, n = 10 to 5000
[0012] The imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane of the present invention has a solid content of 5-20wt%, phosphoric acid and water in the membrane are doped with 85wt% phosphoric acid solution, and the acid doping level is 10-40mol PA / PRU.
[0013] The specific surface area of the imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane of the present invention is 100 to 400 m 2 / g, pore size 0.1~100nm.
[0014] The method for preparing the imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane of the present invention comprises the following steps:
[0015] (1) In an inert atmosphere, 3,3-diaminobenzidine, a dicarboxylic acid monomer and a solvent polyphosphoric acid are mixed to obtain a polybenzimidazole polymer solution through a condensation reaction;
[0016] The dicarboxylic acid monomer is selected from one or a mixture of isophthalic acid and terephthalic acid;
[0017] The preferred mass ratio of 3,3-diaminobenzidine to dicarboxylic acid monomer is 2.07:1.60;
[0018] In the preferred reaction system, the total mass fraction of 3,3-diaminobenzidine and dicarboxylic acid monomer is 1 to 10 wt %;
[0019] The preferred condensation reaction temperature is 190°C and the reaction time is 20h;
[0020] (2) scraping the polymer solution obtained in step (1) onto a glass substrate to obtain an initial polybenzimidazole gel proton exchange membrane through phase inversion;
[0021] The preferred scraping film thickness is 0.1 to 0.3 mm;
[0022] The phosphoric acid content of the obtained initial polybenzimidazole gel proton exchange membrane is 45-75wt% and the acid doping level is 16-60mol PA / PRU;
[0023] (3) soaking the initial polybenzimidazole gel proton exchange membrane obtained in step (2) in deionized water until the pH is neutral (to remove a large amount of phosphoric acid doped in the membrane), then immersing it in a halogenated monoolefin solution, reacting at 50 to 90° C. for 12 to 24 hours, and washing it to obtain a polybenzimidazole gel proton exchange membrane with side-chain grafted monoolefins;
[0024] The halogenated monoolefin is selected from one or more of 3-bromopropylene, 3-chloropropylene, 4-bromobutylene, 4-chlorobutylene, 5-bromopentene and 5-chloropentene;
[0025] The concentration of the halogenated monoolefin solution is 0.05-0.7 mol / L, and the solvent is one or more of ethanol, methanol, ether, carbon tetrachloride, chloroform, dichloromethane, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0026] (4) placing the polybenzimidazole gel proton exchange membrane with side-chain grafted monoolefins formed in step (3) into an imidazolium salt solution having a terminal olefin functional group, reacting at 50 to 90° C. for 18 to 24 hours under the action of an initiator, cleaning to obtain a modified membrane material, immersing the modified membrane material in phosphoric acid for acid doping, and obtaining the imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane;
[0027] The imidazolium salt having a terminal olefin functional group is selected from one or more of 1-allyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium bromide, 1-allyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium bromide, 1-allyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium bromide, 1-allyl-3-methylimidazolium chloride, and 1-allyl-3-methylimidazolium bromide;
[0028] The concentration of the imidazolium salt solution having a terminal olefin functional group is 0.05-0.7 mol / L, and the solvent is one or more of ethanol, methanol, ether, carbon tetrachloride, chloroform, dichloromethane, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0029] The initiator is azobisisobutyronitrile, and the content in the reaction system ranges from 1 to 10 wt%;
[0030] Preferably, the modified membrane material is immersed in 85wt% phosphoric acid for ≥1 day for acid doping, and the halogen anions (from the imidazolium salt) in the modified membrane material are exchanged into H2PO4 through the acid doping reaction. - .
[0031] The imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane of the present invention still has high proton conductivity at a relatively low acid doping level and can be used in fuel cells.
[0032] The beneficial effects of the present invention are:
[0033] The imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane of the present invention has good stability at 25°C, 80°C, 80%RH and 40%RH, when the acid doping level is reduced from 48.77 mol PA / PRU to 14.59 mol PA / PRU, and the proton conductivity at 0°C is increased from 0.01S / cm to 0.019S / cm, the proton conductivity at 25°C is increased from 0.032S / cm to 0.073S / cm, the proton conductivity at 80°C is increased from 0.127S / cm to 0.145S / cm, and the proton conductivity at 200°C is increased from 0.256S / cm to 0.332S / cm.
[0034] The imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane of the present invention overcomes the "trade-off" effect between "phosphoric acid doping level-proton conductivity performance" in this field. The imidazolium cation network formed has efficient phosphoric acid retention capacity, excellent proton conductivity and stability, improved creep resistance and mechanical strength, and exhibited excellent performance in HT-PEMFC durability tests, which is expected to increase the service life of PEMFC. It is suitable for the field of proton exchange membrane fuel cells and has good commercial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 : Proton conductivity of comparative examples and examples.
[0036] Figure 2 : Proton conductivity of comparative examples and examples.
[0037] Figure 3 : Infrared analysis spectra of comparative examples and some embodiments.
[0038] Figure 4 : Comparative Examples and Partial Examples 13 C NMR spectrum.
[0039] Figure 5 : Film components of comparative examples and some examples.
[0040] Figure 6 : Conductivity of comparative examples and some examples at 25°C and 80%RH.
[0041] Figure 7 : Conductivity of comparative examples and some examples at 80°C and 40%RH.
[0042] Figure 8 : Electrical conductivity and acid doping level of comparative examples and some examples at 200°C.
[0043] Fig. 9 : Conductivity and acid doping level of comparative examples and some examples at 0°C.
[0044] Fig.10 : Creep resistance of comparative examples and some embodiments.
[0045] Fig.11 : Mechanical properties diagram of comparative examples and some embodiments.
[0046] Fig.12 : Fuel cell durability test of some embodiments. DETAILED DESCRIPTION
[0047] In order to facilitate the understanding of the present invention, the present invention will be more fully described in conjunction with the following examples. However, the present invention can be implemented in many different forms, and the scope of protection is not limited to the embodiments described herein.
[0048] Comparative Example:
[0049] (1) 2.07 g of 3,3-diaminobenzidine and 1.60 g of terephthalic acid were added to a three-necked reaction bottle equipped with a mechanical stirrer, and 180 g of polyphosphoric acid was used as a solvent. The mixture was reacted at 190° C. for 20 hours under the protection of a nitrogen flow.
[0050] (2) The obtained polymer solution is scraped on a glass substrate with a scraping frame for phase inversion (scraping thickness 0.2 mm, the same below). Since polyphosphoric acid will be hydrolyzed and converted into phosphoric acid in the air, a PA / PBI gel proton membrane is prepared through a solution-gel phase transition process, i.e., an initial PA / PBI gel membrane;
[0051] The obtained PA / PBI gel proton membrane was analyzed and tested:
[0052] Experimental results: Phosphoric acid doping level: 48.77 mol PA / PRU.
[0053] Anhydrous proton conductivity: 0℃ conductivity: 0.011S / cm; 25℃ conductivity: 0.032S / cm; 80℃ conductivity: 0.128S / cm; 200℃ conductivity: 0.256S / cm.
[0054] In addition, the conductivity stability of the membranes at 25°C 80% RH and 80°C 40% RH was tested.
[0055] Embodiment 1:
[0056] (1) 2.07 g of 3,3-diaminobenzidine and 1.60 g of terephthalic acid were added to a three-necked reaction bottle equipped with a mechanical stirrer, and 180 g of polyphosphoric acid was used as a solvent. The mixture was reacted at 190° C. for 20 hours under the protection of a nitrogen flow.
[0057] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion. Since polyphosphoric acid will be hydrolyzed and converted into phosphoric acid in the air, a PA / PBI gel proton membrane is prepared through a solution-gel phase transition process;
[0058] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and then a nucleophilic substitution reaction was carried out at 70° C. for 20 hours with a 0.2 mol / L 3-bromopropylene ethanol solution, and then the membrane was cleaned with ethanol and deionized water.
[0059] (4) The membrane cleaned in (3) was placed in a 0.2 mol / L 1-allyl-3-methylimidazolium chloride DMAc solution, and free radical polymerization was carried out at 70°C for 20 h using 4% equivalent of azobisisobutyl as an initiator under nitrogen atmosphere. The membrane was cleaned with DMAc and deionized water in turn, and then immersed in 85 wt % phosphoric acid for 72 h to obtain a phosphoric acid-doped cross-linked polybenzimidazole gel proton exchange membrane, namely, PA / comb-shaped cross-linked PBI gel membrane-2.
[0060] The PA / comb-shaped cross-linked PBI gel membrane-2 obtained in Example 1 was analyzed and tested:
[0061] Experimental results: Phosphoric acid doping level: 34.18 mol PA / PRU, which is 14.59 mol PA / PRU lower than 48.77 mol PA / PRU of the comparative example.
[0062] 0℃ conductivity: 0.016S / cm, which is 0.005S / cm higher than the control example; 25℃ conductivity: 0.073S / cm, which is 0.0041S / cm higher than the control example; 80℃ conductivity: 0.146S / cm, which is 0.018S / cm higher than the control example; 200℃ conductivity: 0.332S / cm, which is 0.076S / cm higher than the control example.
[0063] In addition, the conductivity stability of the membrane was tested at 25°C 80% RH and 80°C 40% RH, both of which showed better proton transport performance and stability than the comparative example.
[0064] Embodiment 2:
[0065] (1) 2.07 g of 3,3-diaminobenzidine and 1.60 g of terephthalic acid were added to a three-necked reaction bottle equipped with a mechanical stirrer, and 180 g of polyphosphoric acid was used as a solvent. The mixture was reacted at 190° C. for 20 hours under the protection of a nitrogen flow.
[0066] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion. Since polyphosphoric acid will naturally hydrolyze and convert into phosphoric acid in the air, a PA / PBI gel proton membrane is prepared through a solution-gel phase transition;
[0067] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and then nucleophilic substitution was carried out with 0.4 mol / L 3-bromopropylene ethanol solution at 70° C. for 20 hours, and then washed with ethanol and deionized water.
[0068] (4) The membrane cleaned in (3) was placed in a 0.4 mol / L 1-allyl-3-methylimidazolium chloride DMAc solution, and free radical polymerization was carried out at 70°C for 20 h using 4% equivalent of azobisisobutyl as an initiator under nitrogen atmosphere. The membrane was cleaned with DMAc and deionized water in turn, and then immersed in 85 wt % phosphoric acid for 72 h to obtain a phosphoric acid-doped cross-linked polybenzimidazole gel proton exchange membrane, namely, PA / comb-shaped cross-linked PBI gel membrane-4.
[0069] The PA / comb-shaped cross-linked PBI gel membrane-4 obtained in Example 2 was analyzed and tested:
[0070] Experimental results: Phosphoric acid doping level: 27.47 mol PA / PRU, which is 21.30 mol PA / PRU lower than the control group.
[0071] 0℃ conductivity: 0.023S / cm, which is 0.012S / cm higher than the control group; 25℃ conductivity: 0.066S / cm, which is 0.034S / cm higher than the control group; 80℃ conductivity: 0.163S / cm, which is 0.035S / cm higher than the control group; 200℃ conductivity: 0.270S / cm, which is 0.014S / cm higher than the control group.
[0072] In addition, the conductivity stability of the membrane was tested at 25°C 80% RH and 80°C 40% RH, both of which showed better proton transport performance and stability than the comparative example.
[0073] Embodiment 3:
[0074] (1) 2.07 g of 3,3-diaminobenzidine and 1.60 g of terephthalic acid were added to a three-necked reaction bottle equipped with a mechanical stirrer, and 180 g of polyphosphoric acid was used as a solvent. The mixture was reacted at 190° C. for 20 hours under the protection of a nitrogen flow.
[0075] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion. Since polyphosphoric acid will be hydrolyzed and converted into phosphoric acid in the air, a PA / PBI gel proton membrane is prepared through a solution-gel phase transition process;
[0076] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and then nucleophilic substitution was carried out with 0.3 mol / L 3-bromopropylene ethanol solution at 70° C. for 20 hours, and then washed with ethanol and deionized water.
[0077] (4) The membrane cleaned in (3) was placed in a 0.3 mol / L 1-allyl-3-methylimidazolium chloride DMAc solution, and free radical polymerization was carried out at 70°C for 20 h using 4% equivalent of azobisisobutyl as an initiator under nitrogen atmosphere. The membrane was cleaned with DMAc and deionized water in turn, and then immersed in 85 wt % phosphoric acid for 72 h to obtain a phosphoric acid-doped cross-linked polybenzimidazole gel proton exchange membrane, namely, PA / comb-shaped cross-linked PBI gel membrane-3.
[0078] The PA / comb-shaped cross-linked PBI gel membrane-3 obtained in Example 3 was analyzed and tested:
[0079] Experimental results: Phosphoric acid doping level: 30.80 mol PA / PRU, which is 17.97 mol PA / PRU lower than the control example.
[0080] 0℃ conductivity: 0.025S / cm, which is 0.014 higher than the control example; 25℃ conductivity: 0.075S / cm, which is 0.043 higher than the control example; 200℃ conductivity: 0.279S / cm, which is 0.023S / cm higher than the control example.
[0081] Embodiment 4:
[0082] (1) 2.07 g of 3,3-diaminobenzidine and 1.60 g of terephthalic acid were added to a three-necked reaction bottle equipped with a mechanical stirrer, and 180 g of polyphosphoric acid was used as a solvent. The mixture was reacted at 190° C. for 20 hours under the protection of a nitrogen flow.
[0083] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion. Since polyphosphoric acid will be hydrolyzed and converted into phosphoric acid in the air, a PA / PBI gel proton membrane is prepared through a solution-gel phase transition process;
[0084] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and then nucleophilic substitution was carried out with 0.1 mol / L 3-bromopropylene ethanol solution at 70° C. for 20 hours, and then washed with ethanol and deionized water.
[0085] (4) The membrane cleaned in (3) was placed in a 0.1 mol / L 1-allyl-3-methylimidazolium chloride DMAc solution, and free radical polymerization was carried out at 70°C for 20 hours using 4% equivalent of azobisisobutyl as an initiator under nitrogen atmosphere. The membrane was cleaned with DMAc and deionized water in turn, and then immersed in 85 wt % phosphoric acid for 72 hours to obtain a phosphoric acid-doped cross-linked polybenzimidazole gel proton exchange membrane, namely, PA / comb-shaped cross-linked PBI gel membrane-1.
[0086] The PA / comb-shaped cross-linked PBI gel membrane-1 obtained in Example 4 was analyzed and tested:
[0087] Experimental results: 0℃ conductivity: 0.016S / cm; 25℃ conductivity: 0.053S / cm; 200℃ conductivity: 0.249S / cm.
Claims
1. An imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane, characterized in that: Combination of imidazolium cation crosslinked polybenzimidazole, anion H2PO4 - , phosphoric acid and water; The structural formula of imidazolium cationic comb-shaped cross-linked polybenzimidazole is as follows: In the formula: x=1~3, y=1~3, m=10~5000, n=10~5000.
2. The imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane according to claim 1, characterized in that: The solid content of the film is 5-20 wt %, and the acid doping level is 10-40 mol PA / PRU.
3. The imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane according to claim 1, characterized in that: The specific surface area of the membrane is 100~400m 2 / g, pore size 0.1~100nm.
4. The method for preparing the imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane according to claim 1, characterized in that: The steps include: (1) In an inert atmosphere, 3,3-diaminobenzidine, a dicarboxylic acid monomer and a solvent polyphosphoric acid are mixed to obtain a polybenzimidazole polymer solution through a condensation reaction; The dicarboxylic acid monomer is selected from one or a mixture of isophthalic acid and terephthalic acid; (2) scraping the polymer solution obtained in step (1) onto a glass substrate to obtain an initial polybenzimidazole gel proton exchange membrane through phase inversion; (3) soaking the initial polybenzimidazole gel proton exchange membrane obtained in step (2) in deionized water until the pH is neutral, then immersing it in a halogenated monoolefin solution, reacting at 50 to 90° C. for 12 to 24 hours, and washing it to obtain a polybenzimidazole gel proton exchange membrane with a side-chain grafted monoolefin; The halogenated monoolefin is selected from one or more of 3-bromopropylene, 3-chloropropylene, 4-bromobutylene, 4-chlorobutylene, 5-bromopentene and 5-chloropentene; (4) placing the polybenzimidazole gel proton exchange membrane with side-chain grafted monoolefins formed in step (3) into an imidazolium salt solution having a terminal olefin functional group, reacting at 50 to 90° C. for 18 to 24 hours under the action of an initiator, cleaning to obtain a modified membrane material, immersing the modified membrane material in phosphoric acid for acid doping, and obtaining the imidazolium cation comb-shaped cross-linked polybenzimidazole gel proton exchange membrane; The imidazolium salt having a terminal olefin functional group is selected from one or more of 1-allyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium bromide, 1-allyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium bromide, 1-allyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium bromide, 1-allyl-3-methylimidazolium chloride, and 1-allyl-3-methylimidazolium bromide; The initiator is azobisisobutyronitrile.
5. The preparation method according to claim 4, characterized in that: In step (1), the condensation reaction temperature is 190° C. and the reaction time is 20 h.
6. The preparation method according to claim 4, characterized in that: In step (2), the scraping film thickness is 0.1 to 0.3 mm.
7. The preparation method according to claim 4, characterized in that: In step (3), the concentration of the halogenated monoolefin solution is 0.05-0.7 mol / L, and the solvent is one or more of ethanol, methanol, ether, carbon tetrachloride, chloroform, dichloromethane, N,N-dimethylformamide, and N,N-dimethylacetamide.
8. The preparation method according to claim 4, characterized in that: In step (4), the concentration of the imidazolium salt solution having a terminal olefin functional group is 0.05 to 0.7 mol / L, and the solvent is one or more of ethanol, methanol, ether, carbon tetrachloride, chloroform, dichloromethane, N,N-dimethylformamide, and N,N-dimethylacetamide.
9. The preparation method according to claim 4, characterized in that: In step (4), the modified membrane material is immersed in 85 wt % phosphoric acid for ≥ 1 day for acid doping.
10. Use of the imidazolium cation comb-like cross-linked polybenzimidazole gel proton exchange membrane as claimed in claim 1 in a fuel cell.