Lithium ion battery with high and low temperature resistance and preparation method thereof
By setting a low-temperature and high-temperature resistant material layer on the outer surface of the lithium-ion battery case, combined with a buffered thermal conductivity and thermal insulation material layer, the performance problems of lithium-ion batteries at extreme temperatures are solved, and stable operation within a wide temperature range is achieved. Improved safety.
Patent Information
- Application Number
- CN202411206052.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Traditional lithium-ion batteries have unstable performance in high and low temperature environments, and are difficult to meet the requirements of use under extreme temperature conditions, resulting in performance degradation and safety hazards.
The low-temperature resistant material layer and high-temperature resistant material layer are arranged on the outer surface of the battery case, which have phase transition temperatures of -12℃ to -15℃ and 57℃ to 62℃ respectively. The temperature adjustment ability of the battery is improved through groove design and material combination. A buffering and thermally conductive material layer and thermally insulated buffering material layer are embedded on the outer surface of the housing to enhance the thermal conductivity and thermal insulation performance of the battery.
It effectively expands the operating temperature range of lithium-ion batteries, ensures stable operation within the temperature range of -15℃ to 62℃, improves the battery's high and low temperature resistance and safety, and maintains the overall structural strength and energy density of the battery.
Smart Images

Figure CN119009068A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion battery with high and low temperature resistance and a preparation method thereof. Background Art
[0002] As a key component in modern energy applications, lithium-ion batteries are widely used in consumer electronics, electric vehicles, and large-scale energy storage systems due to their high energy density, long cycle life, and environmental friendliness. However, with the diversification and extreme application scenarios, the performance limitations of traditional lithium-ion batteries in high and low temperature environments have become increasingly prominent, becoming a bottleneck restricting their further development.
[0003] Lithium-ion batteries face serious performance degradation problems in low-temperature environments. When the temperature drops, the viscosity of the electrolyte increases significantly, causing the migration speed of lithium ions to decrease significantly. This not only increases the internal impedance of the battery, but also causes a sharp drop in charging and discharging efficiency. Specifically, the charging time is prolonged and the discharge capacity is reduced, which seriously affects the actual use of the battery in cold areas or low-temperature application scenarios. For example, in an environment below minus 15°C, the discharge capacity of a conventional lithium-ion battery may drop to less than 50% of that at room temperature.
[0004] On the other hand, high temperature environments also pose a major challenge to the performance and safety of lithium-ion batteries. Rising temperatures accelerate side reactions inside the battery, such as electrolyte decomposition and structural changes in positive and negative electrode materials. These reactions not only lead to rapid decay of battery capacity and a significant shortening of cycle life, but may also cause more serious safety issues. For example, in a high temperature environment above 60°C, the battery may experience thermal runaway, causing safety accidents such as battery swelling, smoking, and even explosion.
[0005] In the existing technology, researchers have tried many methods to improve the temperature adaptability of lithium-ion batteries, such as developing new electrolyte additives, improving electrode material structure, optimizing battery management systems, etc. However, these methods can only improve the performance of batteries within a specific temperature range to a certain extent, and it is difficult to meet the use requirements in high and low temperature environments at the same time. In addition, some improvement measures may increase the manufacturing cost of the battery or reduce other performance indicators (such as energy density).
[0006] Therefore, developing a lithium-ion battery that can maintain stable performance over a wide temperature range, especially one that can still work efficiently under extreme high and low temperature conditions, is of great significance for expanding the application areas of the battery, improving user experience and ensuring safety of use. Summary of the invention
[0007] The main purpose of the present invention is to provide a lithium ion battery with high and low temperature resistance and a preparation method thereof in view of the deficiency that the existing lithium ion batteries cannot be used under high and low temperature conditions.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0009] A lithium-ion battery with high and low temperature resistance, comprising: a battery cell and a shell encapsulating the battery cell;
[0010] The outer surface of the shell is provided with a first groove and a second groove, and the first groove and the second groove are embedded in the outer surface of the shell side by side, and the first groove and the second groove are respectively extended from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape;
[0011] The first groove is provided with a low temperature resistant material layer, and the phase change temperature of the low temperature resistant material layer is -12°C to -15°C; the second groove is provided with a high temperature resistant material layer, and the phase change temperature of the high temperature resistant material layer is 57°C to 62°C;
[0012] The thickness of the low-temperature resistant material layer is the same as the depth of the first groove, and the thickness of the high-temperature resistant material layer is the same as the depth of the second groove; and the outer surfaces of the low-temperature resistant material layer, the high-temperature resistant material layer and the shell are on the same horizontal plane.
[0013] Preferably, the low-temperature resistant material layer comprises the following components in weight proportion: 40-50 parts of n-tridecane, 25-35 parts of n-dodecane, 10-15 parts of 2-methylpentane, 3-5 parts of polyvinyl alcohol, 2-4 parts of graphene, 1-2 parts of nano-alumina, and 0.5-1 part of silica aerogel.
[0014] Preferably, the high temperature resistant material layer comprises the following components in weight proportion: 45-55 parts of octadecanoic acid glycerol, 20-25 parts of palmitic acid, 10-15 parts of polyethylene glycol 4000, 3-5 parts of carbon nanotubes, 2-3 parts of boron nitride nanosheets, 1-2 parts of expanded graphite, and 0.5-1 part of nano magnesium oxide.
[0015] Preferably, the depth of the first groove is H1, the depth of the second groove is H2, the thickness of the low-temperature resistant material layer is h1, the thickness of the high-temperature resistant material layer is h2, and the wall thickness of the shell is H; wherein H, H1, H2, h1 and h2 satisfy the relationship: h1=h2=H1=H2; 0.2H≤H1≤0.6H; 0.2H≤H2≤0.6H.
[0016] Preferably, the forward projection area of the low-temperature resistant material layer is S1, the forward projection area of the high-temperature resistant material layer is S2, and the forward projection area of the shell is S; wherein S1, S2 and S satisfy the relationship: 0.6S≤S1+S2≤S.
[0017] Preferably, the outer surface of the shell is further provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape;
[0018] The third groove is provided with a buffer heat-conducting material layer; the thickness of the buffer heat-conducting material layer is greater than the thickness of the low-temperature resistant material layer or the high-temperature resistant material layer, and the buffer heat-conducting material layer protrudes from the outer surface of the shell;
[0019] The buffer thermal conductive material layer includes a first foam aluminum, a second foam aluminum and a third foam aluminum, which are arranged in sequence from the outside to the inside. The density ρ1 of the first foam aluminum, the density ρ2 of the second foam aluminum and the density ρ3 of the third foam aluminum satisfy the relationship: ρ1>ρ2>ρ3; and the first foam aluminum, the second foam aluminum and the third foam aluminum are all provided with an alternating pore structure, and the porosity Q1 of the first foam aluminum, the porosity Q2 of the second foam aluminum and the porosity Q3 of the third foam aluminum satisfy the relationship: Q1<Q2<Q3.
[0020] Preferably, the density ρ1 of the first foamed aluminum is 0.8-1.2 g / cm 3 The density of the second aluminum foam is ρ2 0.5-0.8 g / cm 3 The density of the third foam aluminum is ρ3 0.2-0.5 g / cm 3 ;
[0021] The porosity Q1 of the first foam aluminum is 45% to 60%; the porosity Q2 of the second foam aluminum is 60% to 75%; and the porosity Q3 of the third foam aluminum is 75% to 90%.
[0022] Preferably, the outer surface of the shell is further provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape;
[0023] The third groove is provided with a heat-insulating buffer material layer, the thickness of the heat-insulating buffer material layer is greater than the thickness of the low-temperature resistant material layer or the high-temperature resistant material layer, and the heat-insulating buffer material layer protrudes from the outer surface of the shell;
[0024] The thermal insulation buffer material layer is ceramic silicone foam, which includes the following components in weight proportion: 30-40 parts of vinyl silicone oil, 10-20 parts of white carbon black, 20-50 parts of nano-ceramic powder, 0.1-1.0 parts of ethynyl cyclohexanol, 1-10 parts of hydrogen-containing silicone oil, 1-10 parts of hydroxy silicone oil, 0.1-1.0 parts of platinum catalyst, 10-20 parts of β-eucryptite, and 1-8 parts of halloysite nanotubes.
[0025] Preferably, the outer surface of the shell is further provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape;
[0026] The third groove is provided with modified thermally conductive silicone, the porosity of the modified thermally conductive silicone is 65% to 85%, the thickness of the modified thermally conductive silicone is greater than the thickness of the low-temperature resistant material layer or the high-temperature resistant material layer, and the modified thermally conductive silicone protrudes from the outer surface of the shell.
[0027] In addition, the present invention also provides a method for preparing a lithium ion battery with high and low temperature resistance, comprising the following steps:
[0028] 1) Setting a first groove and a second groove on the outer surface of the housing by laser engraving, etching or stamping;
[0029] 2) preparing a low temperature resistant material layer slurry and a high temperature resistant material layer slurry respectively;
[0030] 3) applying the low temperature resistant material layer slurry to the first groove, and applying the high temperature resistant material layer slurry to the second groove;
[0031] 4) Drying the outer surface of the shell, and then encapsulating the battery cell into the shell to obtain the lithium ion battery.
[0032] Compared with the prior art, the present invention has at least the following beneficial effects:
[0033] 1) The present invention effectively solves the performance problem of lithium-ion batteries at extreme temperatures by respectively arranging a low-temperature resistant material layer and a high-temperature resistant material layer on the outer surface of the battery housing, greatly expanding the operating temperature range of the battery. Among them, the phase change temperature of the low-temperature resistant material layer is -12℃~-15℃, and the phase change temperature of the high-temperature resistant material layer is 57℃~62℃. The design of the temperature-resistant material layer can absorb or release heat within a specific temperature range, so that the lithium-ion battery can work stably within the temperature range of -15℃ to 62℃.
[0034] 2) The present invention provides a first groove and a second groove embedded side by side on the outer surface of the shell, and the first groove and the second groove are respectively extended from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape, and then the low-temperature resistant material layer and the high-temperature resistant material layer are respectively provided in the first groove and the second groove, and the outer surfaces of the low-temperature resistant material layer, the high-temperature resistant material layer and the shell are on the same horizontal plane. Through the above-mentioned structural design, the flatness and aesthetics of the battery appearance are guaranteed, and there is no need to increase the wall thickness of the battery shell to ensure that the high and low temperature resistance of the battery is effectively improved without losing the volume energy density of the battery. In addition, the zigzag design of the first groove and the second groove increases the heat exchange area and improves the temperature regulation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic structural diagram of a lithium-ion battery in one embodiment of the present invention;
[0036] Figure 2 is a top view of a lithium-ion battery in one embodiment of the present invention;
[0037] Figure 3 is a schematic structural diagram of a lithium-ion battery in another embodiment of the present invention;
[0038] Figure 4 is a cross-sectional view of a buffer thermal conductive material layer in another embodiment of the present invention;
[0039] Figure 5 is a schematic structural diagram of a lithium-ion battery in another embodiment of the present invention;
[0040] Figure 6 FIG. 4 is a schematic structural diagram of a lithium-ion battery in another embodiment of the present invention.
[0041] In the figure: 1. Shell; 2. Low temperature resistant material layer; 3. High temperature resistant material layer; 4. Buffer thermal conductive material layer; 41. First foam aluminum; 42. Second foam aluminum; 43. Third foam aluminum; 5. Thermal insulation buffer material layer; 6. Modified thermal conductive silicone. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Please refer to the attached Figures 1-2The present embodiment provides a lithium-ion battery with high and low temperature resistance, comprising: a battery cell and a shell 1 for encapsulating the battery cell; wherein the battery cell comprises a positive electrode sheet, a separator and a negative electrode sheet stacked and wound in sequence; wherein the shell material may be made of an aluminum shell, a steel shell or an aluminum alloy material;
[0044] The outer surface of the shell 1 is provided with a first groove and a second groove, and the first groove and the second groove are embedded side by side on the outer surface of the shell 1, and the first groove and the second groove are respectively extended from the center of the outer surface of the shell 1 to the edge of the outer surface of the shell 1 in a zigzag shape;
[0045] The first groove is provided with a low temperature resistant material layer 2, and the phase change temperature of the low temperature resistant material layer 2 is -12°C to -15°C; the second groove is provided with a high temperature resistant material layer 3, and the phase change temperature of the high temperature resistant material layer 3 is 57°C to 62°C;
[0046] The thickness of the low temperature resistant material layer 2 is the same as the depth of the first groove, and the thickness of the high temperature resistant material layer 3 is the same as the depth of the second groove; and the outer surfaces of the low temperature resistant material layer 2, the high temperature resistant material layer 3 and the shell 1 are on the same horizontal plane.
[0047] In one implementation of the present application, the low-temperature resistant material layer 2 includes the following components in weight proportions: 40-50 parts of n-tridecane, 25-35 parts of n-dodecane, 10-15 parts of 2-methylpentane, 3-5 parts of polyvinyl alcohol, 2-4 parts of graphene, 1-2 parts of nano-alumina, and 0.5-1 part of silica aerogel.
[0048] Among them, n-tridecane and n-dodecane are used as the main phase change materials to provide low-temperature phase change ability. Mixing can adjust the phase change temperature and reduce the freezing point; 2-methylpentane further reduces the freezing point of the mixture, increases the fluidity of the material, and improves the low-temperature performance; polyvinyl alcohol (PVA) is used as a thickener and structural stabilizer to improve the mechanical strength and shape stability of the material; graphene significantly improves the thermal conductivity of the material and improves the distribution of heat in the phase change material; nano-alumina enhances the thermal stability of the material, improves thermal conductivity and mechanical strength; silica aerogel provides excellent thermal insulation performance, reduces heat loss, and improves the efficiency of the phase change material. The phase change temperature of the low-temperature resistant material layer 2 is -12℃~-15℃. When the phase change temperature is reached, it can quickly release heat, effectively adjust the battery temperature, and improve the low-temperature resistance of the battery.
[0049] The preparation method of the low temperature resistant material layer 2 is as follows:
[0050] (1) n-tridecane, n-dodecane and 2-methylpentane are mixed according to a proportion and stirred uniformly at room temperature;
[0051] (2) Dissolve polyvinyl alcohol (PVA) in a small amount of deionized water, heat to 60°C and stir until completely dissolved;
[0052] (3) slowly adding the solution of step (2) into the mixture of step (1), and uniformly dispersing the mixture using a high-speed shearing machine for 30 minutes;
[0053] (4) dispersing graphene in a small amount of ethanol and ultrasonically treating for 20 minutes;
[0054] (5) adding the suspension of step (4), nano-alumina and silica aerogel to the mixture of step (3) in sequence, and continuing high-speed shearing for 15 minutes to obtain a low-temperature resistant material layer slurry;
[0055] (6) Applying the low-temperature resistant material layer slurry to the first groove and drying it, thereby obtaining the low-temperature resistant material layer 2 with the desired shape and thickness.
[0056] In one implementation of the present application, the high temperature resistant material layer 3 includes the following components in weight proportions: 45-55 parts of octadecanoic acid glycerol, 20-25 parts of palmitic acid, 10-15 parts of polyethylene glycol 4000, 3-5 parts of carbon nanotubes, 2-3 parts of boron nitride nanosheets, 1-2 parts of expanded graphite, and 0.5-1 parts of nano magnesium oxide.
[0057] Among them, octadecanoic acid glycerol and palmitic acid are used as the main phase change materials to provide high-temperature phase change capability, and the mixed use can adjust the phase change temperature range; polyethylene glycol 4000 adjusts the phase change temperature, increases the heat capacity of the material, and improves the heat storage capacity; carbon nanotubes significantly improve the thermal conductivity of the material and improve the rapid distribution of heat in the phase change material; boron nitride nanosheets further enhance heat conduction and improve the thermal stability of the material; expanded graphite increases the specific surface area of the material, improves the heat exchange efficiency, and improves the thermal conductivity and flame retardancy of the material; nano magnesium oxide enhances the thermal stability and flame retardancy of the material and improves the structural integrity of the material at high temperatures. The phase change temperature of the high temperature resistant material layer 3 is 57°C to 62°C. When the phase change temperature is reached, it can quickly absorb heat, effectively adjust the battery temperature, and improve the high temperature resistance of the battery.
[0058] The preparation method of the high temperature resistant material layer 3 is as follows:
[0059] (1) Stearyl octadecanoate and palmitic acid are mixed according to a ratio, heated to melt in an oil bath at 85-95° C., and stirred evenly;
[0060] (2) adding polyethylene glycol 4000 to the molten mixture of step (1) and continuing to stir until it is completely dissolved;
[0061] (3) dispersing carbon nanotubes and boron nitride nanosheets in a small amount of N-methylpyrrolidone (NMP) and ultrasonically treating for 30 minutes;
[0062] (4) slowly adding the suspension of step (3) into the molten mixture of step (2), and stirring at high speed for 45 minutes;
[0063] (5) adding expanded graphite and nano magnesium oxide, and continuing high-speed stirring for 20 minutes to obtain a high-temperature resistant material layer slurry;
[0064] (6) Apply the high temperature resistant material layer slurry to the second groove and dry it to obtain the high temperature resistant material layer 3 with the required shape and thickness.
[0065] In one implementation of the present application, the depth of the first groove is H1, the depth of the second groove is H2, the thickness of the low-temperature resistant material layer 2 is h1, the thickness of the high-temperature resistant material layer 3 is h2, and the wall thickness of the shell 1 is H; wherein, H, H1, H2, h1 and h2 satisfy the relationship: h1=h2=H1=H2; 0.2H≤H1≤0.6H; 0.2H≤H2≤0.6H. By precisely controlling the size ratio of the first groove, the second groove, the low-temperature resistant material layer 2, the high-temperature resistant material layer 3 and the shell 1, the overall structural strength of the battery and the effective performance of high and low temperature resistance are guaranteed. If the depth of the groove is too small, it is difficult to carry the heat-resistant material layer. If the depth of the groove is too large, it will affect the strength of the shell 1. Therefore, this size ratio combination design ensures that the heat-resistant material layer does not affect the overall integration of the battery, but can fully exert its function.
[0066] In one implementation of the present application, the forward projection area of the low-temperature resistant material layer 2 is S1, the forward projection area of the high-temperature resistant material layer 3 is S2, and the forward projection area of the shell 1 is S; wherein S1, S2, and S satisfy the relationship: 0.6S≤S1+S2≤S. By controlling the sum of the forward projection areas of the low-temperature resistant material layer 2 and the high-temperature resistant material layer 3 to satisfy the above relationship, it is ensured that the coverage of the material layer is large enough to effectively adjust the temperature of the entire shell 1.
[0067] In one implementation according to the present application, as shown in the attached Figures 3-4 As shown, the outer surface of the shell 1 is also provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell 1 to the edge of the outer surface of the shell 1 in a zigzag shape;
[0068] The third groove is provided with a buffer thermal conductive material layer 4; the thickness of the buffer thermal conductive material layer 4 is greater than the thickness of the low temperature resistant material layer 2 or the high temperature resistant material layer 3, and the buffer thermal conductive material layer 4 protrudes from the outer surface of the housing 1;
[0069] The buffer thermal conductive material layer 4 includes a first foam aluminum 41, a second foam aluminum 42 and a third foam aluminum 43 which are arranged in sequence from the outside to the inside, and the density ρ1 of the first foam aluminum 41, the density ρ2 of the second foam aluminum 42 and the density ρ3 of the third foam aluminum 43 satisfy the relationship: ρ1>ρ2>ρ3; and the first foam aluminum 41, the second foam aluminum 42 and the third foam aluminum 43 are all provided with an alternating pore structure, and the porosity Q1 of the first foam aluminum 41, the porosity Q2 of the second foam aluminum 42 and the porosity Q3 of the third foam aluminum 43 satisfy the relationship: Q1<Q2<Q3.
[0070] Among them, each foam aluminum layer can be set in the third groove of the shell 1 by spraying, 3D printing, etc. Foam aluminum is a new type of lightweight functional material that has both metal and bubble characteristics, which can make it have excellent energy absorption and buffering effects and thermal conductivity, effectively absorb the expansion force of the battery, and minimize the overall mass of the battery pack; when the battery is grouped, the three-layer foam aluminum structure design with gradient density and porosity can effectively absorb and disperse the impact energy, and has good thermal conductivity and heat dissipation effects, thus providing excellent buffer protection and thermal conductivity and heat dissipation performance. Among them, the first foam aluminum 41 with high density and low porosity can first receive and disperse the external impact energy, reducing the impact force directly transmitted to the inside; the second foam aluminum 42 with medium density and high porosity can further absorb and disperse the remaining impact energy. The third foam aluminum 43 with low density and high porosity has extremely high energy absorption capacity, which can ultimately absorb and disperse the remaining impact energy and protect the battery cell. The present application realizes the effect of absorbing and dispersing impact energy layer by layer by innovatively combining the porosity and density of each layer, thereby significantly improving the buffering protection performance of the lithium-ion battery and ensuring the safety and reliability of the battery pack.
[0071] In one implementation of the present application, the density ρ1 of the first foam aluminum 41 is 0.8-1.2 g / cm 3 , preferably 0.95 g / cm 3 The density ρ2 of the second foam aluminum 42 is 0.5-0.8 g / cm 3 , preferably 0.65 g / cm 3 The density ρ3 of the third foam aluminum 43 is 0.2-0.5 g / cm 3 , preferably 0.35 g / cm 3 ;
[0072] The porosity Q1 of the first foam aluminum 41 is 45% to 60%, preferably 55%; the porosity Q2 of the second foam aluminum 42 is 60% to 75%, preferably 70%; the porosity Q3 of the third foam aluminum 43 is 75% to 90%, preferably 85%.
[0073] In one implementation according to the present application, as shown in the attached Figure 5 As shown, the outer surface of the shell 1 is also provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell 1 to the edge of the outer surface of the shell 1 in a zigzag shape;
[0074] The third groove is provided with a heat-insulating buffer material layer 5, the thickness of the heat-insulating buffer material layer 5 is greater than the thickness of the low-temperature resistant material layer 2 or the high-temperature resistant material layer 3, and the heat-insulating buffer material layer 5 protrudes from the outer surface of the shell 1;
[0075] The thermal insulation buffer material layer 5 is a ceramic silicone foam, which includes the following components in weight proportion: 30-40 parts of vinyl silicone oil, 10-20 parts of white carbon black, 20-50 parts of nano-ceramic powder, 0.1-1.0 parts of ethynyl cyclohexanol, 1-10 parts of hydrogen-containing silicone oil, 1-10 parts of hydroxy silicone oil, 0.1-1.0 parts of platinum catalyst, 10-20 parts of β-eucryptite, and 1-8 parts of halloysite nanotubes.
[0076] The ceramic silicone foam provided by the present invention not only has good elasticity under normal working conditions, but also can provide good buffering and protection for batteries when the batteries are grouped; moreover, at high temperatures, the ceramic silicone foam can quickly form a foam ceramic body with a self-supporting structure, and can maintain a high degree of pore structure retention rate, thereby exerting excellent heat insulation and flame retardant effects, and it can withstand the burning of flames above 1300°C for a long time, can effectively isolate the transfer of fire and temperature, and control the fire range within a single battery interval to avoid causing fires in adjacent batteries.
[0077] Among them, vinyl silicone oil is the main polymer matrix, which provides the required elasticity and flexibility in the foaming system; it can form a cross-linked structure by reacting with hydrogen-containing silicone oil, thereby enhancing the mechanical strength of the material. Silica is used as a reinforcing agent. Silica increases the tear strength and wear resistance of the composite material, while improving the compression resistance of silicone rubber, making the material less likely to deform even under higher loads. Nano-ceramic powder acts as a flame retardant. At high temperatures, nano-ceramic powder can promote the formation of a hard ceramic layer on the surface of the material, effectively preventing the further spread of flames and heat. Ethylene cyclohexanol is used as an inhibitor. This compound can control the rate of polymerization and avoid structural instability caused by too fast a reaction. Hydrogen-containing silicone oil acts as a cross-linking agent and reacts with vinyl silicone oil to form a silicone rubber network structure, enhancing the overall mechanical properties and thermal stability of the material. Hydroxyl silicone oil acts as a foaming agent in this system. Hydroxyl silicone oil decomposes and produces gas when heated to form a foam structure, thereby providing good cushioning properties and low density. Platinum catalyst catalyzes the addition cross-linking reaction of vinyl silicone oil and hydrogen silicone oil, improving the efficiency and uniformity of the reaction and ensuring the consistency of material performance. β-eucryptite, as a ceramic-forming agent, can promote the transformation of silicone rubber into ceramic body at high temperature, enhancing the high temperature resistance and structural stability of the material. Halloysite nanotubes, as a pore structure stabilizer, can form a uniformly distributed support structure in the material, enhance the stability of the pore structure, and avoid collapse under high temperature or mechanical pressure.
[0078] Therefore, through these specific components and their synergistic effects, the silicone foam of the present invention not only maintains excellent elasticity and flexibility, effectively protects the battery cells, but also significantly improves the performance of the material under extreme conditions. In particular, in the thermal runaway fire scenario, the material can quickly form a self-supporting foam ceramic body, greatly improving the heat insulation and flame retardancy. This foam ceramic body can maintain its structural integrity and flame retardancy when subjected to high temperature or direct flame irradiation, unlike traditional silicone foam, which may crack, deform, collapse or even pulverize under the same conditions, thereby losing its protective ability.
[0079] The preparation method of the ceramic silicone foam is as follows:
[0080] Step S1, adding vinyl silicone oil, white carbon black, nano ceramic powder and β-eucryptite into a kneader, kneading into a mass at 100-150° C., cooling, and obtaining a base rubber;
[0081] Step S2, stirring and mixing the hydroxy silicone oil and the halloysite nanotubes to obtain a foaming mixture; wherein the stirring and mixing speed is 23000-26000 r / min, and the mixing time is 10-25 s;
[0082] Step S3, adding the foaming mixture, ethynyl cyclohexanol, hydrogen-containing silicone oil, and platinum catalyst into the base rubber, mixing evenly, to obtain a rubber material;
[0083] Step S4, vulcanizing and foaming the rubber material by using a casting, calendering or molding process to obtain ceramic silicone foam.
[0084] Among them, the ceramic silicone foam prepared by the present invention has the following advantages:
[0085] 1) Excellent mechanical properties and elasticity: Due to the cross-linked structure of vinyl silicone oil and hydrogen silicone oil, plus the reinforcement effect of white carbon black, the silicone foam of the present invention has good elasticity and resistance to mechanical stress, so that it can maintain its original shape and function after long-term use or repeated compression.
[0086] 2) Highly efficient flame retardant and heat insulation capabilities: The addition of nano-ceramic powder and β-eucryptite enables the material to quickly form a protective ceramic layer when exposed to high temperature or flame. This layer of structure can not only effectively isolate the flame, but also reduce heat transfer and protect the internal structure from damage.
[0087] 3) Highly stable foam structure: The foam structure is formed by the gas generated by the decomposition of hydroxy silicone oil, and its stability is enhanced by halloysite nanotubes, so that the foam is not easy to collapse even at high temperatures and maintains a high pore structure retention rate.
[0088] 4) Excellent heat resistance: The controlled polymerization rate of ethynyl cyclohexanol and the efficient catalytic effect of platinum catalyst ensure the uniform formation and stability of the silicone rubber network structure, thereby maintaining performance in extremely high temperature environments.
[0089] In one implementation according to the present application, as shown in the attached Figure 6 As shown, the outer surface of the shell 1 is also provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell 1 to the edge of the outer surface of the shell 1 in a zigzag shape;
[0090] The third groove is provided with modified thermally conductive silicone 6, the porosity of the modified thermally conductive silicone 6 is 65% to 85%, the thickness of the modified thermally conductive silicone 6 is greater than the thickness of the low temperature resistant material layer 2 or the high temperature resistant material layer 3, and the modified thermally conductive silicone 6 protrudes from the outer surface of the shell 1.
[0091] The modified thermally conductive silicone 6 with a porosity of 65% to 85% is arranged in the third groove, which not only has good thermal conductivity but also has good energy absorption and buffering effect. In addition, when the batteries are grouped, the modified thermally conductive silicone 6 can also fix two adjacent batteries and absorb the expansion force of the batteries. Moreover, its thermal conductivity can reach 6-10W / (m·k), which can accelerate the heat conduction and dissipation of the battery pack at high temperature and reduce the temperature inside the battery pack.
[0092] The preparation method of the modified thermally conductive silica gel 6 is as follows:
[0093] 1) Boron nitride and KH570 silane coupling agent are dispersed in 100 ml of aqueous solution at a mass ratio of 10:1, and the concentrations are 40 mg / ml and 4 mg / ml respectively. The mixed dispersion is placed in a water bath ultrasound at 0°C for 40 minutes, then centrifuged to remove excess solvent, and freeze-dried to obtain modified boron nitride powder.
[0094] 2) The modified boron nitride powder and graphene were dispersed in a mixed solvent of alcohol and water in a mass ratio of 1:5, with concentrations of 1.2 mg / ml and 6 mg / ml, respectively. 2 mg / ml carbon nanotubes were added at the same time, and ultrasonic cell crusher was used for 10 min at a power of 1200 W to obtain graphene slurry.
[0095] 3) The polyurethane sponge foam was immersed in a 2 mol / L NaOH solution, treated in 40°C warm water for 3.5 h, and then placed in a 5 mg / ml anilinemethyltriethoxysilane aqueous solution and immersed for 24 h to obtain a modified polyurethane porous foam.
[0096] 4) The modified polyurethane porous foam structure was immersed in the uniform graphene slurry prepared above, and ultrasonicated in a water bath for 20 minutes at 0°C. It was dried at 60°C, and then heated from 60°C to 200°C at a heating rate of 15°C per minute, and then heated from 200°C to 380°C at a heating rate of 3°C per minute for 30 minutes, and the porous material was removed to obtain a three-dimensional porous graphene-boron nitride composite material.
[0097] 5) The three-dimensional porous graphene-boron nitride composite material obtained above was immersed in silica gel (Wacker SEMICOSIL9212), and the bubbles were removed by vacuum, and the composite material was placed in an oven at 125° C. and cured for 15 minutes to obtain the modified thermally conductive silica gel 6.
[0098] In addition, the present invention also provides a method for preparing a lithium ion battery with high and low temperature resistance, comprising the following steps:
[0099] 1) a first groove and a second groove are provided on the outer surface of the housing 1 by laser engraving, etching or stamping;
[0100] 2) preparing a low temperature resistant material layer slurry and a high temperature resistant material layer slurry respectively;
[0101] 3) applying the low temperature resistant material layer slurry to the first groove, and applying the high temperature resistant material layer slurry to the second groove;
[0102] 4) The outer surface of the shell 1 is dried, and then the battery core is encapsulated in the shell, injected with liquid, and formed to obtain the lithium-ion battery.
[0103] The preparation method sets grooves on the outer surface of the shell by laser engraving, etching or stamping, and can accurately control the size and shape of the grooves to ensure uniform coating of the material layer; the process of coating the low-temperature resistant material layer slurry and the high-temperature resistant material layer slurry can be adjusted and optimized as needed to ensure the quality and performance of the material layer; finally, through the drying and packaging process, the close combination of the material layer and the shell is ensured to improve the overall performance and reliability of the battery.
[0104] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0105] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A lithium-ion battery with high and low temperature resistance, characterized in that: include: Battery cells and shells encapsulating the battery cells; The outer surface of the shell is provided with a first groove and a second groove, and the first groove and the second groove are embedded in the outer surface of the shell side by side, and the first groove and the second groove are respectively extended from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape; The first groove is provided with a low temperature resistant material layer, and the phase change temperature of the low temperature resistant material layer is -12°C to -15°C; the second groove is provided with a high temperature resistant material layer, and the phase change temperature of the high temperature resistant material layer is 57°C to 62°C; The thickness of the low-temperature resistant material layer is the same as the depth of the first groove, and the thickness of the high-temperature resistant material layer is the same as the depth of the second groove; and the outer surfaces of the low-temperature resistant material layer, the high-temperature resistant material layer and the shell are on the same horizontal plane.
2. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The low-temperature resistant material layer comprises the following components in weight proportion: 40-50 parts of n-tridecane, 25-35 parts of n-dodecane, 10-15 parts of 2-methylpentane, 3-5 parts of polyvinyl alcohol, 2-4 parts of graphene, 1-2 parts of nano-alumina, and 0.5-1 part of silicon dioxide aerogel.
3. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The high temperature resistant material layer comprises the following components in weight proportion: 45-55 parts of octadecyl glycerol, 20-25 parts of palmitic acid, 10-15 parts of polyethylene glycol 4000, 3-5 parts of carbon nanotubes, 2-3 parts of boron nitride nanosheets, 1-2 parts of expanded graphite, and 0.5-1 parts of nano magnesium oxide.
4. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The depth of the first groove is H1, the depth of the second groove is H2, the thickness of the low-temperature resistant material layer is h1, the thickness of the high-temperature resistant material layer is h2, and the wall thickness of the shell is H; wherein H, H1, H2, h1 and h2 satisfy the relationship: h1=h2=H1=H2; 0.2H≤H1≤0.6H; 0.2H≤H2≤0.6H.
5. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The forward projection area of the low-temperature resistant material layer is S1, the forward projection area of the high-temperature resistant material layer is S2, and the forward projection area of the shell is S; wherein S1, S2 and S satisfy the relationship: 0.6S≤S1+S2≤S.
6. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The outer surface of the shell is also provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape; The third groove is provided with a buffer heat-conducting material layer; The thickness of the buffer heat-conducting material layer is greater than the thickness of the low-temperature resistant material layer or the high-temperature resistant material layer, and the buffer heat-conducting material layer protrudes from the outer surface of the shell; The buffer thermal conductive material layer includes a first foam aluminum, a second foam aluminum and a third foam aluminum, which are arranged in sequence from the outside to the inside. The density ρ1 of the first foam aluminum, the density ρ2 of the second foam aluminum and the density ρ3 of the third foam aluminum satisfy the relationship: ρ1>ρ2>ρ3; and the first foam aluminum, the second foam aluminum and the third foam aluminum are all provided with an alternating pore structure, and the porosity Q1 of the first foam aluminum, the porosity Q2 of the second foam aluminum and the porosity Q3 of the third foam aluminum satisfy the relationship: Q1<Q2<Q3.
7. The lithium-ion battery with high and low temperature resistance according to claim 6, characterized in that: The density ρ1 of the first foamed aluminum is 0.8-1.2 g / cm 3 The density of the second aluminum foam is ρ2 0.5-0.8 g / cm 3 The density of the third foam aluminum is ρ3 0.2-0.5 g / cm 3 ; The porosity Q1 of the first foam aluminum is 45% to 60%; the porosity Q2 of the second foam aluminum is 60% to 75%; and the porosity Q3 of the third foam aluminum is 75% to 90%.
8. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The outer surface of the shell is also provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape; The third groove is provided with a heat-insulating buffer material layer, the thickness of the heat-insulating buffer material layer is greater than the thickness of the low-temperature resistant material layer or the high-temperature resistant material layer, and the heat-insulating buffer material layer protrudes from the outer surface of the shell; The thermal insulation buffer material layer is ceramic silicone foam, which includes the following components in weight proportion: 30-40 parts of vinyl silicone oil, 10-20 parts of white carbon black, 20-50 parts of nano-ceramic powder, 0.1-1.0 parts of ethynyl cyclohexanol, 1-10 parts of hydrogen-containing silicone oil, 1-10 parts of hydroxy silicone oil, 0.1-1.0 parts of platinum catalyst, 10-20 parts of β-eucryptite, and 1-8 parts of halloysite nanotubes.
9. The lithium-ion battery with high and low temperature resistance according to claim 1, characterized in that: The outer surface of the shell is also provided with a third groove, the third groove is embedded side by side between the first groove and the second groove, and the third groove extends from the center of the outer surface of the shell to the edge of the outer surface of the shell in a zigzag shape; The third groove is provided with modified thermally conductive silicone, the porosity of the modified thermally conductive silicone is 65% to 85%, the thickness of the modified thermally conductive silicone is greater than the thickness of the low-temperature resistant material layer or the high-temperature resistant material layer, and the modified thermally conductive silicone protrudes from the outer surface of the shell.
10. The method for preparing a lithium-ion battery with high and low temperature resistance according to any one of claims 1 to 9, characterized in that: The following steps are involved: 1) Setting a first groove and a second groove on the outer surface of the housing by laser engraving, etching or stamping; 2) preparing a low temperature resistant material layer slurry and a high temperature resistant material layer slurry respectively; 3) applying the low temperature resistant material layer slurry to the first groove, and applying the high temperature resistant material layer slurry to the second groove; 4) Drying the outer surface of the shell, and then encapsulating the battery cell into the shell to obtain the lithium ion battery.
Citation Information
Patent Citations
Battery shell, manufacturing method and power battery
CN115020862A
Heat dissipation protection structure of lithium ion battery pack
CN118448770A
Battery shell, battery and electric equipment
CN220324564U
Secondary battery module and secondary battery pack
US20120270075A1