Lithium ion battery and preparation method thereof

By forming two CEI film layers in the lithium-ion battery and controlling the specific surface area of ​​the positive electrode active material layer and the content of sulfur-containing additives in the electrolyte, the problems of poor low-temperature discharge and high-temperature cycle performance of lithium-ion batteries are solved, and the chemical stability and lithium-ion transport capacity of the battery are improved.

CN119009172AActive Publication Date: 2024-11-22SHENZHEN HIGHPOWER TECH CO LTD

Patent Information

Application Number
CN202411096719.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have poor low-temperature discharge performance and high-temperature cycling performance during cycling, mainly due to the consumption and decomposition of electrolyte at the electrode/electrolyte interface.

Method used

In lithium-ion batteries, two CEI film layers are formed on the surface of the positive electrode. The inner layer is the first CEI film layer composed of lithium salt compounds, and the outer layer is the second CEI film layer formed with the participation of sulfur-containing additives. By controlling the specific surface area of ​​the positive electrode active material layer and the content of sulfur-containing additives in the electrolyte, the relationship 0.5≤(H×W)/A≤20 is satisfied, thus forming a dense and stable interface film.

Benefits of technology

It improves the low-temperature discharge performance and high-temperature cycle performance of lithium-ion batteries, reduces electrolyte consumption and interfacial impedance, enhances chemical and mechanical stability, and improves lithium-ion transport capability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004988643070000021
    Figure BDA0004988643070000021
  • Figure BDA0004988643070000031
    Figure BDA0004988643070000031
  • Figure BDA0004988643070000081
    Figure BDA0004988643070000081
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a lithium ion battery and a preparation method. The lithium ion battery comprises a positive plate, a diaphragm, a negative plate and an electrolyte which are arranged in the lithium ion battery, the diaphragm is arranged between the positive plate and the negative plate; the positive plate comprises a positive current collector, a positive active material layer coated on the surface of the positive current collector, and a first CEI film layer covered on the surface of the positive active material layer; the first CEI film layer comprises a lithium salt compound; a sulfur-containing additive is added into the electrolyte; wherein the thickness of the first CEI film layer is H [mu] m; the specific surface area of the positive active material layer is A m < 2 > / g; the mass percentage content of the sulfur-containing additive in the electrolyte is W%; the lithium ion battery satisfies the following relational expression: 0.5 < = (H * W) / A < = 20. The specific surface area A of the positive electrode active material, the thickness H of the artificial CEI film layer and the content W% of the sulfur-containing additive in the electrolyte are controlled to meet the following relation: (H * W) / A is more than or equal to 0.5 and less than or equal to 20, and the low-temperature discharge performance and the high-temperature cycle performance of the lithium ion battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, in particular to a lithium ion battery and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are a common type of rechargeable lithium-ion battery used in mobile devices, power tools, electric vehicles, and many other applications. They typically have high energy density, long life, and low self-discharge rates, making them ideal for many applications. Lithium-ion batteries contain a positive electrode, a negative electrode, an electrolyte, and a separator. During charging, lithium ions move from the positive electrode to the negative electrode, and vice versa during discharge. This movement of lithium ions causes electrons to flow, which creates an electric current.

[0003] The electrolyte acts as an ion transport medium for the redox reaction between the positive and negative electrodes in lithium-ion batteries, and plays an important role in the thermodynamic and kinetic performance of lithium-ion batteries. In the life cycle of lithium-ion batteries, the electrolyte is a "consumable" and will continue to be consumed and decomposed at the electrode / electrolyte interface during the cycle of lithium-ion batteries. This decomposition is exacerbated by the increase in the surface area (reaction area) of the electrode material, the operating temperature, and the instability of the electrode material, resulting in poor low-temperature discharge performance and high-temperature cycle performance of lithium-ion batteries. Summary of the invention

[0004] The embodiment of the present invention provides a lithium ion battery and a preparation method thereof, so as to solve the problem of poor low temperature discharge performance and high temperature cycle performance of the lithium ion battery during the cycle process of the lithium ion battery in the prior art.

[0005] The invention discloses a lithium ion battery, which comprises a positive electrode sheet, a diaphragm, a negative electrode sheet and an electrolyte arranged inside the lithium ion battery; the diaphragm is arranged between the positive electrode sheet and the negative electrode sheet;

[0006] The positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer coated on the surface of the positive electrode current collector, and a first CEI film layer covering the surface of the positive electrode active material layer; the first CEI film layer includes a lithium salt compound;

[0007] Sulfur-containing additives are added to the electrolyte;

[0008] The thickness of the first CEI film layer is H μm; the specific surface area of ​​the positive electrode active material layer is A m 2 / g; the mass percentage of sulfur-containing additives in the electrolyte is W%; the lithium-ion battery satisfies the following relationship:

[0009] 0.5≤(H×W) / A≤20.

[0010] Optionally, the lithium salt compound includes Li 4 SiO 4, Li 2 SiO 3 , Li 3 N、LiAlH 4 , Li 2 One or more of S.

[0011] Optionally, 10≤H≤100.

[0012] Optionally, the sulfur-containing additive is selected from at least one of the following compounds:

[0013]

[0014]

[0015] Optionally, 0.5%≤W%≤5%.

[0016] Optionally, 5≤A≤20.

[0017] Optionally, the electrolyte further includes an auxiliary additive, and the mass percentage of the auxiliary additive in the electrolyte is 1% to 6%; the auxiliary additive includes at least one of a carbonate additive, a phosphate additive, and a borate additive.

[0018] Optionally, the carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate, 3,3,3-trifluoropropylene carbonate, tetrafluoroethylene carbonate, and vinyl ethylene carbonate; and / or

[0019] The phosphate additive includes at least one of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tripropargyl phosphate, and diethyl fluorophosphate; and / or

[0020] The borate ester additive includes at least one of tris(trimethylsilyl)borate, triallyl borate, and tris(triethylsilyl)borate.

[0021] Optionally, the first CEI film layer further comprises a plasticizer.

[0022] Optionally, the positive electrode active material layer includes a positive electrode active material, a binder and a conductive agent, and the chemical formula of the positive electrode active material is LiNi x Co y Mn (1-x-y) M Z 2 , 0.5≤x≤0.9, x+y<1, 0≤z<0.08, M is one of Al, Mg, Zr and Ti.

[0023] The present invention also discloses a method for preparing the lithium ion battery, comprising the steps of:

[0024] Prepare positive electrode slurry, apply the positive electrode slurry to at least one side of the positive electrode current collector to form a positive electrode active material layer, and obtain a positive electrode sheet intermediate product through drying and cold pressing;

[0025] Preparing a first CEI film precursor slurry, depositing the first CEI film precursor slurry on the surface of the positive electrode active material layer of the positive electrode sheet intermediate product to form a first CEI film layer, and preparing a positive electrode sheet;

[0026] The positive electrode sheet, the separator, the negative electrode sheet and the electrolyte are prepared into a lithium-ion battery.

[0027] Optionally, the steps of preparing the first CEI film precursor slurry are specifically as follows:

[0028] The lithium salt compound and the plasticizer are dispersed in a solvent to obtain a first CEI film precursor slurry.

[0029] Compared with the prior art, the positive electrode sheet provided by the embodiment of the present invention has the following beneficial effects: in the lithium ion battery of the present invention, the surface of the positive electrode active material layer is covered with an artificial CEI film layer; a sulfur-containing additive is added to the electrolyte, and the thickness of the artificial CEI film layer is H μm, and the specific surface area of ​​the positive electrode active material layer is A m 2 / g, the mass percentage content W% of the sulfur-containing additive in the electrolyte satisfies the relationship 0.5≤(H×W) / A≤20. The inventors of the present invention have found that by controlling the specific surface area A of the positive electrode active material, the thickness H of the artificial CEI film layer, and the content W% of the sulfur-containing additive in the electrolyte to satisfy the following relationship: 0.5≤(H×W) / A≤20, the low-temperature discharge performance and high-temperature cycle performance of the lithium-ion battery can be improved. DETAILED DESCRIPTION

[0030] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments of the present invention can be combined with each other. The preferred embodiments of the present invention are now described in detail.

[0031] The embodiment of the present invention provides a lithium-ion battery. The lithium-ion battery includes a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte disposed therein; the separator is disposed between the positive electrode sheet and the negative electrode sheet. The positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer coated on the surface of the positive electrode current collector, and a first CEI film layer covering the surface of the positive electrode active material layer; the first CEI film layer includes a lithium salt compound. A sulfur-containing additive is added to the electrolyte;

[0032] The thickness of the first CEI film layer is H μm; the specific surface area of ​​the positive electrode active material layer is A m 2 / g; the mass percentage of sulfur-containing additives in the electrolyte is W%; the lithium-ion battery satisfies the following relationship:

[0033] 0.5≤(H×W) / A≤20.

[0034] In the lithium ion battery of the present invention, the surface of the positive electrode active material layer is covered with a first CEI film layer; a sulfur-containing additive is added to the electrolyte, and the thickness of the first CEI film layer is H μm, and the specific surface area of ​​the positive electrode active material layer is A m 2 / g, the mass percentage content W% of the sulfur-containing additive in the electrolyte satisfies the relationship 0.5≤(H×W) / A≤20. The inventors of the present invention have found that by controlling the specific surface area A of the positive electrode active material, the thickness H of the first CEI film layer, and the content W% of the sulfur-containing additive in the electrolyte to satisfy the following relationship: 0.5≤(H×W) / A≤20, the low-temperature discharge performance and high-temperature cycle performance of the lithium-ion battery can be improved.

[0035] Specifically, the inventors of the present invention have found that when the lithium-ion battery is cycled at high temperature, the positive electrode CEI film is unstable and prone to decomposition, consuming active lithium and causing capacity decay. The sulfur-containing additive in the electrolyte of the present invention can participate in film formation on the positive electrode sheet to form a second CEI film layer covering the first CEI film layer. To simplify subsequent expressions, the first CEI film layer and the second CEI film layer are collectively referred to as CEI films; the second CEI film layer formed by the sulfur-containing additive, in the two CEI film layers composed of the first CEI film layer and the second CEI film layer, the second CEI film layer is in the outer layer, has the characteristics of high temperature resistance, good chemical stability and few side reactions, and the first CEI film is in the inner layer, has the characteristics of low impedance, the first CEI film layer and the second CEI film layer complement each other, improve the rate and chemical stability of the interface film, the first CEI film formed is denser and thinner, more conducive to the transmission of lithium ions, and the formed interface film has better chemical stability and is not easy to decompose at high temperature. Compared with traditional positive electrode film-forming additives such as 1,3-propane sultone and vinyl sulfate, the film formation on the positive electrode sheet is more stable. The first CEI film layer in the present invention can improve the transmission capacity of lithium ions at the interface, thereby reducing the interfacial impedance of the lithium-ion battery. The first CEI film layer can reduce the reconstruction of the CEI film during formation and circulation (the second CEI film layer will be continuously consumed and decomposed during the battery charging and discharging process, and then re-filmed.) The lithium salt compound is the main component of the first CEI film layer, which is equivalent to a layer of material that plays a protective role on the surface of the positive electrode sheet. It has high conductivity, better chemical stability and thermal stability, which prevents the electrolyte from having more side reactions at the interface. It can build a protective layer with better chemical stability and mechanical stability at the interface, reducing the consumption of active lithium. For example, compounds such as lithium nitride have strong ion conductivity and low interfacial impedance, which is beneficial to the rate performance of lithium-ion batteries. LiAlH 4The mechanical properties and chemical stability of the compounds are strong. During the cycle of lithium-ion batteries, the protective layer is not easy to break and reorganize to consume active lithium. At the same time, by controlling the specific surface area of ​​the positive electrode active material layer, the consumption of electrolyte in the cycle of lithium-ion batteries can be controlled, thereby ensuring that the active lithium content in the lithium-ion battery system is at a reasonable level, thereby improving the low-temperature discharge and high-temperature cycle performance of lithium-ion batteries.

[0036] The larger the specific surface area of ​​the positive electrode active material layer, the more interfaces between the electrolyte and the active material, the more opportunities for reaction, and the faster the electrolyte is consumed. If the specific surface area is too low, the electrolyte and the active material will have less contact, the lithium ion transmission path will be less, the electrolyte consumption will slow down, but the rate performance will be seriously lost.

[0037] Combined with the above relationship, H is the thickness of the first CEI film. The larger H is, the more initial film formation is proved. The sulfur-containing additive with a mass percentage of W% in the electrolyte will participate in the CEI film formation. The larger W is, the better the film formation stability is proved. The larger A is, the larger the specific surface area of ​​the positive electrode active material layer is, and the more side reactions are. The former two H and W are both protections for the latter A, so the content of H×W relative to A is related to the protection of H and W for A.

[0038] In some optional embodiments, the value of (H×W) / A can be any value in the range of greater than or equal to 0.5 and less than or equal to 20, for example, it can be any value in the range of 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20.

[0039] Specifically, the lithium salt compound includes Li 4 SiO 4 , Li 2 SiO 3 , Li 3 N、LiAlH 4 , Li 2 One or more of S. Lithium nitride and other compounds have strong ion conductivity and low interface impedance, which is beneficial to the rate performance of lithium-ion batteries. 4 Such compounds have strong mechanical properties and chemical stability. During the cycle of lithium-ion batteries, the protective layer is not easy to break and reorganize to consume active lithium.

[0040] Specifically, 10≤H≤100. The specific value of the thickness H can be any value within the range of greater than or equal to 10μm and less than or equal to 100μm, for example, it can be any of 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, and 100μm. The thickness of the first CEI film layer is within this range, which can improve the transmission capacity of lithium ions at the interface, thereby reducing the interfacial impedance of the lithium-ion battery. In addition, the first CEI film layer can reduce the consumption of active lithium by CEI film reconstruction during formation and cycling. By controlling the thickness of the first CEI film layer within a certain range (10 μm ≤ H ≤ 100 μm), on the one hand, the first CEI film layer is prevented from being too thick, resulting in greater impedance and higher cost; on the other hand, the first CEI film layer is prevented from being too thin, which fails to achieve the purpose of improving the performance of the lithium-ion battery.

[0041] Furthermore, the first CEI film layer also includes a plasticizer. The plasticizer can increase the viscosity and adhesion of the first CEI film layer slurry, so that the first CEI film layer is better adhered to the positive electrode active material layer. The plasticizer can be carboxymethyl cellulose (CMC).

[0042] Specifically, the sulfur-containing additive is selected from at least one of the following compounds:

[0043]

[0044] Preferably, the sulfur-containing additive is compound 1-1 and / or compound 1-2. Compound 1-1 and compound 1-2 are more stable in nature, easier to form a film than other traditional film-forming agents, and the film-forming is more stable.

[0045] Specifically, 0.5%≤W%≤5%. The specific value of W% can be any value within the range of greater than or equal to 0.5% and less than or equal to 5%, for example, it can be any value in the range of 0.5%, 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, 1.7%, 1.9%, 2.0%, 2.3%, 2.5%, 2.7%, 2.9%, 3.0%, 3.3%, 3.5%, 3.7%, 3.9%, 4.0%, 4.3%, 4.5%, 4.7%, 5%. By controlling the mass percentage of the sulfur-containing additive in the electrolyte within this range, the stability of the positive electrode CEI film is improved, and the loss of active lithium in the positive and negative electrode materials and the electrolyte is effectively avoided, thereby improving the low temperature discharge performance and high temperature cycle performance of the lithium ion battery.

[0046] Furthermore, 5≤A≤20. The specific value of A can be greater than or equal to 5m 2 / g, less than or equal to 20m 2 / g range, for example, it can be 5m 2 / g,6m 2 / g,7m 2 / g,8m 2 / g,9m 2 / g,10m 2 / g,11m 2 / g,12m 2 / g,13m 2 / g,14m 2 / g,15m 2 / g,16m 2 / g,17m 2 / g,18m 2 / g,19m 2 / g,20m 2 / g. By controlling the specific surface area of ​​the positive electrode active material layer, the efficiency of electron conduction and ion mass transfer can be guaranteed, the side reactions of the electrolyte can be reduced, and the electrolyte consumption during the cycle of the lithium-ion battery can be controlled, thereby ensuring that the active lithium content inside the lithium-ion battery system is at a reasonable level, thereby improving the cycle performance of the lithium-ion battery. If the specific surface area of ​​the lithium-ion active material is too small (less than 5m 2 / g), the particles of lithium ion active materials are large, and both electronic conduction and ion mass transfer are limited, resulting in a decrease in kinetic performance, an increase in DCR, and a corresponding increase in voltage polarization, which further increases the degree of electrolyte side reactions and leads to a decrease in cycle performance. If the specific surface area of ​​the lithium ion active material is too large (greater than 20m 2 / g), the contact area between the electrolyte and the positive electrode increases, the degree of side reactions intensifies, the electrolyte consumption accelerates, and the active lithium content cannot be maintained at a reasonable level, which leads to a decrease in cycle performance.

[0047] Furthermore, the electrolyte also includes auxiliary additives, and the mass percentage of the auxiliary additives in the electrolyte is 1% to 6%; the auxiliary additives include at least one of carbonate additives, phosphate additives, and borate additives. The electrolyte of the present invention further adds auxiliary additives on the basis of adding sulfur-containing additives, and the auxiliary additives can further improve the cycle performance. The auxiliary additives and the sulfur-containing additives form a CEI film together, which improves the compactness of the CEI film, effectively avoids the loss of active lithium protection, and enhances the ion conductivity of the CEI film, thereby further improving the cycle performance and improving the low-temperature discharge performance. In particular, when the auxiliary additive is a phosphate additive, it can form a denser CEI film with the lithium salt compound in the first CEI film layer, inhibit the decomposition of the electrolyte solvent, slow down the consumption rate of the electrolyte, make the film thinner and more uniform, reduce the mass transfer resistance of lithium ions in the CEI film, further improve the ion conductivity of the CEI film, and at the same time have the ability to adsorb singlet oxygen on the surface of the positive electrode, thereby further improving the cycle performance and improving the low-temperature discharge performance. The mass percentage of the auxiliary additive in the electrolyte can be any value in the range of greater than or equal to 1% and less than or equal to 6%, for example, it can be any value of 1%, 1.2%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.6%, 3.8%, 4%, 4.2%, 4.5%, 4.6%, 4.8%, 5%, 5.2%, 5.5%, 5.6%, 5.8%, and 6%.

[0048] Specifically, the carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate, 3,3,3-trifluoropropylene carbonate, tetrafluoroethylene carbonate, and vinyl ethylene carbonate.

[0049] Specifically, the phosphate additive includes at least one of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, trispropargyl phosphate, and diethyl fluorophosphate.

[0050] Specifically, the borate ester additive includes at least one of tris(trimethylsilyl)borate, triallyl borate, and tris(triethylsilyl)borate.

[0051] The electrolyte also includes a solvent, and the solvent includes at least one of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, diphenyl carbonate, methyl acetate, methyl propionate, methyl butyrate, methyl acetate, ethyl acetate, propyl acetate, ethyl butyrate, propyl propionate, γ-butyrolactone, 1,3-dioxolane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether. It should be noted that the present invention does not specifically limit the preparation method of the electrolyte, and those skilled in the art can prepare it into an electrolyte according to conventional technical means, for example, the raw materials of the electrolyte are mixed evenly according to a ratio.

[0052] Furthermore, the positive electrode active material layer includes a positive electrode active material, a binder and a conductive agent, and is prepared into a positive electrode active slurry by a solvent during the preparation process. The chemical formula of the positive electrode active material is LiNixCoyMn(1-xy)MzO 2 , 0.5≤x≤0.9, x+y<1, 0≤z<0.08, M is one of Al, Mg, Zr and Ti. A positive electrode active material layer is disposed on at least one surface of the positive electrode current collector.

[0053] In the present invention, the type of positive electrode current collector is not particularly limited, and it can be any known material suitable for use as a positive electrode current collector. In one embodiment, the positive electrode current collector includes metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth and carbon paper. In one embodiment, the positive electrode current collector is a metal material.

[0054] In one embodiment, the carbon material may be one or more of natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, soft carbon, silicon, and silicon-carbon composites.

[0055] In one embodiment, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material layer is coated on the surface of the negative electrode current collector.

[0056] In the present invention, there is no particular limitation on the negative electrode current collector as long as the purpose of the present invention can be achieved. For example, it can be copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foamed nickel, foamed copper or a composite current collector.

[0057] In one embodiment, the negative electrode active material layer includes a negative electrode active material, a conductive agent, and a binder, and is prepared into a negative electrode active slurry by a solvent during the preparation process.

[0058] In one embodiment, the types of the conductive agents in the positive electrode active material layer and the negative electrode active material layer mentioned in the present invention are not limited, and any known conductive agent can be used. The conductive agent of the positive electrode active material layer can be at least one of acetylene black, carbon nanotubes, and graphene. The conductive agent of the negative electrode active material layer can be at least one of natural graphite, artificial graphite, and needle coke.

[0059] In one embodiment, the types of binders in the positive electrode active material layer and the negative electrode active material layer mentioned in the present invention are not limited, and any known binder can be used. The binder of the positive electrode active material layer can be at least one of polyethylene, polypropylene, and polyethylene terephthalate, and the binder of the negative electrode active material layer can be at least one of polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and nitrocellulose.

[0060] In the lithium-ion battery mentioned in the present invention, a separator is provided between the positive electrode and the negative electrode to prevent short circuit. There is no particular restriction on the material and shape of the separator. In one embodiment, the separator includes a porous sheet or non-woven fabric with excellent liquid retention. The material of the resin or glass fiber separator includes but is not limited to polyolefin, aromatic polyamide, polytetrafluoroethylene, polyether sulfone, etc.

[0061] The lithium-ion battery may include an outer packaging, which is used to encapsulate the above-mentioned positive electrode sheet, negative electrode sheet, separator and electrolyte. In some embodiments, the outer packaging of the lithium-ion battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as polypropylene, polybutylene terephthalate and polybutylene succinate, etc. The present invention has no particular restrictions on the shape of the lithium-ion battery, which can be cylindrical, square or other arbitrary shapes.

[0062] Furthermore, the present invention also discloses a method for preparing the above-mentioned lithium-ion battery, comprising the steps of:

[0063] Prepare positive electrode slurry, apply the positive electrode slurry to at least one side of the positive electrode current collector to form a positive electrode active material layer, and obtain a positive electrode sheet intermediate product through drying and cold pressing;

[0064] Preparing a first CEI film precursor slurry, depositing the first CEI film precursor slurry on the surface of the positive electrode active material layer of the positive electrode sheet intermediate product to form a first CEI film layer, and preparing a positive electrode sheet;

[0065] The positive electrode sheet, the separator, the negative electrode sheet and the electrolyte are prepared into a lithium-ion battery.

[0066] Specifically, the step of preparing the first CEI film precursor slurry is as follows: mixing the lithium salt compound and the plasticizer to obtain the first CEI film precursor slurry.

[0067] More specifically, the positive electrode sheet of the embodiment of the present invention comprises the following steps:

[0068] (1) A positive electrode active material, a binder and a conductive agent are mixed in a solvent to obtain a positive electrode slurry, the positive electrode slurry is coated on at least one side of a positive electrode current collector to form a positive electrode active material layer, and a positive electrode sheet intermediate product is obtained through drying and cold pressing.

[0069] (2) The lithium salt compound and the plasticizer are mixed to obtain a first CEI film precursor slurry, and the first CEI film precursor slurry is deposited on the surface of the positive electrode active material layer of the positive electrode sheet intermediate product to form a first CEI film layer, thereby obtaining a positive electrode sheet.

[0070] Among them, in step (2), the plasticizer is firstly evenly dispersed in the solvent to obtain a precursor slurry solution, and the lithium salt compound is evenly dispersed in the precursor slurry solution to obtain a first CEI film precursor slurry; then the first CEI film precursor slurry is continuously and evenly deposited on the surface of the positive electrode active material layer under non-vacuum conditions by atomic layer deposition technology, and dried to obtain a positive electrode sheet.

[0071] Specifically, in step (1), mixing the positive electrode active material, binder and conductive agent into the solvent helps to form a uniform slurry, ensures the uniform distribution of the electrode material, facilitates coating and subsequent drying processes, and improves the conductivity and mechanical stability of the electrode. Drying can remove the solvent, solidify the electrode material, and prevent solvent residues from affecting battery performance. Cold pressing can increase the density and mechanical strength of the electrode, which helps to improve the cycle stability of the battery.

[0072] In step (2), the lithium salt compound and the plasticizer are mixed, and the plasticizer can improve the flexibility and adhesion of the film and enhance the protective effect of the film. The first CEI film layer formed can enhance the transmission capacity of lithium ions at the interface, thereby reducing the interfacial impedance of the lithium-ion battery. The added lithium salt compound is the main component of the first CEI film layer, which is equivalent to a material that plays a protective role on the surface of the positive electrode sheet. It has high conductivity, better chemical stability and thermal stability, avoids more side reactions of the electrolyte at the interface, and can construct a protective layer with better chemical stability and mechanical stability at the interface, reducing the consumption of active lithium. Furthermore, the atomic layer deposition technology can achieve uniform film deposition under non-vacuum conditions, ensure the uniformity of the CEI film, and improve the overall performance and life of the battery. The first CEI film precursor slurry is deposited on the surface of the positive electrode active material layer and then dried, which can solidify the first CEI film, ensure its adhesion to the positive electrode active material layer, and improve the long-term stability of the battery.

[0073] The technical solution of the present invention is described in detail below through specific embodiments.

[0074] Example 1

[0075] The lithium ion battery of Example 1 of the present invention is prepared according to a method comprising the following steps:

[0076] (1) Preparation of electrolyte

[0077] Ethylene carbonate EC, propylene carbonate PC, and propyl propionate PP were mixed in a mass ratio of 1:1:3 to obtain a solvent. Then, based on the total mass of the electrolyte, sulfur-containing additives and auxiliary additives in the mass percentages shown in Table 1 were added and mixed, and then lithium salt LiPF was added. 6 , and mix evenly to obtain an electrolyte.

[0078] (2) Preparation of positive electrode

[0079] The positive electrode active material is lithium cobalt oxide (LiCoO 2 ), conductive carbon nanotubes CNT, and binder polyvinylidene fluoride PVDF are fully stirred and mixed in N-methylpyrrolidone NMP solvent at a mass ratio of 97:1.5:1.5 to form a uniform positive electrode slurry; the positive electrode slurry is uniformly coated on the surface of the positive electrode collector to form a positive electrode active material layer; after drying, cold pressing, slitting, welding, gluing and other processes, a positive electrode sheet intermediate is made.

[0080] 5% by mass of plasticizer CMC powder is uniformly dispersed in N-methylpyrrolidone NMP solvent to obtain precursor slurry solution I, and 95% by mass of lithium salt compound powder as shown in Table 1 is uniformly dispersed in precursor slurry solution I to obtain a first CEI film precursor slurry; the obtained first CEI film precursor slurry is continuously and uniformly deposited on the surface of the positive active material layer of the first positive electrode sheet under non-vacuum conditions by atomic layer deposition technology, and then dried to obtain a positive electrode sheet that meets the winding requirements.

[0081] (3) Preparation of negative electrode sheet

[0082] The negative electrode active material graphite, silicon, conductive agent acetylene black, adhesive styrene butadiene rubber SBR, and thickener sodium carboxymethyl cellulose CMC are mixed in a proper amount of deionized water solvent at a mass ratio of 90:6:1.2:1.5:1.3, and are fully stirred to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode collector copper foil, and the negative electrode sheet with negative electrode active material layers coated on both sides is obtained by drying and cold pressing to obtain a negative electrode sheet that meets the winding requirements.

[0083] (4) Preparation of lithium-ion batteries

[0084] Using PE porous polymer film as a separator, stack the positive electrode sheet, isolation membrane and negative electrode sheet in order, so that the isolation membrane is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wind the stacked electrode sheet and isolation membrane to obtain a bare battery cell. Place the bare battery cell in the aluminum-plastic film that has been punched and formed to complete the top and side sealing. Inject the electrolyte prepared above into the baked and dried battery cell, vacuum package, stand, and form according to the formation current and formation temperature parameters in Table 1 to complete the preparation of the lithium-ion battery.

[0085] The lithium ion batteries of Examples 2-18 and Comparative Examples 1-9 were prepared by the same preparation method as that of Example 1, and the differences are shown in Table 1. That is, the thickness of the first CEI film layer, the specific surface area of ​​the positive electrode active material, the type and amount of the sulfur-containing additive, and the type and amount of the auxiliary additive of Examples 1-18 and Comparative Examples 1-9 are shown in Table 1.

[0086] Table 1

[0087]

[0088]

[0089] Lithium-ion battery performance test: 45°C cycle test:

[0090] The test method is: in a 45±2℃ constant temperature box, charge the lithium-ion battery to 4.5V at 1C constant current and constant voltage, cut off the current at 0.05C, and then discharge it to 3V at 1C. Perform multiple charge and discharge cycles under the above conditions, and calculate the capacity retention rate of the lithium-ion battery after 600 cycles, with 5 lithium-ion batteries in each group.

[0091] Capacity retention rate (%) = discharge capacity corresponding to the number of cycles (mAh) / discharge capacity of the third cycle (mAh) * 100%

[0092] The average value of the capacity retention rate of each group of 5 lithium-ion batteries after different cycles is recorded in Table 1 above.

[0093] -30℃-0.2C rate discharge test:

[0094] The test method is: in a 25±2℃ constant temperature box, charge the lithium-ion battery to 4.5V at 1C constant current and constant voltage, cut off the current at 0.05C, and then discharge it to 3V at 0.2C, and record the discharge capacity R1; then place the battery cell in a -30±2℃ constant temperature box, charge the lithium-ion battery to 4.5V at 1C constant current and constant voltage, cut off the current at 0.05C, and then discharge it to 3V at 0.2C, and record the discharge capacity R2.

[0095] -30℃-0.2C rate discharge capacity retention rate (%) = R2 / R1*100%

[0096] The average value of each group of 5 lithium-ion batteries is recorded in Table 1 above.

[0097] The data from Comparative Example 2 and Comparative Example 1 show that adding the sulfur-containing additive alone in Comparative Example 2 can improve the low-temperature discharge performance and high-temperature cycle performance of the lithium-ion battery. This is because the sulfur-containing additive can form a denser, thinner, and more chemically stable CEI film at the positive electrode.

[0098] The data of Comparative Example 3 and Comparative Example 1 show that when the content of sulfur-containing additive added alone in Comparative Example 3 is too high, the low-temperature discharge performance and high-temperature cycle performance deteriorate. This is because excessive sulfur-containing additives can cause the interface impedance to rise sharply, deteriorating the performance of the lithium-ion battery.

[0099] The data from Examples 1 to 3 show that when the content of the sulfur-containing additive gradually increases between 0.5% and 5%, the low-temperature discharge performance and high-temperature cycle performance are improved. This is because the sulfur-containing additive can form a denser, thinner, and more chemically stable CEI film at the positive electrode.

[0100] The data from Examples 4 to 7 show that when the specific surface area of ​​the positive electrode active material layer is 5 m 2 / g-20m 2 When the γ / g range increases, the low-temperature discharge performance and high-temperature cycle performance are improved. This is because the contact area between the electrolyte and the active material increases, which is beneficial to the transmission of lithium ions.

[0101] The data of Comparative Examples 4 to 5 show that if the specific surface area of ​​the positive electrode active material layer is too small (less than 5), the lithium ion active material particles are large, and both electronic conduction and ion mass transfer are limited, resulting in decreased kinetic performance, increased DCR, and correspondingly aggravated voltage polarization, which further causes the electrolyte side reaction degree to increase, thereby resulting in decreased cycle performance. If the specific surface area of ​​the positive electrode active material layer is too large (greater than 20), the electrolyte and the positive electrode contact surface increase, the side reaction degree intensifies, the electrolyte consumption accelerates, and the active lithium content cannot be maintained at a reasonable level, thereby resulting in decreased cycle performance. When the specific surface area A of the positive electrode active material layer is 5≤A≤20, by controlling the specific surface area of ​​the active material, the efficiency of electronic conduction and ion mass transfer can be guaranteed, the side reaction of the electrolyte can be reduced, and the electrolyte consumption of the lithium ion battery during the cycle can be controlled, thereby ensuring that the active lithium content inside the lithium ion battery system is at a reasonable level, thereby improving the cycle performance and low temperature discharge performance of the lithium ion battery.

[0102] The data from Comparative Examples 1 and 6-7 show that when the thickness of the first CEI film layer is too small or too large, the 45°C cycle capacity retention rate is poor, and the first CEI film layer is slightly better when the thickness is 10 μm;

[0103] The data from Examples 4, 8 to 10 show that when the thickness of the first CEI film layer increases within the range of 10-100 μm, the low-temperature discharge and high-temperature cycle performances are improved. The increase in the first CEI film layer helps to improve the transmission of lithium ions in the electrolyte and reduce the consumption of lithium sources due to reconstruction of the interface film, thereby improving the performance of lithium-ion batteries.

[0104] The data from Examples 4 and 13 to 15 show that when the sulfur-containing additives are other types involved in the present invention, the improvement effect is consistent. The data from Examples 4 and 16 show that when the first CEI membrane component is other lithium-containing compounds, the improvement effect is consistent. The data from Examples 11 to 12 and Example 4 show that the present invention can further improve the cycle performance by adding auxiliary additives on the basis of adding sulfur-containing additives, among which the phosphate additives can form a film on the positive electrode surface, inhibit the decomposition of the electrolyte solvent, slow down the consumption rate of the electrolyte, make the film thinner and more uniform, reduce the mass transfer resistance of lithium ions in the CEI membrane, and have the ability to adsorb singlet oxygen on the positive electrode surface.

[0105] The data from Examples 11 and 17 to 19 show that when the content of the auxiliary additive increases within the range of 1% to 6%, the low-temperature discharge and high-temperature cycle performances are improved.

[0106] As can be seen from Table 1, the present invention can significantly improve the low-temperature discharge performance and high-temperature cycle performance of sodium-ion lithium-ion batteries by controlling the specific surface area of ​​the positive electrode active material and the mass percentage of the sulfur-containing additive in the electrolyte to satisfy the following relationship: 0.5≤(H×W) / A≤20, 0.5%≤W%≤5%, 10≤H≤100, 5≤A≤20.

[0107] It should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. For those skilled in the art, the technical solutions described in the above embodiments can be modified, or some of the technical features therein can be replaced by equivalents; and all these modifications and replacements should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a diaphragm, a negative electrode sheet and an electrolyte arranged inside the battery; the diaphragm is arranged between the positive electrode sheet and the negative electrode sheet; The positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer coated on the surface of the positive electrode current collector, and a first CEI film layer covering the surface of the positive electrode active material layer; the first CEI film layer includes a lithium salt compound; The electrolyte is added with a sulfur-containing additive; The thickness of the first CEI film layer is H μm; the specific surface area of ​​the positive electrode active material layer is Am 2 / g; the mass percentage of the sulfur-containing additive in the electrolyte is W%; the lithium-ion battery satisfies the following relationship: 0.5≤(H×W) / A≤20.

2. The lithium-ion battery according to claim 1, characterized in that The lithium salt compound includes one or more of Li4SiO4, Li2SiO3, Li3N, LiAlH4, and Li2S.

3. The lithium-ion battery according to claim 1, characterized in that 10≤H≤100。 4. The lithium ion battery according to any one of claims 1 to 3, characterized in that: The sulfur-containing additive is selected from at least one of the following compounds:

5. The lithium ion battery according to any one of claims 1 to 3, characterized in that: 0.5%≤W%≤5%。 6. The lithium ion battery according to any one of claims 1 to 3, characterized in that: 5≤A≤20。 7. The lithium ion battery according to any one of claims 1 to 3, characterized in that: The electrolyte further includes an auxiliary additive, the mass percentage of the auxiliary additive in the electrolyte is 1% to 6%; the auxiliary additive includes at least one of a carbonate additive, a phosphate additive, and a borate additive.

8. The lithium-ion battery according to claim 7, characterized in that: The carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate, 3,3,3-trifluoropropylene carbonate, tetrafluoroethylene carbonate, and vinyl ethylene carbonate; and / or The phosphate additive includes at least one of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tripropargyl phosphate, and diethyl fluorophosphate; and / or The borate ester additive includes at least one of tris(trimethylsilyl)borate, triallyl borate, and tris(triethylsilyl)borate.

9. The lithium ion battery according to any one of claims 1 to 3, characterized in that: The first CEI film layer also includes a plasticizer.

10. The lithium ion battery according to any one of claims 1 to 3, characterized in that: The positive electrode active material layer includes a positive electrode active material, a binder and a conductive agent, and the chemical formula of the positive electrode active material is LiNi x Co y Mn (1-x-y) MzO2, 0.5≤x≤0.9, x+y<1, 0≤z<0.08, M is one of Al, Mg, Zr and Ti.

11. The method for preparing a lithium ion battery according to any one of claims 1 to 10, characterized in that: Includes steps: Prepare positive electrode slurry, apply the positive electrode slurry to at least one side of the positive electrode current collector to form a positive electrode active material layer, and obtain a positive electrode sheet intermediate product through drying and cold pressing; Preparing a first CEI film precursor slurry, depositing the first CEI film precursor slurry on the surface of the positive electrode active material layer of the positive electrode sheet intermediate product to form a first CEI film layer, and preparing a positive electrode sheet; The positive electrode sheet, the separator, the negative electrode sheet and the electrolyte are prepared into a lithium-ion battery.

12. The method for preparing a lithium ion battery according to claim 11, characterized in that: The steps of preparing the first CEI film precursor slurry are specifically as follows: The lithium salt compound and the plasticizer are dispersed in a solvent to obtain a first CEI film precursor slurry.

Citation Information

Patent Citations

  • Secondary battery and device

    CN116435600A

  • Lithium ion battery

    CN117096440A

  • Lithium ion battery and manufacturing method thereof

    CN118016972A

  • Lithium-ion battery

    WO2024037187A1

Cited By

  • Lithium ion battery

    CN119400963A

  • Battery and electronic equipment

    CN119742421A

  • Battery cell, electrolyte, battery device, and electric device

    CN120127224A

  • Positive electrode sheet, battery and preparation method therefor, battery pack, and electric device

    WO2026153326A1

  • Lithium-ion battery

    WO2026170819A1