Composite frame sprayed with conductive paint
By using conductive paint sprayed composite frames in offshore photovoltaic systems, combined with the mixing technology of metal powder, resin and glass fiber, the problems of frame corrosion and electrical grounding in the marine environment are solved, and the conductive performance with high stability and safety is achieved , extends the service life of photovoltaic modules.
Patent Information
- Application Number
- CN202411089169.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
In offshore photovoltaic systems, commonly used aluminum frames and steel frames are prone to corrosion in the marine environment and are difficult to operate for a long time. At the same time, composite frames as insulators cannot meet the grounding needs of the electrical system, which poses electrical safety risks.
The composite frame preparation method is made using conductive paint spray. By mixing metal powder, resin and glass fiber in a specific proportion, forming an integrated composite material structure, and spraying conductive paint on the surface of the frame to ensure that the frame has conductive properties and mechanical strength and meets the electrical capacity. Grounding requirements.
It achieves good conductivity and corrosion resistance of composite frames, extends the service life of photovoltaic modules, meets international electrical safety standards, and provides an effective solution for offshore photovoltaic systems.
Smart Images

Figure CN119010762A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic assembly preparation, and in particular to a composite frame sprayed with conductive paint. Background Art
[0002] Offshore photovoltaic systems refer to solar photovoltaic systems that install photovoltaic modules on ocean waters for power generation. With the reduction of available land space and the increase in demand for renewable energy, offshore photovoltaics have gradually become an important energy solution. Offshore photovoltaics can effectively utilize the vast water space of the ocean, reduce the occupation of land resources, and use the natural cooling effect of seawater to improve the efficiency and life of photovoltaic modules. In addition, offshore photovoltaics do not compete with agricultural, residential and other land uses, which helps to protect the terrestrial ecological environment. However, the high salinity and humidity in the marine environment have serious corrosive effects on photovoltaic modules. For example, commonly used aluminum frames and steel frames are easily corroded in seawater environments and are difficult to operate for a long time in the marine environment. Therefore, after research, it was found that composite frames prepared with resins and glass fibers have excellent corrosion resistance and can remain stable for a long time in the marine environment. The composite frames are relatively lightweight, which helps to reduce installation costs and complexity. However, the composite frames are essentially insulators and cannot meet the grounding requirements of the electrical system (according to international electrical safety standards, all electrical products must be grounded to prevent electrical failures and lightning strikes. The risk of electric shock and fire). Summary of the invention
[0003] The purpose of the present invention is to provide a composite frame sprayed with conductive paint to solve the problems existing in the above-mentioned prior art.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] One of the technical solutions of the present invention: a method for preparing a composite frame sprayed with conductive paint, comprising the following steps:
[0006] The frame is prepared from metal powder, resin and glass fiber;
[0007] Conductive paint is sprayed on the surface of the frame to obtain the composite frame.
[0008] Furthermore, the mass percentages of the metal powder, resin and glass fiber are 5-10%: 15-35%: 65-85%, which is 100% in total.
[0009] Furthermore, the particle size of the metal powder is 1 to 10 microns; the resin includes polyurethane or epoxy acrylate; the diameter of the glass fiber is 20 microns, and the length is the same as the length of the composite frame;
[0010] The metal powder is a metal powder with good electrical conductivity.
[0011] Furthermore, the metal powder includes copper powder or nickel powder.
[0012] The metal powder, resin and glass fiber used in the present invention have good compatibility and uniform dispersibility.
[0013] Furthermore, the method for preparing the frame comprises the following steps:
[0014] The metal powder is uniformly mixed into the resin, and then glass fiber is added and mixed uniformly, and then molded and cured to obtain the frame.
[0015] Mixing metal powder with resin and glass fiber can form an integrated composite material structure, which not only maintains the mechanical strength of the material but also provides conductive properties (the metal powder evenly distributed inside the frame forms a continuous conductive network inside the frame, giving the entire frame consistent conductive properties).
[0016] The metal powder forms a continuous conductive network inside the frame, giving the entire frame consistent conductivity. When current passes through the photovoltaic module, the conductive network of the metal powder can effectively conduct the current, ensuring the stability and reliability of the electrical connection.
[0017] Furthermore, when preparing the frame, the shear speed of the mixed raw materials is 3000-5000 rpm, the mixing time is 15-30 minutes, and the temperature during mixing is 20-25°C.
[0018] Furthermore, the mold used for the compression molding needs to be preheated to 120-150° C., the temperature of the compression molding is 120-150° C., the pressure is 20-50 MPa, and the time is 30-60 min.
[0019] Compression molding under these conditions ensures that the metal powder is evenly distributed in the material.
[0020] Furthermore, the curing method specifically includes: first heating to 60-80° C., curing for 2-4 hours, and then heating to 100-120° C., curing for 1-2 hours.
[0021] Curing under these conditions ensures the mechanical strength and stability of the material.
[0022] The frame containing metal powder prepared by the present invention has consistent conductive properties, which can ensure the reliability of electrical connection; the metal powder is evenly distributed inside the frame, which avoids the problem of loss of conductive properties after the surface coating is worn (after the surface coating is worn, a complete circuit cannot be formed. At this time, due to the metal powder inside the frame, the frame still has conductive properties), and has a longer service life. The metal powder is combined with other materials in the frame to improve the mechanical strength of the material and increase the overall durability of the frame; during the production process, the metal powder can be directly mixed with other materials for integrated molding preparation, which reduces subsequent processing steps and improves production efficiency. Even in harsh marine environments, the corrosion resistance of the frame is still excellent, and the addition of metal powder (such as nickel powder or copper powder) can also minimize corrosion problems.
[0023] Further, the conductive component in the conductive paint includes particles of conductive material;
[0024] The conductive material includes copper, copper alloy, silver or aluminum;
[0025] The particle size of the microparticles is 1 to 10 microns.
[0026] Furthermore, the copper alloy includes the following components in percentage by mass: 60-70% copper, 10-20% chromium, and 10-20% zirconium.
[0027] Furthermore, the conductive material accounts for 20-50 wt % in the conductive paint.
[0028] Furthermore, the spraying thickness of the conductive paint is 20 microns, which can ensure the conductive performance and mechanical strength.
[0029] Conductive paint sprayed on the surface of the frame can form a continuous conductive path, giving the frame good conductive properties. When current passes through the conductive part of the photovoltaic module, the particles of these conductive materials can effectively conduct current, ensuring the stability and reliability of the electrical connection.
[0030] Conductive paint containing copper has good conductivity and economy, and is suitable for large-scale applications.
[0031] Conductive paint can be covered on the surface of the frame by spraying. The process is relatively simple and can be directly implemented on the existing frame production line without large-scale transformation of the production equipment. It can be sprayed on frames of different shapes and sizes and has strong adaptability. The cost of using conductive paint materials is relatively low, and the spraying process is mature, easy to control and implement. If the conductive coating is damaged, it can be repaired by spraying again, and the maintenance cost is low.
[0032] The second technical solution of the present invention: a composite frame prepared by the above-mentioned preparation method.
[0033] The third technical solution of the present invention: an application of the above-mentioned composite frame in the photovoltaic field.
[0034] The composite frame of the present invention has the following advantages:
[0035] (1) Improve electrical conductivity: The frame of the photovoltaic module needs to have good electrical conductivity to ensure efficient conduction of current. Adding conductive components (such as silver, copper, copper alloy or aluminum) to conductive paint can significantly improve electrical conductivity, reduce resistance loss, and improve the overall efficiency of the photovoltaic module.
[0036] (2) Enhanced corrosion resistance: Photovoltaic modules are usually exposed to outdoor environments and face erosion by rain, moisture and various corrosive gases. The addition of conductive components can enhance the corrosion resistance of conductive paint and protect the frame from corrosion, thereby extending the service life of photovoltaic modules.
[0037] (3) Improve mechanical strength and wear resistance: The frame of the photovoltaic module needs to have a certain mechanical strength and wear resistance to cope with the physical wear during installation and maintenance. The addition of conductive components can improve the hardness and wear resistance of the conductive paint, making the frame stronger and more durable.
[0038] (4) Improved anti-oxidation performance: The conductive components (especially silver and aluminum) have good anti-oxidation properties, which can effectively prevent the frame from oxidizing during use and maintain the stability of its conductive properties.
[0039] (5) Optimizing the thermal management of photovoltaic modules: The conductive component has a higher thermal conductivity, which can help the conductive paint dissipate heat more effectively, reduce the impact of heat accumulation on the performance of photovoltaic modules, and thus improve the working efficiency and reliability of photovoltaic modules.
[0040] (6) Weight reduction: Compared with traditional metal frames, composite frames can significantly reduce weight while ensuring performance, which helps in the transportation and installation of photovoltaic modules while reducing costs.
[0041] (7) Improve electromagnetic shielding capability: In photovoltaic systems, electromagnetic interference may affect power transmission and conversion efficiency. Conductive paint plus conductive components can provide effective electromagnetic shielding and reduce the impact of electromagnetic interference on the system.
[0042] The present invention discloses the following technical effects:
[0043] The method of combining conductive paint spraying with adding metal powder of the present invention provides the composite frame with more excellent conductivity and corrosion resistance, can meet international electrical safety standards (grounding requirements of photovoltaic systems), has high stability, safety and durability, greatly extends the service life of photovoltaic modules, provides an effective solution for offshore photovoltaic systems, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 This is a schematic diagram of the structure of the mold used in Example 1;
[0046] Figure 2 This is a schematic diagram of the structure of the small sample. DETAILED DESCRIPTION
[0047] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0048] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0050] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0051] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0052] The particle size of the metal powder used in the present invention is 1 to 10 microns; the diameter of the glass fiber is 20 microns, and the length is the same as that of the composite frame.
[0053] The conductive component in the conductive paint used in the present invention includes particles of conductive material; the conductive material includes copper, copper alloy, silver or aluminum; and the particle size of the particles is 1 to 10 microns.
[0054] The conductive paint used in the present invention is a commercially available conductive paint, which contains particles of conductive material, and the proportion of the conductive material particles in the conductive paint is 20-50wt%.
[0055] Example 1
[0056] A method for preparing a composite frame sprayed with conductive paint:
[0057] (1) High shear mixing: 5 parts by mass of metal powder (copper powder) was mixed into 15 parts by mass of resin (polyurethane), and then 80 parts by mass of glass fiber were added, and mixed evenly using a high shear mixing equipment (shear speed of 4000 rpm, mixing time of 25 min, and temperature maintained at 25° C.) to obtain a mixture.
[0058] (2) Compression molding: The mixed material is evenly spread in a mold preheated to 130°C (mold dimensions: width of the A-level surface is 11 mm, width of the B-level surface is 30 mm, width of the C-level surface is 20.8 mm, width of the D-level surface is 18 mm, cavity width is 11.7 mm, cavity height is 15.3 mm, overflow groove width is 6.1 mm, wall thickness is 2.5 mm), and a pressure of 40 MPa is applied to the inner cavity for 40 minutes of compression molding. The temperature during compression molding is controlled at 135°C to obtain a molded frame. See the schematic diagram of the mold structure. Figure 1 .
[0059] (3) Curing treatment: The formed frame is taken out of the mold and placed in a curing furnace. The curing temperature is first set at 70°C for 3 hours, and then the temperature of the curing furnace is increased to 120°C and the curing treatment is performed for 2 hours to obtain the frame.
[0060] (4) Surface treatment: Clean the surface of the frame and make sure it is free of oil and dust to ensure the adhesion of the conductive paint.
[0061] (5) Spraying conductive paint: Use high-precision spraying equipment to evenly spray conductive paint on the surface of the frame, covering the entire surface of the frame, with a spray thickness of 20 microns.
[0062] The conductive material contained in the conductive paint is copper particles with a particle size of 1 to 10 microns, and the copper particles account for 35wt% of the conductive paint.
[0063] (6) Drying and curing: After the conductive paint is sprayed, it is dried (temperature is 120-150°C, 3 min / m) and cured (so that the conductive paint is firmly attached to the surface of the frame) by drying equipment to obtain a composite frame.
[0064] (7) Application and installation
[0065] Ground connection: Reserve ground connection points in the composite frame design and ensure that these connection points are well connected to the conductive coating or internal metal powder network. Through these connection points, the ground wire is reliably connected to the composite frame to ensure that the current can be effectively guided to the ground.
[0066] Electrical safety: Ensure that the installed PV panels comply with international electrical safety standards (IEC61730) and can effectively conduct current in the event of electrical faults or lightning strikes, ensuring the electrical safety and reliability of the system.
[0067] System debugging and verification: After the installation is completed, the entire offshore photovoltaic system is fully debugged and verified to ensure that the conductivity and grounding effect of each component meet the design standards.
[0068] (8) Maintenance and repair: If the conductive coating is damaged during use, it can be repaired by re-spraying to ensure the conductive performance during long-term use.
[0069] Effect Example 1
[0070] 1. Conductive performance test
[0071] (1) Resistance measurement:
[0072] Method: Use a resistance measuring instrument to measure the resistance of the sample to ensure that its conductive performance meets the design requirements.
[0073] Standard: According to the international electrical safety standard (IEC61730), measure the resistance value, record the measurement results, and compare them with the standard requirements to ensure compliance with the specifications.
[0074] (2) Corrosion resistance test:
[0075] Method: Carry out corrosion resistance tests on samples, such as salt spray tests, to simulate the corrosion conditions in the marine environment and verify the corrosion resistance of the samples.
[0076] Objective: To observe the test results and ensure that the samples (such as frames) with added metal (metal powder, conductive material) still maintain excellent corrosion resistance and that the conductivity of the metal is not affected by corrosion and does not affect its long-term use in the offshore environment.
[0077] 2. Experimental process:
[0078] (1) Sample preparation: Prepare several processed small samples (cut from the already prepared conductive composite frame; the size is generally 300mm×20mm×10mm, see the structural diagram Figure 2 );
[0079] (2) Experimental equipment: volume resistivity tester, TC environmental chamber, HF environmental chamber, DH environmental chamber, salt spray tester, three-point bending tester, tensile tester, impact tester, compression tester;
[0080] (3) Volume resistivity test experimental steps:
[0081] Electrode arrangement: Apply conductive silver paint to both ends of the sample to form two electrodes. The area of the electrodes should be consistent to ensure the accuracy of the test. The distance between the electrodes (the effective length of the sample) should be accurately measured.
[0082] Connect the test circuit: Connect the sample to the precision resistance tester, using the four-terminal method to eliminate the influence of contact resistance. The test circuit includes power supply, standard resistor and sample resistor.
[0083] Measuring Voltage and Current: A known constant current is applied through the electrodes and the voltage drop across the sample is measured. The current and voltage drop data are recorded to calculate the volume resistivity.
[0084] (4) Environmental test (three small samples are used for each type of environmental test):
[0085] 1.TC200 (thermal cycle test):
[0086] ① The sample temperature in the aging box cycles between -40±2℃ and 85±2℃, and the temperature change rate does not exceed 100℃ / h. At each extreme temperature, it should remain stable for at least 10 minutes, and one cycle should not exceed 6 hours.
[0087] ② After the test is completed, there is at least 1 hour of recovery time to test performance.
[0088] 2.DH1000 (high temperature and high humidity test):
[0089] ① Test for 1000h at temperature 85±2℃ and relative humidity 85±5%.
[0090] ② After the test is completed, there is at least 2 to 4 hours of recovery time to test performance.
[0091] 3. HF10 (humidity-freeze cycle test):
[0092] ① The sample temperature in the aging box cycles between -40±2℃ and 85±2℃, maintaining at 85℃ for at least 20h, at 85℃ for a maximum of 4h, and at -40℃ for at least 0.5h, for 10 cycles.
[0093] ② At all temperatures above room temperature, maintain relative humidity within 85%±5%; there is no relative humidity control requirement for temperatures below room temperature.
[0094] ③The temperature change rate above 0℃ shall not exceed 100℃ / h, and the temperature change rate below 0℃ shall not exceed 200℃ / h.
[0095] ④ After the test is completed, there is at least 2 to 4 hours of recovery time to test performance.
[0096] 4. Salt spray corrosion test:
[0097] ①Salt spray: salt spray concentration 5±1%, test temperature 15~35℃, spray volume 1~2mL / h / 80cm 2 , pH value 6.5~7.2 at 35±2℃; relative humidity>85%RH.
[0098] ② Sample position: The inclination angle of the upper surface of the component to the vertical direction is 15 to 30°.
[0099] ③Test cycle: The national standard is 96h.
[0100] After the environmental test is completed, its mechanical strength and volume resistivity are tested.
[0101] Table 1 Performance comparison before and after environmental testing
[0102]
[0103] Comparative Example 1
[0104] The same as Example 1, except that the amount of metal powder in the mixture is 15 parts by mass, the amount of resin is 15 parts by mass, and the amount of glass fiber is 70 parts by mass; no conductive paint is sprayed. The specific preparation method is as follows:
[0105] (1) High shear mixing: 15 parts by mass of metal powder (copper powder) was mixed into 15 parts by mass of resin (polyurethane), and then 70 parts by mass of glass fiber was added, and mixed evenly using a high shear mixing equipment (shear speed of 4000 rpm, mixing time of 25 min, and temperature maintained at 25° C.) to obtain a mixture.
[0106] (2) Compression molding: The mixed material is evenly spread in a mold preheated to 130°C (mold dimensions: width of the A-level surface is 11 mm, width of the B-level surface is 30 mm, width of the C-level surface is 20.8 mm, width of the D-level surface is 18 mm, cavity width is 11.7 mm, cavity height is 15.3 mm, overflow groove width is 6.1 mm, wall thickness is 2.5 mm), and a pressure of 40 MPa is applied in the inner cavity for 40 minutes of compression molding. The temperature is controlled at 135°C during compression molding to obtain a molded frame.
[0107] (3) Curing treatment: The molded frame is taken out of the mold and placed in a curing furnace. The curing temperature is first set at 70°C for 3 hours, and then the temperature of the curing furnace is increased to 120°C and the curing treatment is performed for 2 hours to obtain a composite frame.
[0108] The performance of the composite frame prepared in this comparative example was measured using the same method as in Example 1. The results are shown in Table 2.
[0109] Table 2 Performance comparison before and after environmental testing
[0110]
[0111]
[0112] Comparative Example 2
[0113] The same as Example 1, the only difference is that the spraying thickness of the conductive paint is 30 microns, and no metal powder is added to the mixture. The specific preparation method is as follows:
[0114] (1) High shear mixing: 85 parts by mass of glass fiber were added to 15 parts by mass of resin (polyurethane), and mixed evenly using a high shear mixer (shear speed of 4000 rpm, mixing time of 25 min, and temperature maintained at 25° C.) to obtain a mixture.
[0115] (2) Compression molding: The mixed material is evenly spread in a mold preheated to 130°C (mold dimensions: width of the A-level surface is 11 mm, width of the B-level surface is 30 mm, width of the C-level surface is 20.8 mm, width of the D-level surface is 18 mm, cavity width is 11.7 mm, cavity height is 15.3 mm, overflow groove width is 6.1 mm, wall thickness is 2.5 mm), and a pressure of 40 MPa is applied in the inner cavity for 40 minutes of compression molding. The temperature is controlled at 135°C during compression molding to obtain a molded frame.
[0116] (3) Curing treatment: The formed frame is taken out of the mold and placed in a curing furnace. The curing temperature is first set at 70°C for 3 hours, and then the temperature of the curing furnace is increased to 120°C and the curing treatment is performed for 2 hours to obtain the frame.
[0117] (4) Surface treatment: Clean the surface of the frame and make sure it is free of oil and dust to ensure the adhesion of the conductive paint.
[0118] (5) Spraying conductive paint: Use high-precision spraying equipment to evenly spray conductive paint on the surface of the frame, covering the entire surface of the frame, with a spraying thickness of 30 microns.
[0119] The conductive material contained in the conductive paint is copper particles with a particle size of 1 to 10 microns, and the copper particles account for 35wt% of the conductive paint.
[0120] (6) Drying and curing: After the conductive paint is sprayed, it is dried (temperature is 120-150°C, 3 min / m) and cured (so that the conductive paint is firmly attached to the surface of the frame) by drying equipment to obtain a composite frame.
[0121] The performance of the composite frame prepared in this comparative example was measured using the same method as in Example 1. The results are shown in Table 3.
[0122] Table 3 Performance comparison before and after environmental testing
[0123]
[0124] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a composite frame sprayed with conductive paint, characterized in that: The following steps are involved: The frame is prepared from metal powder, resin and glass fiber; Conductive paint is sprayed on the surface of the frame to obtain the composite frame.
2. The preparation method according to claim 1, characterized in that: The mass percentages of the metal powder, resin and glass fiber are 5-10%: 15-35%: 65-85%, which is 100% in total.
3. The preparation method according to claim 1, characterized in that: The particle size of the metal powder is 1 to 10 microns; the resin includes polyurethane or epoxy acrylate; the diameter of the glass fiber is 20 microns, and the length is the same as that of the composite frame.
4. The preparation method according to claim 1, characterized in that: The metal powder includes copper powder or nickel powder.
5. The preparation method according to claim 1, characterized in that: The method for preparing the frame comprises the following steps: The metal powder is uniformly mixed into the resin, and then glass fiber is added and mixed uniformly, and then molded and cured to obtain the frame.
6. The preparation method according to claim 1, characterized in that: The conductive component in the conductive paint includes particles of conductive material; The conductive material includes copper, copper alloy, silver or aluminum; The particle size of the microparticles is 1 to 10 microns.
7. The preparation method according to claim 6, characterized in that: The conductive material accounts for 20 to 50 wt.% in the conductive paint.
8. The preparation method according to claim 1, characterized in that: The spraying thickness of the conductive paint is 20 microns.
9. A composite frame prepared by the preparation method according to any one of claims 1 to 8.
10. Application of the composite frame according to claim 9 in the photovoltaic field.