Method for producing airbag module or safety belt for safety system in vehicle

Through thermoplastic polymer melt spinning technology, airbags and seat belts for vehicle safety systems are prepared using recycling and bio-based materials, which solves the greenhouse gas emission problems caused by plastic materials in the prior art, and achieves sustainable production and performance considerations Effect.

CN119013166APending Publication Date: 2024-11-22ZF AUTOMOTIVE GERMANY GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033491.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Plastic materials in existing vehicle safety systems lead to greenhouse gas emissions, affecting global climate warming, and bio-based plastics and recycled plastics have not been promoted in safety devices, making it difficult to meet the reliability requirements of components.

Method used

Multi-monofilament yarns are prepared by melt spinning using thermoplastic polymers, braided into airbags and seat belts, and utilize recycled and renewable raw materials, combined with bio-based materials to form sustainable fabric-based components and be compared with traditional petroleum-based materials. In combination, a safety system with a low carbon footprint was prepared.

Benefits of technology

It realizes sustainable production of vehicle safety systems, reduces greenhouse gas emissions, maintains the performance characteristics of safety devices, reduces dependence on fossil materials, and saves resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a method for manufacturing an airbag module of a safety system in a vehicle, where the airbag module comprises a module housing, an airbag disposed in the module housing and a gas generator connected to the module housing, where the method comprises the following steps: providing a multifilament yarn by melt spinning; weaving the multi-monofilament yarn into a fabric, and selectively finishing the fabric; cutting the fabric into wall portions of an airbag and sewing the wall portions to form an airbag having a gas inlet; the airbag module is formed by introducing the airbag having the gas inlet into the module housing and coupling the gas inlet to the gas generator, in which the multi-monofilament yarn is formed from at least a thermoplastic polymer, the thermoplastic polymer is partially or completely prepared using recycled or renewable raw materials. The invention also relates to a method for manufacturing the safety belt.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for manufacturing an airbag module or a seat belt of a safety system in a vehicle.

[0002] Airbag modules are elements of safety systems that are currently commonly provided in vehicles, with which vehicle occupants or third parties are to be protected from injury in a wide variety of accidents. This is accomplished in that a suitable triggering sensor device activates a gas generator when necessary, which provides pressurized gas that is introduced into the airbag. The airbag is deployed from its folded rest position in order, for example, to provide a restraining effect for a vehicle occupant.

[0003] Seat belt tensioner modules that contain gas generators or other actuators operate in a similar manner, which are activated in the event of an accident and act on the seat belt to remove the so-called slack in the seat belt. This ensures that the seat belt is held against the body of the vehicle occupant in the event of a vehicle accident and that the vehicle occupant participates in vehicle deceleration as early as possible.

[0004] A wide range of plastics are used to produce safety systems. However, the plastics used so far are based on petroleum and some of them lead to significant greenhouse gas emissions along their value-added chain. The CO2 released through the value-added chain intensifies the greenhouse effect, which is responsible for global warming. Such greenhouse gas emissions are quantified by the product carbon footprint (PCF) obtained and defined via the standards DIN EN ISO 14067 and DIN EN ISO 14064-3. The product carbon footprint (PCF) represents the greenhouse gas emissions generated during the production of a product through its use until it is discarded. The aim is therefore to improve environmentally friendly plastic handling and reduce the PCF even in the field of safety-related components.

[0005] The production of bio-based plastics or recycled plastics is known per se. Due to the required reliability of the components, the use of bio-based plastics or recycled plastics in safety devices of vehicles has not yet been promoted.

[0006] Therefore, it is a basic object of the present invention to provide a method for manufacturing a safety system based on sustainable raw materials.

[0007] This object is achieved by a method for producing an airbag module according to claim 1 and by a method for producing a seat belt of a safety system in a vehicle according to claim 2 .

[0008] Advantageous embodiments of the method according to the invention for producing an airbag module and of the method for producing a seat belt of a safety system in a vehicle are specified in the dependent claims, which advantageous embodiments can be selectively combined with one another.

[0009] According to the invention, this object is achieved by a method for producing an airbag module of a safety device in a vehicle, wherein the airbag module comprises a module housing, an airbag arranged in the module housing, and a gas generator connected to the module housing. The method comprises the following steps:

[0010] Providing a multifilament yarn by melt spinning;

[0011] weaving the multi-filament yarn into a fabric, and optionally finishing the fabric;

[0012] cutting the fabric into wall portions of an airbag and sewing the wall portions to form an airbag having a gas inlet;

[0013] introducing the airbag with the gas inlet into the module housing, and

[0014] The gas inlet is coupled to the gas generator, thereby forming the airbag module.

[0015] The multi-filament yarn is formed from at least one thermoplastic polymer that is partially or completely produced using recycled or renewable raw materials.

[0016] The invention also relates to a method for producing a seat belt of a safety device in a vehicle, the method comprising the following steps:

[0017] providing a multifilament yarn by melt spinning a thermoplastic polymer;

[0018] weaving the multi-filament yarn into a fabric tape and optionally finishing the fabric; and

[0019] The fabric belt is cut into safety belts having a defined length.

[0020] In this case, the thermoplastic polymers for producing the multifilament yarns by melt spinning are also produced completely or partly from recycled and / or renewable raw materials.

[0021] The seat belt can preferably be coupled to a belt tensioner module which can be activated mechanically, electromechanically or explosively in the event of an accident and acts on the seat belt.

[0022] Relying on recycled or renewable raw materials for the production of thermoplastic polymers and their subsequent processing into multifilament yarns can make textile-based components of safety systems in vehicles sustainable and can be produced with reduced PCF. This can significantly contribute to the climate-friendly production of these components without affecting the safety-related properties of the product. In addition, the dependence of the manufacturing process on fossil starting materials can be further reduced. Eliminating fossil starting substances in the production can also include reducing energy-intensive chemical reactions and thus contribute to designing the proposed method in a resource-saving, sustainable and environmentally friendly manner.

[0023] The invention is based on the recognition that recycled and renewable materials are also suitable for producing safety-related components in vehicles. This is not self-evident in view of the high demands placed on airbags and / or seat belts. The inventors have recognized that thermoplastic polymers made of renewable or recycled materials can be integrated into the production of seat belts and airbag modules without affecting the safety-related properties of these components.

[0024] In principle, the present invention is not limited to a specific thermoplastic polymer, but any thermoplastic polymer known in the art to be suitable as a component of a multifilament yarn for airbags and seat belts may be used.

[0025] According to one aspect, the thermoplastic polymer is advantageously at least partially formed from recycled polyesters and / or recycled polyamides. Optionally, the thermoplastic polymer may also contain a certain proportion of petroleum-based polyesters and / or petroleum-based polyamides. In the following, "petroleum-based" is understood to be polyesters and / or polyamides prepared from non-recycled starting materials and raw materials derived from petroleum or its derivatives.

[0026] According to another aspect, however, the thermoplastic polymer can also be formed completely from recycled polyester and / or recycled polyamide.

[0027] The thermoplastic polymer can also be formed from bio-based polyesters and / or bio-based polyamides, ie polyesters and / or polyamides prepared from renewable raw materials. Optionally, the thermoplastic polymer can also contain a certain proportion of petroleum-based polyesters and / or polyamides.

[0028] According to another aspect, however, the thermoplastic polymer can also be formed completely from bio-based polyesters and / or bio-based polyamides.

[0029] In addition, three-component compositions of the thermoplastic polymer are also conceivable, wherein the thermoplastic polymer comprises (A) a portion consisting of bio-based polyester and / or bio-based polyamide, (B) a portion consisting of recycled polyester and / or recycled polyamide, and (C) a portion consisting of petroleum-based polyester and / or petroleum-based polyamide.

[0030] The three-component composition advantageously comprises, respectively, relative to the total weight of the thermoplastic polymer, (A) a bio-based polyester and / or a bio-based polyamide in a proportion of 5 to 90 wt. %, (B) a recycled polyester and / or a recycled polyamide in a proportion of 5 to 90 wt. %, and (C) a petroleum-based polyester and / or a petroleum-based polyamide in a proportion of 0 to 20 wt. %, wherein components (A) to (C) total 100 wt. %.

[0031] The use of raw materials from different sources offers the advantage that the PCF of the thermoplastic polymer formed therefrom can be set as desired. A higher proportion of recycled polyester and / or recycled polyamide and / or bio-based polyester and / or bio-based polyamide reduces the PCF, whereas an increasing proportion of petroleum-based polyester and / or petroleum-based polyamide results in an increase in the PCF. The PCF of the thermoplastic polymer can be determined as described above.

[0032] The polymers described have already been used to manufacture fabrics for airbags and / or seat belts, so that known specifications can be utilized.

[0033] According to another aspect, the recycled polyester is selected from the group consisting of recycled polyethylene terephthalate (PET), polyethylene terephthalate (PET) with a proportion of at least 30 wt. % from renewable raw materials and polyethylene terephthalate (PET) with a proportion of 100 wt. % from renewable raw materials and combinations thereof.

[0034] The recycled polyamide may be selected from the group consisting of polyamide 4.10, polyamide 4.6, polyamide 5.6, polyamide 5.10, polyamide 6, polyamide 6.10, polyamide 10.10, polyamide 10.12 and polyamide 11 and combinations thereof, hereinafter referred to as PA 4.10, PA 4.6, PA 5.6, PA 5.10, PA 6, PA 6.10, PA 10.10, PA 10.12 and PA 11.

[0035] The polyamides mentioned above are characterized by particularly high tear strength and load-bearing capacity, making them particularly suitable as polymer materials for airbag fabrics and seat belts.

[0036] The recycled raw materials are in particular thermoplastic polymers. With regard to the thermoplastic polymers, the recycled raw materials are essentially not restricted and all known thermoplastic polymers can be used.

[0037] The recycled raw material is advantageously obtained from the initial raw material, which may originate from various sustainable sources. The initial raw material preferably originates from production waste, recycling systems and / or residual waste.

[0038] For example, industrial product waste and packaging waste, for example from bottle recycling systems, can be used. From these wastes, an almost homogeneous starting material can be obtained. However, it is also possible to use starting materials from tertiary waste (for example household garbage), from which plastic waste can be separated by mechanical and chemical methods.

[0039] Recycled raw materials can be obtained from the above sources by recycling materials, especially removing foreign matter.

[0040] In the text which follows, material recycling is understood to mean a process for recycling initial raw materials, in particular recycling plastics such as thermoplastic polymers, wherein the polymer structure remains unchanged during the recycling process.

[0041] The material recycling comprises at least one step selected from the group consisting of classification, comminution, cleaning, drying, post-polymerization, for example by solid state polycondensation (SSP) and / or liquid state polycondensation (LSP), extrusion and re-pelletization.

[0042] The classification of the initial raw materials to be recycled can be carried out by a recycling system or by spectroscopic methods such as near infrared spectroscopy (NIR). The spectral study of the initial raw materials can especially separate the individual plastic categories from each other. Auxiliary, the initial raw materials can be separated from each other by inductive and magnetic metal separation, air separation and screening processes. If necessary, the separated plastic categories can now be crushed. After the crushing, a wet machine treatment is carried out, which consists of a multi-stage cleaning and separation process. In particular, foreign components such as food residues, minerals and other organic residues can be removed. The individual target plastic categories can be separated from each other in a pool or by classification centrifugation by means of their density. Similar methods for density separation are known in the prior art and can also be used. In the case of similar density ranges of the plastics to be separated, the near infrared spectroscopy mentioned above can be used for targeted differentiation. The plastic can then be dried by mechanical and / or thermal methods. Vacuum drying is particularly suitable for this. The single-classified recyclate obtained in this way can now be completely melted in an extruder under pressure and temperature. Finally, the melt is granulated and cooled.

[0043] Alternatively, the thermoplastic polymer can also be dissolved in a suitable solvent and freed of impurities, the molecular structure of the polymer remaining unchanged. By means of special solvents adapted to the respective plastic, the plastic can be introduced into solution, the polymer structure remaining unchanged. The residues thus obtained can be removed, for example, by filtration. After separation, the plastic that has entered the solution can be precipitated, the solvent removed and the plastic dried. The plastic thus obtained can then be granulated in an extruder.

[0044] The use of solvents offers the advantage that even heavily impure plastic waste can be recycled in high quality. Impurities that are otherwise difficult to separate from the plastic can thus be removed, since they are insoluble in the solvent. Multilayer plastic stacks can also be separated. The choice of a suitable solvent depends on the plastic to be recycled.

[0045] Melt filtration provides another possibility for the purification and recycling of thermoplastic polymers. Here, the starting raw materials to be recycled are melted and the resulting melt is filtered through a suitable filter element, where the impurities are retained. The filter element can especially be a porous metal filter element.

[0046] Melt filtration offers the technical advantage that impurities can be removed to ensure the desired polymer purity even without the use of solvents.

[0047] Material recycling is particularly suitable for purifying thermoplastic polymers from industrial waste and packaging waste. Material recycling offers the advantage of lower processing costs associated with the recycling process itself. However, this is associated with a corresponding feed quality, which is ensured in particular by the initial sorting.

[0048] In order to purify waste materials with a lot of impurities, raw material recycling or chemical recycling can also be used, in which the polymer is depolymerized and split into its basic monomers or other basic substances by means of thermochemical or wet chemical methods. Chemical recycling includes at least one step selected from the group consisting of: depolymerization, purification, polymerization and regranulation.

[0049] Particularly suitable are solvolysis processes, in which the polymer is selectively transferred into an aqueous or organic solution at elevated temperature and pressure using suitable reagents such as acids, bases, alcohols and amines. The polymer is thereby decomposed into its base monomers or derivatives thereof, which can then be separated from the reaction mixture and purified separately. It can then be converted again into the desired polymer by polymerization.

[0050] Renewable raw materials are advantageously monomers obtained from biomass. These are referred to hereinafter as bio-based monomers.

[0051] The choice of bio-based monomers is essentially unlimited and any known bio-based monomer that can be prepared from biomass and is suitable for polymerization to form a thermoplastic polymer can be used. Thus, thermoplastic polymers prepared entirely or in part using bio-based monomers are bio-based thermoplastic polymers. Using biomass to prepare such polymers provides the advantages that these polymers are readily available, renewable, and sustainable under appropriate growth conditions.

[0052] In an advantageous embodiment, the bio-based monomer is selected from the group consisting of aliphatic polycarbonates, aliphatic polyamines, terephthalic acid, isophthalic acid and aliphatic polyols, especially monoethylene glycol, and combinations thereof.

[0053] Other bio-based monomers that can be obtained from renewable raw materials are succinic acid formed from glucose by fermentation, valeric acid from the hydrolysis step of biogas plants, pimelic acid from castor oil, azelaic acid formed from oleic acid by oxidation, and dodecanedioic acid from the fermentation of coconut or palm kernel oil and capric acid. Starting from these monomers, the corresponding diols and / or diamines can be obtained by biotechnological methods and optionally by other chemical reactions.

[0054] In particular, sugar-containing plants, starch-containing plants, lignocellulose and / or agricultural waste are suitable as biomass. Such plants are particularly suitable because they have a particularly high proportion of sugar building blocks linked to one another by glycosidic bonds, such as starch.

[0055] Examples of suitable plants are potatoes, sugar beets, wheat and corn.

[0056] Also suitable are oleaginous fruits, including oleaginous seeds, and oleaginous plants and plant parts.

[0057] For example, the seeds of the castor tree are suitable as oily fruits.

[0058] The starting material polysaccharides, in particular sugars and starch, lignin, cellulose and / or vegetable oils, in particular castor oil, can advantageously be obtained from biomass, optionally by means of fermentation and / or catalytic processes. More precisely, the starch contained in the biomass can be converted into sugars. Sugars are understood to be, in particular, all types of pentasaccharides such as ribose, arabinose and xylose, hexasaccharides such as fructose, glucose, mannose, galactose and rhamnose, and derivatives thereof such as derivatized amines, amides, esters and deoxy compounds.

[0059] The starting materials discussed herein can be used to prepare bio-based monomers.

[0060] The steps for preparing thermoplastic bio-based polymers from renewable raw materials include, in particular, the formation of bio-based monomers from biomass by oxidation or reduction, fermentation, chemical transformation and / or hydrolysis, as well as the polymerization of the monomers and the pelletization of the polymers prepared therefrom.

[0061] In this way, for example, the alcohols and dicarboxylic acids required for the preparation of polyesters and also dicarboxylic acids and diamino compounds or amino-substituted carboxylic acids or lactones required for the preparation of polyamides can be obtained.

[0062] According to another aspect, the thermoplastic polymer is a bio-based polymer PA5.6 provided by the following steps:

[0063] hydrolyzing the biomass to obtain a sugar-starch mixture;

[0064] Bacterially fermenting the sugar-starch mixture to form 1,5-diaminopentane;

[0065] fermenting the sugar-starch mixture with yeast to form 1,6-adipic acid; and

[0066] 1,5-diaminopentane and 1,6-adipic acid are polycondensed to obtain the thermoplastic bio-based polymer PA5.6.

[0067] According to another aspect, the thermoplastic polymer is a bio-based polymer PA4.10 provided by the following steps:

[0068] extrusion of biomass to obtain extrusion residues and vegetable oil;

[0069] fermenting the extrusion residue and / or biomass to form 1,4-butanediamine;

[0070] alkaline hydrolysis of vegetable oil to obtain 1,8-octanedicarboxylic acid; and

[0071] 1,8-octanedicarboxylic acid and 1,4-butanediamine are polycondensed to obtain the thermoplastic bio-based polymer PA4.10.

[0072] In this way, polyamide 4.10 can be produced directly from biomass without using any starting materials from fossil raw materials. The polyamide 4.10 produced in this way is particularly suitable for use as multifilament yarns in airbags or seat belts.

[0073] In another aspect, the thermoplastic polymer is Bio-PET 100% provided by the following steps:

[0074] hydrolyzing the biomass to obtain a sugar-starch mixture;

[0075] fermenting the sugar-starch mixture to form bioethanol;

[0076] Dehydrating bioethanol to obtain ethylene;

[0077] oxidizing ethylene with oxygen to obtain ethylene oxide;

[0078] hydrolyzing ethylene oxide to obtain monoethylene glycol;

[0079] selectively a) acid-catalyzed dehydration of sugars to (hydroxymethyl)furfural (HMF), which is then hydrogenated to 2,5-dimethylfuran, which is added to ethylene and subsequently dehydrated to give p-xylene;

[0080] or b) catalytically hydrogenating the hydrolyzed biomass to obtain a deoxygenated starting material which is subsequently converted into para-xylene through a refining process;

[0081] catalytically oxidizing para-xylene to terephthalic acid; and

[0082] Monoethylene glycol and terephthalic acid are polycondensed to obtain the thermoplastic polymer bio-PET 100%.

[0083] The thermoplastic polymer BioPET 100% obtained in this way consists essentially (ie 100%) of renewable raw materials (ie monoethylene glycol and terephthalic acid). BioPET 100% can also be used directly to produce airbag modules and seat belts.

[0084] The thermoplastic polymer may also be bio-PET 30%, wherein bio-based monoethylene glycol and terephthalic acid prepared in a conventional manner from petroleum-based raw materials are provided and reacted with one another in a subsequent step in a polycondensation, thereby obtaining bio-PET 30%.

[0085] The designation BioPET 30% is here merely a common name for the thermoplastic PET polymer obtained. Based on the stoichiometric ratio of the polycondensation, bio-based monoethylene glycol is present in the PET polymer in a proportion of 31.2% by weight and terephthalic acid in a proportion of 68.8% by weight.

[0086] For the preparation of bio-based monoethylene glycol, the same process can be used as already explained above for bio-PET 100%.

[0087] The preparation of terephthalic acid from crude oil is known in the prior art. For example, naphtha (raw gasoline) can be obtained from crude oil by fractional distillation as a starting material. By steam cracking of naphtha, p-xylene can be obtained, which can in turn be separated by fractional distillation. Targeted oxidation of p-xylene produces the desired terephthalic acid. For example, p-xylene can be reacted with air oxidation and in the presence of a cobalt-based catalyst to produce terephthalic acid.

[0088] The monomers thus obtained from renewable raw materials can also be polycondensed to give polyamides.The polycondensation reaction between aliphatic polyamides and aliphatic dicarboxylic acids to give polyamides has been known for a long time.

[0089] In general, bio-based polymers as well as recycled polymers may also be post-polymerized to achieve a degree of polymerization suitable for the intended application.

[0090] Recycled polymers and bio-based polymers, especially polyamides and polyesters, produced by the above-described method can be used as base polymers in the production of airbag modules and seat belts.

[0091] The melt spinning of the base polymer obtained in this way is carried out according to known methods of yarn manufacturing technology, as described, for example, in Ulmann's Encyclopedia of Industrial Chemistry, Vol. 13, p. 465 et seq. (2003).

[0092] In this way, multifilament yarns are obtained which are produced completely or partly from recycled or renewable raw materials.

[0093] In one aspect, the multifilament yarn used in the process of the invention is formed from PA 6.6 and has a count of 235 to 700 dtex, preferably 350 to 700 dtex, a breaking strength in the range of 20 to 60 N and a tear elongation in the range of 15 to 25%.

[0094] In other aspects, the multifilament yarn used in the method of the present invention is formed from PET and has a count of 470 to 555 dtex, a breaking strength in the range of 35 to 40 N, and a tear elongation in the range of 15 to 30%. Example

[0095] Two examples of multifilament yarns which can be used in the method of the present invention are given below.

[0096] In a first example, a bio-based polyamide 5.6, hereinafter PA5.6, was prepared.

[0097] To produce bio-based polyamide 5.6, biomass is provided in the form of plant waste in a first step. The biomass is subsequently hydrolyzed, thereby obtaining a sugar-starch mixture. This mixture is then fermented, thereby forming 1,5-diaminopentane. In addition, adipic acid is obtained from petroleum refineries by means of an oxidation reaction. The subsequent polycondensation of 1,5-diaminopentane and adipic acid produces bio-based PA5.6.

[0098] The PA5.6 obtained is processed by melt spinning into monofilaments, from which multifilament yarns can then be formed.

[0099] The obtained multifilament yarns made of bio-based PA5.6 each had a filament count of f96. The breaking strength and tearing elongation were determined according to standard ISO 13934-1, and the count was determined according to standard ISO 1144 (Table 1).

[0100] The yarn count and the fabric structure and the resulting breaking strength / tear elongation are characteristic for use in airbag fabrics or seat belts. The characteristic values ​​reproduced in Table 1, such as count, tear resistance, breaking strength and tear elongation of PA 5.6, are similar to yarns made from petroleum-based raw materials.

[0101] Table SEQ Tabelle \* ARABIC 1

[0102] In the second example, a multifilament yarn was produced from recycled PET. The PET required for producing the multifilament yarn was recycled by means of a material recycling process, so that the polymer structure was not changed. PET bottles were used as the starting material for the multifilament yarn.

[0103] In a first step, the PET beverage bottles from the collection system are freed of foil, metal and other plastics, classified and subsequently mechanically shredded into fragments. A thermal cleaning process is carried out, followed by vacuum drying. The fragments obtained are again subsequently classified and then re-pelletized. Finally, the re-pelletized material is spun into multifilament yarns in a melt spinning process.

[0104] The yarn thus obtained had a filament count of f 96. The breaking strength and the tearing elongation were determined according to standard ISO 13934-1 and the count was determined according to standard ISO 1144 (Table 2).

[0105] The yarn count and the fabric structure and the resulting breaking strength and tear elongation are important for use in airbag fabrics or seat belts. Multifilament yarns should have approximately the same properties as yarns based on non-recycled raw materials.

[0106] In Table 2, two multifilament yarns produced from recycled PET bottles according to the above method (Recycled) are compared with two multifilament yarns produced from non-recycled output feedstock (Standard).

[0107] A multifilament yarn (recycled) with a count of 470 dtex and a filament count of 96 f has the same properties as a multifilament yarn spun from non-recycled starting material with a similar count and the same filament count. Likewise, a multifilament yarn with a count of 555 dtex and a filament count of 96 f has the same properties as a multifilament yarn spun from non-recycled starting material with a similar count and the same filament count.

[0108] Table SEQ Tabelle \* ARABIC 2 BRIEF DESCRIPTION OF THE DRAWINGS

[0109] The present invention is described in detail below with reference to the accompanying drawings by means of embodiments, which should not be understood in a limiting sense. In the drawings:

[0110] Figure 1A schematic flow chart showing the steps of a method for manufacturing an airbag module and a seat belt according to the present invention;

[0111] Figure 2 A schematic flow chart showing the steps of the method for manufacturing from bio-based PA5.6;

[0112] Figure 3 a schematic flow chart showing the steps of the method for manufacturing from bio-based PA4.10; and

[0113] Figure 4 Schematic flow chart showing the steps of the method for manufacturing 100% from bio-PET.

[0114] Figure 1 A schematic flow chart showing the steps of a method for manufacturing an airbag module and a seat belt according to the present invention.

[0115] In the first step, starting materials are provided (S1).

[0116] The initial feedstock may be feedstock to be recycled or biomass.

[0117] The raw materials to be recycled originate in particular from primary, secondary and / or tertiary recycling. Primary recycling involves the use of initial raw materials from production waste, secondary recycling involves the use of initial raw materials from recycling systems, and tertiary recycling uses initial raw materials from other waste, in particular from residual waste that is difficult to recycle (such as household waste, bulky waste, electronic waste, post-consumer textiles), from waste collected from landfills or water bodies or industrial residues (for example from agriculture and / or the construction industry) from recovery measures.

[0118] In particular, sugar- and starch-containing plants and plant residues as well as oil-containing plants can be used as biomass. That is, almost any plant component can be used. The valorization of agricultural waste is advantageous because it avoids the use of land in competition with food production.

[0119] In the next step, the initial raw material is purified (S2). The raw material to be recycled is sent to material recycling or chemical recycling.

[0120] The material recycling is subdivided into the following sub-steps: classification, comminution, optional first extrusion of the granules, optional subsequent post-polymerization, optional second extrusion, thermal cleaning, drying, quality control and re-granulation by extrusion.

[0121] Melt filtration of the initial raw material can also be carried out as material recycle.

[0122] In addition to the purification of the recycled raw material, melt filtration of the initial raw material can also be employed.

[0123] Chemical recycling comprises, inter alia, the following sub-steps: classification, deagglomeration, purification, aggregation and re-granulation.

[0124] After material recycling or chemical recycling, recycled thermoplastic polymers are obtained.

[0125] The material recycling or chemical recycling is advantageously carried out in such a way that polyamide or polyester is obtained.

[0126] Instead, the biomass provided is processed in a separation step, so that a thermoplastic polymer formed from a renewable raw material is obtained ( S3 ).

[0127] The oil contained in the biomass or the starch contained in the biomass is firstly macerated and separated from the remaining biological components. The processing of the biomass can be subdivided into the following sub-steps: hydrolysis, fermentation and / or one or more chemical reactions, polymerization and granulation.

[0128] In the next step, the thermoplastic polymers from steps 2 (S2) and 3 (S3) can be combined again and processed into yarn (S4). The preparation of the yarn is divided into the following sub-steps: melt spinning, stretching and relaxing the spun filaments to the desired length and thickness, cooling the stretched filaments, connecting the individual monofilaments to form a multi-filament yarn and winding the obtained multi-filament yarn onto a yarn ring.

[0129] The individual filaments can be connected as required to form multifilament yarns with different numbers of filaments and / or different counts. For multifilament yarns made of PET, the yarn count and the number of filaments are particularly preferably different from those of multifilament yarns made of PA, and vice versa. Table 3 gives an overview of preferred yarn counts for multifilament yarns, depending on the thermoplastic polymer used.

[0130] Table 3

[0131] The multifilament yarn produced in this way can be processed further (for example by applying a protective layer or a sizing agent) in order to be used in a later weaving process ( S5 ). This can be done in particular by finishing the multifilament yarn.

[0132] Now, the multi-filament yarn is woven into a fabric or a fabric tape and the fabric is optionally finished (S6). Weaving can again be subdivided into the following sub-steps: weaving, washing, drying and optionally finishing the obtained fabric.

[0133] The fabric is then cut into wall parts of the airbag and the wall parts are sewn together to form the airbag with the gas inlet (S7). The fabric strip can also be cut into a safety belt, for example by cutting the fabric strip to a desired length.

[0134] In the last step, the airbag is installed in the module housing to obtain an airbag module, and the seatbelt is installed in the seatbelt retractor housing to obtain a seatbelt retractor module ( S8 ).

[0135] Figure 2 Schematic flow chart showing the steps of a method for producing a polyamide 5.6 multifilament yarn for use in airbags or seat belts.

[0136] In a first step, biomass is provided (S1). As already explained above, the biomass can be starch- and / or sugar-containing plants.

[0137] In the next step, hydrolysis is carried out, usually in an acid-catalyzed manner, at elevated pressure and elevated temperature, to obtain a sugar-starch mixture ( S2 ).

[0138] Sugar-starch mixtures are understood hereinafter to mean sugar-starch solutions, sugar-starch suspensions or other starch- and sugar-containing compositions which can be prepared from biomass.

[0139] In a further step, the mixture thus obtained can be further processed in a separate reaction step by fermentation with different microorganisms and / or enzymes (S3). This step is carried out so that the intermediate 1,5-diaminopentane or adipic acid is formed, respectively. The former is produced in particular by bacterial fermentation, while the latter is produced in particular by yeast fermentation. The biotechnological preparation of adipic acid can also include fermentation to muconic acid or glucaric acid, which are converted into adipic acid by subsequent hydrogenation (indirect fermentation).

[0140] For the fermentation, in particular the bacteria Corynebacterium glutamicum or Escherichia coli and also recombinant strains of Saccharomyces cerevisiae are used.

[0141] In the last step, the intermediate product obtained is reacted in a polycondensation reaction to obtain the desired polyamide 5.6 (S4). For the polycondensation, preference is given to a two-step reaction of the intermediately formed stoichiometric aminocarboxylates, in particular, since this ensures the ideal monomer ratio for achieving a high degree of polymerization.

[0142] Figure 3 Schematic flow chart showing the steps of a method for producing a polyamide 4.10 multifilament yarn for use in airbags or seat belts.

[0143] In a first step, biomass is provided (S1).

[0144] In this method, in particular oily plants or plant residues are used. For example, the oilseeds of the castor tree can be used in the process.

[0145] In the next step, the biomass is pressed to obtain vegetable oil and vegetable residues (S2). These are then separated from each other.

[0146] The intermediate 1,8-octanedicarboxylic acid (S3) was obtained from vegetable oil by alkaline hydrolysis.

[0147] Next, the plant residues and / or biomass are sent to bacterial fermentation in order to obtain the intermediate product 1,4-butanediamine (S4).

[0148] The two intermediate products are subsequently reacted with one another in a polycondensation reaction, thereby obtaining the desired polyamide 4.10 (S5).

[0149] Figure 4 Schematic flow chart showing the steps of a method for producing a bio-PET 100% multi-filament yarn for use in airbags or seat belts.

[0150] In a first step, starch- and sugar-containing biomass is provided ( S1 ).

[0151] In the next step, the biomass is hydrolyzed to obtain a sugar-starch mixture (S2).

[0152] In the next step, the sugar-starch mixture thus obtained is fermented and undergoes further chemical reactions, thereby obtaining the intermediates bioethanol and 2,5-dimethylfuran (S3). 2,5-Dimethylfuran is subsequently reacted to produce p-xylene. The sugar-starch mixture can be processed to p-xylene by means of two synthetic pathways.

[0153] In a first alternative, 2,5-dimethylfuran can be obtained by acid-catalyzed dehydration of sugars to (hydroxymethyl) furfural (HMF) and its subsequent hydrogenolysis. The addition of 2,5-dimethylfuran to ethylene and subsequent dehydration can then be carried out to obtain p-xylene (S4). For this purpose, part of the ethylene obtained in step S5 can be advantageously used.

[0154] According to a second alternative, catalytic hydrogenation of the hydrolyzed biomass can be carried out to obtain a deoxygenated starting material, wherein the deoxygenated starting material is subsequently reacted by a refining process to produce paraxylene (S4). For this purpose, refining processes known from the prior art can be used.

[0155] Bioethanol is obtained by fermentation of a sugar-starch mixture. For this purpose, the sugar-starch mixture is mixed with different microorganisms and / or enzymes. For example, Saccharomyces cerevisiae can be used to prepare bioethanol.

[0156] The p-xylene is then reacted chemically to form the intermediate terephthalic acid (S6). The reaction can be carried out in particular by air oxidation of the p-xylene in the presence of a cobalt-based catalyst.

[0157] In the next step, bioethanol is converted by dehydration to ethylene (S5).

[0158] The ethylene obtained is converted in the next step by dehydration to ethylene oxide (S7).

[0159] Ethylene oxide is then hydrolyzed to obtain the intermediate monoethylene glycol (S8).

[0160] In the last step, the intermediate products monoethylene glycol and terephthalic acid react with each other in a polycondensation reaction to produce bio-PET 100%.

Claims

1. A method for manufacturing an airbag module of a safety device in a vehicle, wherein the airbag module comprises a module housing, an airbag arranged in the module housing, and a gas generator connected to the module housing, wherein the method comprises the following steps: Providing a multifilament yarn by melt spinning; weaving the multi-filament yarn into a fabric, and optionally finishing the fabric; cutting the fabric into wall portions of an airbag and sewing the wall portions to form an airbag having a gas inlet; introducing the airbag with the gas inlet into the module housing, and coupling the gas inlet to the gas generator, thereby forming the airbag module, The multi-filament yarn is formed at least from a thermoplastic polymer which is partially or completely produced using recycled and / or renewable raw materials.

2. A method for manufacturing a seat belt of a safety device in a vehicle, wherein the method comprises the following steps: providing a multifilament yarn by melt spinning a thermoplastic polymer; weaving the multi-filament yarn into a fabric tape, and optionally finishing the fabric; as well as cutting the fabric belt into a safety belt having a defined length, The multi-filament yarn is formed at least from a thermoplastic polymer which is partially or completely produced using recycled and / or renewable raw materials.

3. The method according to claim 2, characterized in that The seat belt is coupled to a seat belt tensioner module which is designed to be activated mechanically, electromechanically or pyrotechnically in the event of an accident and to act on the seat belt.

4. The method according to any one of the preceding claims, characterized in that The thermoplastic polymer is formed of polyester and / or polyamide, wherein the polyester and / or the polyamide is selected from the group consisting of recycled polyester and / or recycled polyamide, bio-based polyester and / or bio-based polyamide and petroleum-based polyester and / or petroleum-based polyamide and combinations thereof.

5. The method according to any one of the preceding claims, characterized in that The polyester is selected from the group consisting of recycled polyethylene terephthalate (PET), bio-based polyethylene terephthalate (PET) having a monomer proportion from renewable raw materials of at least 30% by weight, and bio-based polyethylene terephthalate (PET) having a monomer proportion from renewable raw materials of at least 100% by weight, and combinations thereof.

6. The method according to claim 4 or 5, characterized in that: The recycled polyamide is selected from the group consisting of PA 4.10, PA 4.6, PA 5.6, PA 5.10, PA 6, PA 6.10, PA 10.10, PA 10.12 and PA 11 and combinations thereof.

7. The method according to any one of the preceding claims, characterized in that The recycled raw materials are obtained from initial raw materials originating from production waste, recycling systems and / or residual waste.

8. The method according to claim 7, characterized in that The recycled raw material is obtained by material recycling of the initial raw material.

9. The method according to claim 8, characterized in that The material recycling includes at least one step selected from the group consisting of classification, pulverization, cleaning, drying, post-polymerization, extrusion and re-granulation.

10. The method according to any one of claims 8 and 9, characterized in that The recycled raw material is purified from the raw material by means of melt filtration, wherein the melt filtration comprises the steps of melting the raw material to obtain a raw material melt, and subsequently filtering the raw material melt through a filter element to separate impurities and obtain the recycled raw material.

11. The method according to claim 7, characterized in that The recycled raw material is obtained from the initial raw material by chemical recycling.

12. The method according to claim 11, characterized in that The chemical recycling is a solvation process, wherein the solvation process comprises at least one step selected from the group consisting of: depolymerization, purification, polymerization and re-granulation.

13. The method according to any one of the preceding claims, characterized in that The renewable raw material is a monomer obtained from biomass, the monomer being selected from the group consisting of aliphatic polycarbonates, aliphatic polyamines, terephthalic acid and aliphatic polyols, especially monoethylene glycol, and combinations thereof.

14. The method according to claim 13, characterized in that The biomass is selected from the group consisting of sugar-containing plants, starch-containing plants, oil-containing plants and agricultural wastes, and combinations thereof.

15. The method according to any one of claims 13 and 14, characterized in that The starting raw material for preparing the monomer is derived from the biomass, and wherein the starting raw material is selected from the group consisting of sugars, polysaccharides, especially starch and / or cellulose, lignin, vegetable oils, especially castor oil, and combinations thereof.

16. The method according to any one of the preceding claims, characterized in that The thermoplastic polymer is a bio-based PA 5.6 provided by the following steps: hydrolyzing the biomass to obtain a sugar-starch mixture; Bacterial fermentation of the sugar-starch mixture to form 1,5-diaminopentane; fermenting the sugar-starch mixture with yeast to form 1,6-adipic acid; as well as 1,5-Diaminopentane and 1,6-adipic acid are polycondensed to obtain the thermoplastic polymer PA 5.

6.

17. The method according to any one of the preceding claims, characterized in that The thermoplastic polymer is a bio-based PA 4.10 provided by the following steps: extrusion of biomass to obtain extrusion residues and vegetable oil; fermenting the extrusion residue and / or biomass to form 1,4-butanediamine; alkaline hydrolysis of vegetable oil to obtain 1,8-octanedicarboxylic acid, and 1,8-Octanedicarboxylic acid and 1,4-butanediamine are polycondensed to obtain the thermoplastic polymer PA 4.

10.

18. The method according to any one of the preceding claims, characterized in that The thermoplastic polymer is 100% bio-PET provided by the following steps: hydrolyzing the biomass to obtain a sugar-starch mixture; fermenting the sugar-starch mixture to form bioethanol; Dehydrating bioethanol to obtain ethylene; oxidizing ethylene with oxygen to obtain ethylene oxide; hydrolyzing ethylene oxide to obtain monoethylene glycol; selectively a) acid-catalyzed dehydration of sugars to (hydroxymethyl)furfural (HMF), which is then hydrogenolyzed to 2,5-dimethylfuran, which is added to ethylene and subsequently dehydrated to give p-xylene; or b) catalytically hydrogenating the hydrolyzed biomass to obtain a deoxygenated starting material which is subsequently converted into para-xylene via a refining step; catalytically oxidizing para-xylene to terephthalic acid; and Monoethylene glycol and terephthalic acid are polycondensed to obtain the thermoplastic polymer bio-PET 100%.

19. The method according to any one of the preceding claims, characterized in that The thermoplastic polymer is bio-PET 30%, in which monoethylene glycol prepared from biomass and petroleum-based terephthalic acid are reacted with each other in a polycondensation process, thereby obtaining bio-PET 30%.