Aluminum hydroxide particles, method for preparing same, separator comprising aluminum hydroxide particles, electrode assembly, and lithium secondary battery

By using separators prepared with characteristic aluminum hydroxide particles, the heat shrinkage problem of polyolefin film in lithium secondary batteries is solved, the capacity retention and safety of the battery are improved, and more efficient ion conduction and flame retardancy are achieved.

CN119013231APending Publication Date: 2024-11-22LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480001969.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-01-04
Filing Date
2024-01-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Polyolefin-based porous membrane separators in lithium secondary batteries exhibit heat shrinking behavior at high temperatures, resulting in a short circuit between the positive electrode and the negative electrode, affecting the capacity retention rate and safety of the battery.

Method used

Using aluminum hydroxide particles with specific particle sizes and lithium content, after eluting and crushing in alkaline aqueous solution, a partition with improved battery performance is prepared, including forming organic on porous polymer films or nonwoven fabrics- Inorganic composite coating for separators and electrode assembly.

Benefits of technology

The capacity retention rate of lithium secondary batteries is improved, side reactions are avoided, the ionic conductivity and flame retardancy of the battery is enhanced, the heat shrinkage phenomenon is reduced, and the safety and performance of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005061642160000201
    Figure BDA0005061642160000201
Patent Text Reader

Abstract

Aluminum hydroxide particles are disclosed in which the particles have a D50 of about 3.0 [mu] m or less, a BET of about 3.0 m2 / g or more, and a Li content of about 500 ppm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to aluminum hydroxide particles, a preparation method thereof, a separator including the aluminum hydroxide particles, an electrode assembly, and a lithium secondary battery.

[0002] This application is based on and claims the benefit of priority of Korean Patent Application No. 10-2023-0025344 filed on February 24, 2023, in the Korean Intellectual Property Office, and Korean Patent Application No. 10-2024-0001329 filed on January 4, 2024, in the Korean Intellectual Property Office, the disclosures of which are incorporated herein by reference in their entirety. Background Art

[0003] The separator constituting the electrode assembly of the secondary battery is used as a separator to allow the flow of ions between the positive electrode and the negative electrode without electrical connection. For example, the separator allows the electrolyte to pass therethrough while preventing the same diffusion of the electrolyte, thereby preventing an electrical short circuit between the positive electrode and the negative electrode. Therefore, since the separator may affect the capacity, charge and discharge rate, and life of the secondary battery, the material and structure of the separator are considered to be important factors in determining the performance and safety of the secondary battery.

[0004] The polyolefin-based porous film commonly used as a separator for lithium secondary batteries exhibits severe thermal shrinkage behavior at a temperature equal to or greater than 100°C due to its material properties and characteristics in the manufacturing process (including stretching), and therefore tends to cause a short circuit between the positive electrode and the negative electrode. In order to solve the safety problem of separators made of polyolefin-based porous films, separators using inorganic particles have been proposed.

[0005] The inorganic particles are applied to the separator by mixing the inorganic particles with the polymer and coating the mixture on the surface of a nonwoven fabric or a porous polymer film made of a polymer such as a polyolefin. Alternatively, the inorganic particles are applied to a self-supporting separator by mixing the inorganic particles with the polymer, coating the mixture on a support, and then peeling off the coating. Alternatively, the inorganic particles are applied to the separator by mixing the inorganic particles with the polymer and coating the mixture on the surface of the positive or negative electrode or the surface of both electrodes. Summary of the invention

[0006] Technical issues

[0007] One aspect of the present disclosure provides aluminum hydroxide particles that improve the capacity retention rate of a lithium secondary battery and do not cause a side reaction in the lithium secondary battery.

[0008] Another aspect of the present disclosure provides a method for preparing aluminum hydroxide particles having the above-mentioned characteristics.

[0009] Still another aspect of the present disclosure provides a separator, an electrode assembly, and a lithium secondary battery including the aluminum hydroxide particles having the above-mentioned characteristics.

[0010] It is quite obvious that the objects and advantages of the present disclosure can be achieved by the means or methods described in the claims and their combinations.

[0011] Technical Solution

[0012] One aspect of the present disclosure provides aluminum hydroxide particles according to the following embodiments.

[0013] A first embodiment relates to aluminum hydroxide particles,

[0014] It has a D50 of about 3.0 μm or less, about 3.0 μm 2 / g or more BET and a lithium (Li) content of about 500 ppm or more.

[0015] A second embodiment relates to the aluminum hydroxide particles according to the above-mentioned first embodiment, and

[0016] D50 is about 2.5 μm or less, BET is about 3.5 μm 2 / g or more and the Li content is about 800 ppm or more.

[0017] A third embodiment relates to the aluminum hydroxide particles according to the above-mentioned first embodiment, and

[0018] D50 is about 2.7 μm or less, BET is about 3.8 μm 2 / g or more and the Li content is about 900 ppm or more.

[0019] A fourth embodiment relates to the aluminum hydroxide particles according to the above-mentioned first embodiment, and

[0020] D50 is about 2.2 μm or less, BET is about 4.2 μm 2 / g or more and the Li content is about 1050 ppm or more.

[0021] A fifth embodiment relates to the aluminum hydroxide particles according to any one of the first to fourth embodiments described above, and

[0022] The sodium (Na) content is about 900 ppm or less.

[0023] The sixth embodiment is directed to the aluminum hydroxide particles according to any one of the first to fourth embodiments described above, and

[0024] The Na content is about 100 ppm or less.

[0025] The seventh embodiment is directed to the aluminum hydroxide particles according to any one of the first to fourth embodiments described above, and

[0026] The Na content is about 10 ppm or less.

[0027] One aspect of the present disclosure provides a separator according to the following embodiments.

[0028] An eighth embodiment relates to a method for preparing aluminum hydroxide particles according to any one of the first to seventh embodiments described above, the method comprising:

[0029] (S1) obtaining an eluate by adding bauxite to an alkaline aqueous solution containing Li;

[0030] (S2) separating the eluate by filtering the solid from the eluate obtained in (S1); and

[0031] (S3) precipitating aluminum hydroxide from the separated eluate, wherein the aluminum hydroxide particles have a D50 of about 3.0 μm or less, a particle size of about 3.0 μm or less, and a particle size of about 3.0 μm or less. 2 / g or more BET and a lithium (Li) content of about 500 ppm or more.

[0032] A ninth embodiment relates to a method for preparing aluminum hydroxide particles according to the eighth embodiment described above,

[0033] The preparation method further comprises: before the above (S3), adding aluminum hydroxide seed crystals to the separated eluate, stirring the eluate, and then filtering the aluminum hydroxide seed crystals to separate the eluate again.

[0034] The tenth embodiment relates to a method for preparing aluminum hydroxide particles according to the eighth embodiment or the ninth embodiment described above,

[0035] The aluminum hydroxide precipitated from (S3) is pulverized, and then the pulverized aluminum hydroxide is added to (S1) instead of bauxite to repeat (S1) to (S3).

[0036] An eleventh embodiment is directed to a separator comprising:

[0037] a porous polymer membrane; and

[0038] an organic-inorganic composite coating layer formed on at least one surface of the porous polymer film and comprising a mixture of inorganic particles and a polymer,

[0039] The inorganic particles include the aluminum hydroxide particles according to any one of the first to seventh embodiments described above.

[0040] A twelfth embodiment is directed to a separator comprising:

[0041] porous polymer nonwoven fabrics; and

[0042] an organic-inorganic composite coating layer coated on at least one surface of the porous polymer nonwoven fabric and comprising a mixture of inorganic particles and a polymer,

[0043] The inorganic particles include the aluminum hydroxide particles according to any one of the first to seventh embodiments described above.

[0044] A thirteenth embodiment relates to a separator,

[0045] It includes a self-supporting organic-inorganic composite film comprising a mixture of inorganic particles and a polymer,

[0046] The inorganic particles include the aluminum hydroxide particles according to any one of the first to seventh embodiments described above.

[0047] One aspect of the present disclosure provides an electrode assembly according to the following embodiments.

[0048] A fourteenth embodiment is directed to an electrode assembly comprising:

[0049] a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode,

[0050] The separator is the separator according to any one of the above-described eleventh to thirteenth embodiments.

[0051] A fifteenth embodiment relates to an electrode assembly,

[0052] It includes a separator formed on at least one surface of a positive electrode, a negative electrode, or both of the positive electrode and the negative electrode and comprising a porous organic-inorganic composite coating layer of a mixture of inorganic particles and a binder polymer,

[0053] The inorganic particles include the aluminum hydroxide particles according to any one of the first to seventh embodiments described above.

[0054] One aspect of the present disclosure provides a lithium secondary battery according to the following embodiments.

[0055] The sixteenth embodiment is directed to a lithium secondary battery including the electrode assembly according to any one of the above-described fourteenth embodiment or fifteenth embodiment.

[0056] Beneficial Effects

[0057] According to one embodiment of the present disclosure, in aluminum hydroxide particles containing a predetermined content or more of Li while D50 and BET are controlled within a predetermined range, Li remaining as an impurity in the particles does not cause side reactions in a lithium secondary battery, but instead improves the capacity retention rate of the lithium secondary battery.

[0058] The effects of the various components of the present disclosure will be described in more detail below. DETAILED DESCRIPTION

[0059] Hereinafter, the present disclosure will be described in detail. Before the description, it should be understood that the terms or words used in the specification and claims should not be interpreted as limited to the general meaning and dictionary meaning, but should be interpreted as the meaning and concept of the technical concept corresponding to the present disclosure based on the principle that allows the inventor to define the terms in order to explain his / her invention in the best possible way. Therefore, the descriptions presented herein are merely examples for illustrative purposes and are not intended to indicate all technical concepts of the present disclosure, so it should be understood that various equivalents and modifications may be made to them at the time of filing this application.

[0060] Throughout the specification herein, unless specifically described to the contrary, when a part is regarded as “including” or “provided with” a certain component, this does not exclude other components but means that the part may also include or may also be provided with other components.

[0061] Throughout the specification of the present application, the feature of having holes means that the object includes a plurality of holes to allow gaseous and / or liquid fluids to pass from one side surface to another side surface of the object through a structure in which the holes are connected to each other.

[0062] Throughout the specification of the present disclosure, particles refer to small objects having a diameter of several micrometers or less, and thus they are almost invisible regardless of their shape (eg, spherical shape, elliptical shape, or irregular shape).

[0063] As used herein, "about," "approximately," and "substantially" are used to refer to a range of numerical values ​​or degrees or approximate values ​​thereof taking into account inherent manufacturing and material tolerances, and to prevent an infringer from unfairly using the disclosed content in which precise or absolute numbers provided to aid in understanding the present disclosure are mentioned.

[0064] Throughout this disclosure, a separator is referred to as including a plurality of pores and having a porous character and serving as a porous ion-conducting barrier that allows ions to pass therethrough while preventing electrical contact between a negative electrode and a positive electrode in an electrochemical device.

[0065] In forming a separator by applying inorganic particles, various types of inorganic particles that are electrochemically stable within the operating voltage range of lithium secondary batteries have been proposed. Among the inorganic particles, aluminum trihydroxide (ATH) has attracted attention as an inorganic particle due to, for example, its flame retardant properties.

[0066] ATH is prepared by adding bauxite powder as a raw material to an aqueous NaOH solution and eluting an aluminum component therefrom to obtain an eluate, then precipitating ATH from the eluate and pulverizing ATH.

[0067] In the ATH obtained by using a NaOH solution during the elution process of bauxite powder, the Na component remains as an impurity. The Na component remaining in the ATH may not contribute to the performance (such as capacity retention) of the lithium secondary battery, but may instead cause a side reaction in the lithium secondary battery.

[0068] As described above, in order to solve the performance and safety problems of lithium secondary batteries, a separator having ATH particles, which are inorganic materials having flame retardant properties, has been proposed.

[0069] On the other hand, NaOH aqueous solution is used when preparing ATH particles, so Na component remains in the obtained ATH as an impurity. The remaining Na component in ATH is not conducive to the performance of the lithium secondary battery, such as capacity retention, but may cause side reactions in the lithium secondary battery, which may cause performance and safety problems of the lithium secondary battery.

[0070] In the present disclosure, a LiOH aqueous solution is used instead of a NaOH aqueous solution in the preparation of ATH, so that the impurities remaining in the prepared ATH are Li components instead of Na components. Unlike Na impurities, Li impurities do not cause side reactions in lithium secondary batteries, and increase the ionic conductivity of lithium secondary batteries, thereby improving capacity retention. At the same time, the alkaline aqueous solution according to an embodiment of the present disclosure is not limited to the LiOH aqueous solution, and may be, for example, any alkaline aqueous solution containing Li.

[0071] According to one aspect of the present disclosure, there is provided an ATH particle having a D50 (which is the average particle size of the inorganic particles) of about 3.0 μm or less, a particle diameter of about 3.0 μm or less, and a particle size of about 3.0 μm or less. 2 / g or more BET (which is a specific surface area) and a Li content of about 500 ppm or more.

[0072] For example, the ATH particles may have a D50 of about 2.5 μm or less, a D50 of about 3 ... 2 / g or more BET and about 800 ppm or more Li content.

[0073] Alternatively, the ATH particles may have a D50 of about 2.7 μm or less, a D50 of about 3.8 μm or less, a D50 of about 1.5 μm or less, ... 2 / g or more BET and a Li content of about 900 ppm or more.

[0074] In another example, the D50 may be about 2.2 μm or less and the BET may be about 4.2 μm or less. 2 / g or more, and the Li content may be about 1050 ppm or more. In another example, the D50 may be about 1.2 μm or less, and the BET may be about 7.8 m 2 / g or more, and the Li content may be about 1910 ppm or more.

[0075] When the Li content of the ATH particles is relatively low, for example, less than 500 ppm, there may be a limitation in improving the capacity retention rate of the lithium secondary battery. In addition, when the D50 of the ATH particles exceeds 3.0 μm, or when the BET becomes too small, it may be difficult to prepare ATH particles having a Li content of 500 ppm or more.

[0076] When the Li content of the ATH particles is equal to or greater than 500 ppm, the Li content of the ATH particles is sufficient, so the upper limit thereof is not limited. For example, the upper limit of the Li content of the ATH particles may be 10,000 ppm, but is not limited thereto.

[0077] The smaller the D50 of the ATH particles, the larger the BET. Conversely, the larger the BET, the smaller the D50. Therefore, the lower limit of the D50 of the ATH particles and the upper limit of the BET are not limited thereto. For example, the lower limit of the D50 of the ATH particles may be 0.01 μm, and the upper limit of the BET may be 20,000 g / m 2 , but the present disclosure is not limited thereto.

[0078] When D50 of the ATH particles exceeds 3.0 μm, BET becomes too small, in which case it may be difficult to produce ATH particles having a Li content of 500 ppm or more.

[0079] According to one embodiment, the aforementioned ATH particles may be prepared as follows.

[0080] First, bauxite, which is an aluminum-rich mineral, is added to a LiOH aqueous solution to obtain an eluate (S1). From this step, the aluminum component of the bauxite is eluted. In one embodiment, the eluate can be prepared by powdering the bauxite and placing the powdered bauxite in a high-pressure reactor together with a LiOH aqueous solution and stirring the solution at a high temperature.

[0081] Subsequently, the solid is filtered from the resultant of (S1) to separate the eluate (S2).

[0082] ATH is then precipitated from the separated eluate (S3). For example, ATH can be precipitated by lowering the temperature of the separated eluate and then stirring the eluate.

[0083] Prior to step (S3), ATH seed crystals may be added to the separated eluate, the eluate may be stirred, and then the ATH seed crystals may be filtered to separate the eluate again. The eluate separated again is put into step (S2).

[0084] The ATH precipitated from step (S3) is crushed, and then the crushed ATH can be put into step (S1) instead of bauxite to repeat steps (S1) to (S3) one or more times. By repeating the steps, the Li content and the content of other impurities in ATH can be controlled.

[0085] At the same time, in the preparation of the ATH particles of the present disclosure, bauxite powder as an aluminum-rich mineral can be used together with a LiOH aqueous solution to perform the aforementioned elution process and precipitation process, and then the precipitated result can be used together with a NaOH aqueous solution to perform the elution process and precipitation process again, thereby preparing an ATH precipitate. The ATH obtained in this way has a Li impurity of about 500ppm or more, and also has a Na impurity. In this case, the Na content can be about 900ppm or less to minimize the side reactions caused by Na impurities in the lithium secondary battery. According to one embodiment, the Na content can be about 100ppm or less, or the Na content can be about 10ppm or less.

[0086] The ATH precipitate obtained through the aforementioned process may be washed with distilled water and then pulverized using a pulverizer such as a bead mill to obtain ATH particles having a desired particle size.

[0087] The term "D50" of the present disclosure means the average particle size of the inorganic particles as described above. For example, "D50" means the particle size corresponding to 50% of the total volume when the particle size is measured by a particle size analyzer and accumulated in order from small particles.

[0088] In the present disclosure, the average particle size can be measured by laser diffraction. Laser diffraction can measure particle sizes generally ranging from the submicron region to a few nanometers, and highly reproducible and highly resolvable results can be obtained with laser diffraction.

[0089] In the present disclosure, the specific surface area (BET) of particles is measured from the amount of adsorbed nitrogen using a specific surface area analysis instrument.

[0090] In the present disclosure, the content of Li or Na impurities is measured using, for example, inductively coupled plasma-optical emission spectroscopy (ICP-OES).

[0091] The ATH particles of the present disclosure as described above can be used in lithium secondary batteries, for example, can be used as separators in lithium secondary batteries. For example, the ATH particles of the present disclosure can be used as separators of lithium secondary batteries in the form of an organic-inorganic composite layer containing a mixture of inorganic particles and a polymer, but the present disclosure is not limited thereto.

[0092] In the first form of the separator, the separator includes a porous polymer film; and an organic-inorganic composite coating formed on at least one surface of the porous polymer film and containing a mixture of inorganic particles and a polymer, the inorganic particles including the ATH particles of the present disclosure described above.

[0093] The porous polymer membrane substrate may be a porous polymer membrane made of polyolefin (eg, polyethylene, polypropylene, polybutylene, or polypentene), and the polyolefin porous polymer membrane exhibits a shutdown function at a temperature of, for example, about 80°C to 130°C.

[0094] In this case, the polyolefin porous polymer membrane may be formed using one or a mixture of two or more of polyolefin-based polymers, such as polyethylene, including high-density polyethylene, linear low-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene; polypropylene; polybutene or polypentene.

[0095] In addition, in addition to the above-mentioned polyolefins, the porous polymer film can also be formed using one or a mixture of two or more heat-resistant polymers having a melting point of 200°C or higher, such as polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide or polyethylene naphthalate, but not limited to these.

[0096] The porous polymer film may be formed into a structure in which two or more film layers are stacked, and each film layer may be formed of the above-mentioned polymer such as polyolefin or polyester alone, or of a mixture of two or more polymers.

[0097] An organic-inorganic composite coating is formed on at least one surface of the porous polymer film, the organic-inorganic composite coating mainly comprising a mixture of polymer and inorganic particles, the inorganic particles comprising the ATH of the present disclosure described above.

[0098] The ATH of the present disclosure described above helps to improve the capacity retention rate of the lithium secondary battery and improve the flame retardancy of the separator.

[0099] In addition to ATH, other inorganic particles can be mixed. The inorganic particles inhibit the thermal shrinkage phenomenon of the porous polymer film during the so-called thermal runaway of the battery, and even if the polymer film melts, the inorganic particles prevent direct contact between the positive electrode and the negative electrode and prevent the battery from exploding.

[0100] In addition to ATH, there are no particular limitations on the inorganic particles that can be mixed, as long as the inorganic particles to be used are electrochemically stable. For example, there are no particular limitations on the inorganic particles that can be used in the present disclosure, as long as the inorganic particles to be used do not cause oxidation and / or reduction reactions within the operating voltage range of the lithium secondary battery to which they are applied (for example, based on Li / Li + is 0 V to 5 V). For example, using inorganic particles with a relatively high dielectric constant as the inorganic particles can help increase the dissociation degree of electrolyte salts such as lithium salts in the electrolyte liquid, thereby improving the ionic conductivity of the electrolyte.

[0101] For the foregoing reasons, the inorganic particles can include high-dielectric inorganic particles with a dielectric constant of about 5 or greater, or about 10 or greater. Non-limiting examples of inorganic particles with a dielectric constant of about 5 or greater can include any one of the inorganic particles selected from the following: BaTiO3, Pb(Zr x ,Ti 1-x )O3 (PZT, where 0 < x < 1), Pb 1-x La x Zr 1-y Ti y O3 (PLZT, where 0 < x < 1, 0 < y < 1), (1 - x)Pb(Mg 1 / 3 Nb 2 / 3 )O 3-x PbTiO3 (PMN-PT, where 0 < x < 1), hafnium oxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, boehmite, AlOOH, SiC, and TiO2, or a mixture of two or more of them.

[0102] In addition, for the inorganic particles, inorganic particles with lithium ion transport ability can be used, that is, inorganic particles containing lithium element but not storing lithium and having the function of transporting lithium ions. Non-limiting examples of inorganic particles with lithium ion transport ability include lithium phosphate (Li3PO4); lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3); lithium aluminum titanium phosphate (Lix Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, 0 < z < 3; (LiAlTiP) x O y -series glasses (0 < x < 4, 0 < y < 13), such as 14Li2O - 9Al2O3 - 38TiO2 - 39P2O5; lithium lanthanum titanate (Li x La y TiO3, where 0 < x < 2, 0 < y < 3); lithium germanium thiophosphate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), such as Li 3.25 Ge 0.25 P 0.75 S4; lithium nitride (Li x N y , where 0 < x < 4, 0 < y < 2), such as Li3N; SiS2 - series glasses (Li x Si y S z , where 0 < x < 3, 0 < y < 2, 0 < z < 4), such as Li3PO4 - Li2S - SiS2; P2S5 - series glasses (Li x P y S z , where 0 < x < 3, 0 < y < 3, 0 < z < 7), such as LiI - Li2S - P2S5; or a mixture of two or more of them.

[0103] Mix the inorganic particles with a polymer and coat at least one surface of the porous polymer membrane substrate. Non - limiting examples of the polymer can include polyvinylidene fluoride, polyvinylidene fluoride - co - hexafluoropropylene, polyvinylidene fluoride - co - trichloroethylene, polyvinylidene fluoride - co - trifluorochloroethylene, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, ethylene - vinyl acetate copolymer, poly(ethylene oxide), cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile - styrene - butadiene copolymer, polyimide, or a mixture of two or more of them, for which an ion - conductive polymer or an ion - non - conductive polymer can be used.

[0104] The inorganic particles can be positioned substantially in contact with each other. In this case, when the mixed polymer is formed as a coating on part or the whole surface of the inorganic particles, the polymer can connect and fix the inorganic particles so that the inorganic particles remain bound together.

[0105] The first form separator as described above can be manufactured by further dispersing inorganic particles in a slurry obtained by dissolving or dispersing a polymer in a solvent, and then coating the slurry on at least one surface of a porous polymer film and drying to form an organic-inorganic composite coating.

[0106] In the second form of the separator, the separator includes: a porous polymer nonwoven fabric; and an organic-inorganic composite coating comprising a mixture of inorganic particles and a polymer, the organic-inorganic composite coating being coated on at least one surface of the porous polymer nonwoven fabric, the inorganic particles comprising the ATH particles of the present disclosure as described above.

[0107] The porous polymer nonwoven fabric refers to a porous polymer nonwoven fabric having holes formed between the fibers constituting the nonwoven fabric, and examples of the porous polymer nonwoven fabric may include spunbonded nonwoven fabrics and meltblown nonwoven fabrics. The nonwoven fabric refers to a fabric formed by interlocking fibers, rather than a fabric woven with warp and weft yarns using a loom or a knitted fabric knitted using a knitting machine.

[0108] The fibers constituting the nonwoven fabric may be made of the above-mentioned heat-resistant polymer, and fibers made of a polyolefin-based polymer may be used alone or in combination with heat-resistant polymer fibers.

[0109] As for the inorganic particles and the polymer, the aforementioned inorganic particles and polymers can be used.

[0110] The second form of separator can be further dispersed in the slurry obtained by dissolving or dispersing the polymer in a solvent, and then the slurry is coated on at least one surface of the porous polymer nonwoven fabric and dried to form an organic-inorganic composite coating. According to the pore size of the porous polymer nonwoven fabric, the organic-inorganic composite coating can be located on the surface of the porous polymer nonwoven fabric, can be located in both the surface and the internal pores of the porous polymer nonwoven fabric, or can be mainly located in the interior of the porous polymer nonwoven fabric.

[0111] The inorganic particles may be positioned substantially in contact with each other except for a state in which fibers are interposed therebetween.

[0112] In a third form of the separator, the separator includes a self-supporting organic-inorganic composite film including a mixture of inorganic particles and a polymer, the inorganic particles including the ATH particles of the present disclosure as described above.

[0113] The term self-supporting type refers to a form in which the separator can maintain a shape by itself without being coated or adhered to an additional support.

[0114] As for the inorganic particles and the polymer, the aforementioned inorganic particles and polymers can be used.

[0115] The separator of the third form can be by inorganic particles further dispersed in the slurry obtained by dissolving or dispersing polymer in a solvent, the slurry is coated on a support such as polytetrafluoroethylene and dried, and then peeled off the coating from the support to make. In this case, the inorganic particles of the self-supporting organic-inorganic composite film can be basically in contact with each other. When the mixed polymer is formed as coating on the part or whole surface of inorganic particles, polymer can connect and fix inorganic particles so that inorganic particles remain combined together.

[0116] The fourth form of the separator may be a separator in the form of a porous organic-inorganic composite coating layer formed on at least one surface of the positive electrode, the negative electrode, or both and including a mixture of inorganic particles and a binder polymer.

[0117] As for the inorganic particles and the polymer, the aforementioned inorganic particles and polymers can be used.

[0118] The fourth form of the separator can be manufactured by further dispersing inorganic particles in a slurry obtained by dissolving or dispersing a polymer in a solvent, and then coating the slurry on at least one surface of the positive electrode, the negative electrode, or both the positive electrode and the negative electrode and drying to form an organic-inorganic composite coating.

[0119] In the separator of any one of the first to fourth forms described above, the organic-inorganic composite coating or the organic-inorganic composite film may be porous. The weight ratio of the inorganic particles to the polymer may be in the range of about 99:1 to 50:50, but is not limited thereto. The thickness of the separator may be in the range of about 1 μm to 30 μm, but is not limited thereto.

[0120] In this case, the pores formed in the organic-inorganic composite coating or the organic-inorganic composite film may be formed in the polymer matrix by plasticizer extraction, or may be configured as gaps formed between inorganic particles as the inorganic particles are positioned substantially in contact with each other.

[0121] The above-mentioned separator of the present disclosure may be applied to the following electrode assemblies, but is not limited thereto.

[0122] The separator of any one of the first to third forms is stacked on or interposed between a positive electrode, a negative electrode, or both, and they are bonded to each other through a process such as a lamination process to manufacture an electrode assembly.

[0123] The fourth form of the separator is stacked in the form of a coating on at least one surface of the positive electrode, the negative electrode, or both the positive electrode and the negative electrode, and they are bonded to each other through a process such as a lamination process to manufacture an electrode assembly.

[0124] As necessary, in addition to the aforementioned separator of the present disclosure, a typical conventional separator may be interposed between the positive electrode and the negative electrode.

[0125] Hereinafter, a positive electrode and a negative electrode constituting an electrode assembly will be described by way of example.

[0126] The positive electrode includes a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector.

[0127] For the positive electrode, the positive electrode collector is not particularly limited as long as it is conductive and does not cause chemical changes in the battery. For example, stainless steel; aluminum; nickel; titanium; calcined carbon or aluminum or stainless steel surface-treated with carbon, nickel, titanium or silver can be used for the positive electrode collector. In addition, the thickness of the positive electrode collector can generally be about 3 μm to 500 μm, and fine unevenness can be formed on the surface of the positive electrode collector to increase the adhesion of the positive electrode active material. For example, the positive electrode collector can be used in a variety of forms, such as films, sheets, foils, nets, porous materials, foams and non-woven materials.

[0128] The positive electrode active material layer may include a known positive electrode active material, a conductive material, and a binder.

[0129] The positive electrode active material may include a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxide represented by LiMnO4 (wherein x is 0 to 0.33), LiMnO3, LiMn2O3 or LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxide, such as LiV3O8, V2O5 or Cu2V2O7; 1-x M x Ni-site lithium nickel oxide represented by O2 (wherein M is Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x is 0.01 to 0.3); represented by the chemical formula LiMn 2-x M x Lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M is Fe, Co, Ni, Cu or Zn) or Li2Mn3MO8 (wherein M is Fe, Co, Ni, Cu or Zn); LiMn2O4 in which part of Li is replaced by alkaline earth metal ions; disulfide compounds; and Fe2(MoO4)3, but are not limited thereto.

[0130] The conductive material is used to provide conductivity to the electrode, and can be used without particular limitation, as long as it does not cause chemical changes in the battery and has electronic conductivity. Examples of conductive materials may include graphite, such as natural graphite or artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber, such as copper, nickel, aluminum, and silver; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, and any one of them may be used alone, or a mixture of two or more of them may be used. The conductive material may be included in an amount of about 1% by weight to 30% by weight based on the total weight of the positive electrode active material layer.

[0131] Binder is used to improve the adhesion between positive active material particles and the adhesion between positive active material and positive current collector. Examples of binders may include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber or its various copolymers, any one of which may be used alone, or a mixture of two or more of which may be used. Based on the gross weight of the positive active material layer, the binder may be included in an amount of about 1% by weight to 30% by weight.

[0132] The positive electrode can be manufactured according to a conventional positive electrode preparation method. For example, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer comprising a positive electrode active material and an optional binder and a conductive material to a positive electrode current collector, followed by drying and rolling. In this case, the types and contents of the positive electrode active material, the binder and the conductive material are as described above.

[0133] The solvent may be any solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, any one of which may be used alone, or a mixture of two or more of which may be used. Considering the thickness of the slurry applied, its manufacturing yield, the amount of the solvent used is sufficient as long as it can dissolve or disperse the positive electrode active material, the conductive material and the binder and has a viscosity that can show good thickness uniformity when subsequently applied to prepare the positive electrode.

[0134] Alternatively, the positive electrode can be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the film obtained by peeling from the support on the positive electrode current collector.

[0135] The negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0136] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, for example, copper; stainless steel; aluminum; nickel; titanium; calcined carbon; or copper or stainless steel surface-treated with carbon, nickel, titanium or silver; or aluminum-cadmium alloy can be used for the negative electrode current collector. In addition, the thickness of the negative electrode current collector can generally be about 3 μm to 500 μm, and similar to the positive electrode current collector, fine concave-convex can be formed on the surface of the current collector to enhance the binding force of the negative electrode active material. For example, the negative electrode current collector can be used in a variety of forms, such as films, sheets, foils, nets, porous materials, foams, and non-woven materials.

[0137] Together with the negative electrode active material, the negative electrode active material layer optionally contains a binder and a conductive material. As an example, the negative electrode active material layer can be manufactured by coating a composition for forming a negative electrode containing a negative electrode active material and an optional binder and a conductive material on a negative electrode current collector and drying, or by casting the composition for forming a negative electrode on a separate support and laminating a film obtained by peeling off from the support on the negative electrode current collector.

[0138] As for the negative electrode active material, a compound that allows reversible insertion and deinsertion of lithium can be used. Examples of the negative electrode active material may include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metal compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metal oxides capable of doping and dedoping lithium, such as SiO β (0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite material comprising a metal compound and a carbonaceous material, such as a Si-C composite material or a Sn-C composite material, any of which can be used alone, or a mixture of two or more of them can be used. In addition, a metallic lithium film can be used as a negative electrode active material. Regarding carbon materials, both low-crystalline carbon and high-crystalline carbon can be used. Typical examples of low-crystalline carbon can be soft carbon and hard carbon. Typical examples of high-crystalline carbon can be amorphous, planar, flaky, spherical or fibrous natural or artificial graphite, condensed graphite (Kish graphite), cracked carbon, carbon fiber based on mesophase pitch, mesophase carbon microbeads, mesophase pitch and high-temperature calcined carbon, such as coke derived from petroleum or coal tar pitch.

[0139] In addition, the binder and the conductive material may be the same as those described above for the positive electrode.

[0140] Meanwhile, a lithium secondary battery according to one aspect of the present disclosure includes the above-mentioned electrode structure.

[0141] The lithium secondary battery includes the above-mentioned electrode structure and an electrolyte. The electrolyte used in the present disclosure includes, for example, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes and molten inorganic electrolytes that can be used to manufacture lithium secondary batteries, but is not limited thereto.

[0142] According to one embodiment, the electrolyte may include an organic solvent and a lithium salt.

[0143] As for the organic solvent, any solvent can be used without particular limitation, as long as it can be used as a medium through which ions participating in the electrochemical reaction of the battery can move. For example, as for the organic solvent, an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone can be used; an ether-based solvent such as dibutyl ether or tetrahydrofuran; a ketone-based solvent such as cyclohexanone; an aromatic hydrocarbon-based solvent such as benzene or fluorobenzene; a carbonate-based solvent such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethylene carbonate (EC) or propylene carbonate (PC); an alcohol-based solvent such as ethanol or isopropanol; a nitrile such as R-CN (R is a linear, branched or cyclic C2 to C20 hydrocarbon group, which may contain a double bond aromatic ring or an ether bond); an amide such as dimethylformamide; a dioxolane such as 1,3-dioxolane; or cyclopentane sulfone. Among them, a carbonate-based solvent can be used, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) with high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a low-viscosity linear carbonate-based compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) can be used. In this case, when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.

[0144] Lithium salts can be used without particular limitation, as long as they are compounds that can provide lithium ions used in lithium secondary batteries. For example, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used for lithium salts. For example, the concentration of the lithium salt can be used in the range of about 0.1M to 2.0M. When the concentration of the lithium salt is within this range, since the electrolyte has appropriate conductivity and viscosity, it can exhibit excellent electrolyte performance and effectively move lithium ions.

[0145] In order to improve the life characteristics of the battery, suppress the reduction of the battery capacity and improve the discharge capacity of the battery, for example, in addition to the above electrolyte components, one or more additives may be further added, such as halogenated alkylene carbonate-based compounds, such as difluoroethylene carbonate; pyridine; triethyl phosphite; triethanolamine; cyclic ether; ethylenediamine; n-glyme; hexaphosphoric triamide; nitrobenzene derivatives; sulfur; quinone imine dyes; N-substituted Oxazolidinone; N,N-substituted imidazolidine; ethylene glycol dialkyl ether; ammonium salt; pyrrole; 2-methoxyethanol or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 wt % to 5 wt % based on the total weight of the electrolyte.

[0146] The lithium secondary battery according to the present disclosure may be used in the field of portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0147] Hereinafter, embodiments of the present disclosure will be described in detail so that those skilled in the art can easily implement the present disclosure. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein.

[0148] Example 1

[0149] [Preparation of aluminum hydroxide particles]

[0150] (1) Elution step

[0151] 100 g of bauxite that had been squeezed and pulverized into powder with a ball mill and a 40% concentration LiOH aqueous solution were added to a high pressure reactor and stirred at 200° C. for 1 hour to prepare an eluate. In this case, the content ratio of the added bauxite and LiOH was adjusted to 0.6.

[0152] (2) Precipitation step

[0153] The red mud in a solid form was filtered from the washing liquid, and then 40 g of ATH seed crystals were mixed with the separated solution, and the mixed solution was stirred at 80° C. for 1.5 hours. After the aluminum hydroxide seed crystals were filtered out therefrom, the filtrate was stirred at 50° C. for 12 hours or longer to prepare an ATH precipitate. The prepared ATH precipitate was washed with distilled water.

[0154] (3) Repeat steps

[0155] Instead of bauxite, the ATH precipitate obtained from step (2) is squeezed, crushed and added, and steps (1) and (2) are repeated. By these repeated steps, the content of Li and the content of other impurities can be adjusted.

[0156] (4) Crushing step

[0157] Distilled water was added to the ATH precipitate obtained by the above process so that the solid content of the ATH precipitate was about 40%, and the mixture was pulverized using a ball mill. In this case, 3 passes were performed with a bead size of 0.7 mm, a bead filling ratio of 75%, and a line speed of 700 rpm (the pulverization step was repeated 3 times). After the bead mill treatment, a slurry in which fine ATH particles were dispersed was obtained, and the obtained slurry was dried at 120° C. to obtain fine ATH particles.

[0158] The D50, BET, and Li content of the ATH obtained through the above process were measured and shown in Table 1.

[0159] [Manufacturing of separator]

[0160] 20 g of the ATH particles obtained by the above process, 1.0 g of a polyacrylic acid dispersant solution (solid content of 42 wt%) and 20 g of beads with a diameter of 0.5 mm for dispersion were added to 30.5 g of a dispersion mixed with water: ethanol at a weight ratio of about 95:5, and the dispersion was stirred for 2 hours using a paint shaker to prepare an ATH particle dispersion. Next, 0.24 g of a surfactant (FC4430, 3M Company, solid content of 90 wt%) and a water-dispersed particulate acrylic polymer (particle size 150 nm, Tg-25°C) were added to the ATH particle dispersion at a content of 40 wt%, and the dispersion was shaken to prepare a slurry for coating.

[0161] The prepared coating slurry was filtered through a 200 mesh filter, coated on one surface of a wet porous polyethylene membrane (SEMCORP, porosity 45%, thickness 9 μm) using a rod coater, then dried, and coated on the other surface of the membrane under the same conditions to produce a double-sided coated separator (a separator coated with slurry on both surfaces). The total thickness of the coating formed on both surfaces of the membrane after coating is presented in Table 1.

[0162] [Manufacturing of lithium secondary batteries]

[0163] (Manufacturing of positive electrode)

[0164] LiNi 0.8 Co 0.1 Mn 0.1 The O2 positive electrode active material, the carbon black conductive material, the binder and the dispersant (which is a mixture of PVDF-HFP copolymer and PVDF) are mixed with water in a weight ratio of 97.5:0.7:1.66:0.14 to prepare a slurry for forming a positive electrode active material layer in such a manner that the total content of the remaining components except water is 50% by weight. Next, the slurry is coated on an aluminum thin film current collector having a thickness of 10 μm and dried to manufacture a positive electrode having a positive electrode active material layer having a thickness of 120 μm formed therein.

[0165] (Manufacturing of negative electrode)

[0166] A graphite (a mixture of natural graphite and artificial graphite) negative electrode active material, a carbon black conductive material, a binder and a dispersant (which is a mixture of a PVDF-HFP copolymer and PVDF) were mixed with water in a weight ratio of 97.5:0.7:1.66:0.14 to prepare a slurry for forming a negative electrode active material layer in such a manner that the total content of the remaining components except water was 50% by weight. Next, the slurry was applied to a copper thin film current collector having a thickness of 10 μm and dried to manufacture a negative electrode having a negative electrode active material layer having a thickness of 120 μm formed therein.

[0167] (Manufacturing of single cells)

[0168] The separators manufactured by the above method were stacked and interposed between the positive electrode and the negative electrode, and the side surfaces thereof were fixed with a polyimide tape to manufacture a single cell electrode assembly.

[0169] (Manufacturing of lithium secondary batteries)

[0170] A lithium secondary battery was manufactured by injecting an electrolyte solution in which 1 M of LiPF 6 was dissolved in a solvent mixed in a volume ratio of ethylene carbonate / ethyl methyl carbonate=3:7 into a single cell.

[0171] Example 2

[0172] Example 2 was performed in the same manner as Example 1, except that in the (4) pulverization step in [Preparation of ATH particles], the bead size was changed to 1 mm and performed 2 times in total (the pulverization step was repeated twice).

[0173] Example 3

[0174] Example 3 was carried out in the same manner as Example 2, except that the repetition step (3) in [Preparation of ATH particles] was omitted.

[0175] Comparative Example 1

[0176] Comparative Example 1 was conducted in the same manner as Example 2, except that an aqueous NaOH solution was used in place of an aqueous LiOH solution in the elution step (1) during the repetition of step (3) in [Preparation of ATH particles].

[0177] Comparative Example 2

[0178] Comparative Example 2 was prepared in the same manner as Example 1, except that during the (1) elution step in [Preparation of ATH particles], an aqueous NaOH solution was used instead of an aqueous LiOH solution.

[0179] Comparative Example 3

[0180] Comparative Example 3 was prepared in the same manner as Example 2, except that during the (1) elution step in [Preparation of ATH particles], an aqueous NaOH solution was used instead of an aqueous LiOH solution.

[0181] D50 measurement method of aluminum hydroxide particles

[0182] The D50 of the ATH particles was measured using a laser diffraction method by placing the ATH particles in a wet particle size analysis device (Mastersizer 3000, Malvern Company).

[0183] BET Measurement Method for Aluminum Hydroxide Particles

[0184] The BET of the ATH particles was measured from the amount of adsorbed nitrogen using a BET analysis device (BELSORP-mini II, BEL Corporation).

[0185] Measurement method of Li content in aluminum hydroxide particles

[0186] About 0.1 g of ATH particles were placed in a Corning tube to measure the weight. Subsequently, 1.5 mL of concentrated hydrochloric acid and 0.2 mL of hydrogen peroxide were added to the ATH particles and shaken well to mix, and then eluted by boiling the mixture in boiling water (at 130° C. for 4 hours or more).

[0187] Next, the eluted product was cooled to room temperature, and then 200 μL of hydrofluoric acid was added thereto, and the resultant material was sealed and reacted at room temperature for 3 hours.

[0188] Then, 1 mL of boric acid and 0.2 mL of an internal standard substance (Sc, scandium) were added to the reaction product, and diluted with 20 mL of ultrapure water.

[0189] A sample was prepared by filtering the diluted resultant using a 0.45 μm filter.

[0190] The Li and Na contents in the ATH particles were measured using an ICP-OES instrument (OPTIMA 5300OV, Perkin Elmer).

[0191] Thermal shrinkage measurement method

[0192] The manufactured separators of Examples and Comparative Examples were placed in an oven at 150° C. for 30 minutes, and then their heat shrinkage rates were measured.

[0193] The heat shrinkage rate was obtained by marking two arbitrary points in the machine direction (MD) and transverse direction (TD) of the separator and calculating the rate of change (variance) of the distance (gauge distance) between the two points according to the following equation 1,

[0194] (Equation 1)

[0195] Thermal shrinkage (%) = {(BA) / A}X100

[0196] In Equation 1, A is the gauge distance before the separator is placed at the high temperature, and B is the gauge distance after the separator is placed at the high temperature for 30 minutes.

[0197] Capacity retention rate measurement method

[0198] The lithium secondary batteries of the embodiments and comparative examples manufactured by the above method are repeatedly charged and discharged at a rate of 1C (current) in the range of 2.5V to 4.25V at 25°C, and the ratio of the discharge capacity after 200 cycles to the initial discharge capacity is calculated to measure the capacity retention rate. Here, 1C is a unit that defines the charge and discharge rate of a secondary battery, and means the rate at which the battery is fully charged or fully discharged when charged or discharged for one hour. For example, when the capacity of the secondary battery is 1000mA, when the secondary battery is fully charged within one hour, it can be considered to be charged at a rate of 1C, and when the secondary battery is fully charged within 30 minutes, it can be considered to be charged at a rate of 2C.

[0199] [Table 1]

[0200]

[0201] As seen in Table 1, it can be determined that in Examples 1 to 3 to which the present disclosure is applied, the capacity retention rates are 96%, 95%, and 93%, respectively, which are significantly improved compared to 88%, 86%, and 83% of the comparative example.

[0202] Although the present disclosure has been described above with reference to preferred embodiments, it will be appreciated by those skilled in the art or those with ordinary knowledge in the relevant technical field that various embodiments of the present disclosure are described herein for illustrative purposes, and various modifications and changes may be made without departing from the scope and spirit of the present disclosure. Therefore, the various embodiments disclosed herein are not intended to be limiting, and the true scope and spirit are indicated by the appended claims.

Claims

1. Aluminum hydroxide particles comprising a D50 of about 3.0 μm or less, a 2 / g or more BET, and a Li content of about 500 ppm or more.

2. The aluminum hydroxide particles according to claim 1, wherein the particles have a D50 of about 2.5 μm or less and a BET of about 3.5 μm. 2 / g or more, and the Li content is about 800 ppm or more.

3. The aluminum hydroxide particles of claim 1, wherein the particles have a D50 of about 2.7 μm or less and a BET of about 3.8 μm. 2 / g or more, and the Li content is about 900 ppm or more.

4. The aluminum hydroxide particles of claim 1, wherein the particles have a D50 of about 2.2 μm or less and a BET of about 4.2 μm. 2 / g or more, and the Li content is about 1050 ppm or more.

5. The aluminum hydroxide particles according to claim 1, wherein the Na content is about 900 ppm or less.

6. The aluminum hydroxide particles according to claim 1, wherein the Na content is about 100 ppm or less.

7. The aluminum hydroxide particles according to claim 1, wherein the Na content is about 10 ppm or less.

8. A method for preparing aluminum hydroxide particles, the preparation method comprising: (S1) obtaining an eluate by adding bauxite to an alkaline aqueous solution containing Li; (S2) separating the eluate obtained in (S1) by filtering solids from the eluate; and (S3) separating aluminum hydroxide from the separated eluate, The aluminum hydroxide particles have a D50 of about 3.0 μm or less, a 2 / g or more BET and a lithium (Li) content of about 500 ppm or more. 9 . The preparation method according to claim 8 , wherein the alkaline aqueous solution containing Li is LiOH.

10. The preparation method according to claim 8, further comprising: Prior to (S3), aluminum hydroxide seed crystals are added to the separated eluate, the eluate is stirred, and then the aluminum hydroxide seed crystals are filtered to separate the eluate again.

11. The production method according to claim 8, wherein the aluminum hydroxide precipitated from (S3) is pulverized, and then the pulverized aluminum hydroxide is added to (S1) instead of the bauxite to repeat (S1) to (S3).

12. A separator, comprising: A porous polymer film or a porous polymer nonwoven fabric; and an organic-inorganic composite coating layer formed on at least one surface of the porous polymer film and comprising a mixture of inorganic particles and a polymer, The inorganic particles include the aluminum hydroxide particles according to claim 1.

13. A separator comprising a self-supporting organic-inorganic composite film comprising a mixture of inorganic particles and a polymer, The inorganic particles include the aluminum hydroxide particles according to claim 1.

14. An electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, The separator is according to claim 12.

15. An electrode assembly comprising: positive electrode; negative electrode; as well as a separator interposed between the positive electrode and the negative electrode, The separator is according to claim 13.

16. An electrode assembly comprising a separator formed on at least one surface of a positive electrode, a negative electrode, or both of the positive electrode and the negative electrode and comprising a porous organic-inorganic composite coating layer of a mixture of inorganic particles and a binder polymer, The inorganic particles include the aluminum hydroxide particles according to claim 1. 17 . A lithium secondary battery comprising the electrode assembly according to claim 14 .

18. A lithium secondary battery comprising the electrode assembly according to claim 15.

19. A lithium secondary battery comprising the electrode assembly according to claim 16.