Method for obtaining nickel concentrate, method for processing nickel concentrate and method for recovering material derived from nickel ore

Through the scrubbing, magnetic sorting and hydrochloric acid heating of laterite nickel ore, combined with microwave radiation assisted leaching, the problems of resource waste and environmental pollution in laterite nickel ore are solved, efficient nickel and cobalt recycling is achieved, and CO2 emissions are reduced. Improve resource utilization.

CN119013424APending Publication Date: 2024-11-22HIPPUDIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033850.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-14
Filing Date
2023-02-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art cannot efficiently recover high-purity nickel and other economically related materials from laterite nickel mines, resulting in waste of resources and environmental pollution, and reliance on fossil source heating leads to high CO2 emissions.

Method used

Through steps such as scrubbing, magnetic sorting, grinding and hydrochloric acid heating, nickel concentrate is obtained, and microwave radiation assisted leaching and hydrochloric acid regeneration are used to improve the conversion of soluble chloride form of nickel and cobalt, reduce the formation of insoluble oxides of iron, and achieve the realization of High-efficiency chemical processing of nickel concentrate.

Benefits of technology

It realizes efficient recycling of resources in laterite nickel mineral areas, reduces the use of fossil source heating, reduces CO2 emissions, improves the recovery of nickel and cobalt, promotes the extraction of magnesium and other materials, improves resource utilization and environmental friendliness sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013424A_ABST
    Figure CN119013424A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for recovering material derived from nickel ore, which relates to a method for obtaining a nickel concentrate and a method for processing said concentrate, whereby a nickel ore can be processed in an efficient and ecological manner and it is possible to recover material and residues that have not been developed currently from the nickel ore.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for recovering material derived from nickel originating from supergene alteration, to a process for obtaining a nickel concentrate and to a process for processing said concentrate.

[0002] By means of the invention, ecological and economic benefits and advantages can be obtained, in particular:

[0003] (i) enabling the recovery of currently unexploited materials and nickel ores from the nickel, significantly reducing waste discharged into the environment;

[0004] (ii) reduce the use of heating from fossil sources, thereby reducing CO2 emissions typical of this type of process;

[0005] (iii) Recover economically relevant materials in line with the new reality of the circular economy. Background Art

[0006] Nickel is an essential strategic metal in the construction of stainless steel. Nickel is also strategic in battery technology along with iron phosphate, and in the production of medical devices, wind turbines, special steel alloys and other applications.

[0007] Today, more than two thirds of the nickel market is related to the production of steel and steel alloys (Type II nickel) and less than one third is related to the production of high-purity derivatives with a minimum purity of 99.0% (Type I nickel), the latter being a key metal in the development of the energy sector, which is constrained by bottlenecks in energy storage and shows high growth as the energy matrix changes from fossil fuels to renewable energy sources.

[0008] Known nickel deposits come from laterites, sulfates, and seafloor magnesium nodules, which are large but unsuitable for mining. The former two are later used as raw materials for the production of nickel and nickel alloys.

[0009] Sulfate nickel deposits are of volcanic and hydrothermal origin and, because the nickel is sulfated, this type of ore is easily processed by conventional flotation. In contrast, sulfate nickel deposits account for approximately 30% to 40% of the world's nickel reserves that can be processed.

[0010] Laterite nickel ore deposits account for 60% to 70% of the world's reserves, which means that laterite ore is the most relevant source for processing.

[0011] For practical grouping purposes for processing, laterite nickel ore deposits can generally be divided into four zones: Zone 1, red laterite, which has a lower nickel content (0.5% to 0.8% Ni); Zone 2, yellow laterite, which has a larger nickel content (0.8% to 1.2% Ni); Zone 3, which transitions to saprolite, with an even greater nickel content (1.2% to more than 2% Ni); and Zone 4, saprolite, which has a nickel content of more than 1.5% and a different magnesium and iron composition than Zone 3.

[0012] Different types of processing are carried out on these deposits, mainly as follows: Hydrometallurgical processing methods such as High Pressure Acid Leaching (HPAL) and Caron process are used on the first 3 zones. And zone 4 (saprolite) is used in pyrometallurgical process to produce metallic ferronickel.

[0013] The formation of nickel deposits by lateritization involves the combination and interaction of various geological and environmental factors. It begins with the intrusion and serpentinization of ultramafic rock bodies, which are subsequently exposed and subjected to tropical humid climates by tectonic events and / or erosional methods, which promote the development of deep and strongly weathered regoliths. During this stage, nickel is concentrated in goethite and / or montmorillonite in the form of residues due to the strong dissolution of magnesium and silicon from the original rock. This is where the iron laterite layers of red (LV) and yellow (LM) limonite develop. Next, most deposits are subjected to tectonic events and climate change. In these less variable places, the deposits may have been buried, or in more arid climates, weathering is weakened and the deposits are preserved. When uplift is significant, erosion losses may increase, but under the effect of humid climates and deeper groundwater levels, erosion losses are offset by continued weathering and the enrichment of nickel migrated from the upper part of the profile in the newly formed magnesium silicate hydrates, thereby forming a deeper mineralized saprolite layer. This process allows ions with greater mobility to remain in solution, resulting in an oxidized layer of the ore bed enriched in minerals of interest, such as nickel and cobalt, which precipitate as fine particles and cover other particles of the ore bed, including some nickel- and cobalt-rich particles, such as olivine.

[0014] To improve understanding, Figure 1 A schematic diagram of the laterite zone is disclosed, which includes an area A1 representing the ferrous part near the surface, an area A2 representing the oxidized part (red and yellow limonite), and an area A3 representing the saprolitic zone. It should be emphasized that the laterite zone is not fully utilized or completely ignored by the ferro-nickel production companies, being considered below the plant feed specifications or undevelopable. In this sense, 52% of the world's nickel production is concentrated in sulfate ores and 48% in laterite ores. Laterite ores are mainly used for the production of nickel pig iron (NPI) and ferro-nickel, and the part used for this purpose is found in the saprolitic zone.

[0015] Of the world's laterite reserves, only 5% to 8% of laterite areas are used to produce Type I nickel (primarily by the HPAL process).

[0016] It is noteworthy that the main known methods for processing laterite nickel ores are the Caron process and the High Pressure Acid Leaching (HPAL) process and these processes are unable to use the saprolite zone of the deposit.

[0017] In fact, the Caron process is economically and environmentally disadvantageous because it requires high production and operating costs in addition to its high carbon dioxide (CO2) emissions.

[0018] In contrast, the commonly used HPAL process can generally be described as a high pressure acid leaching process, which uses high temperatures (about 255 degrees Celsius) and high pressures (about 50 bar or 725 psi) in addition to sulfuric acid to separate nickel and cobalt from laterite ores.

[0019] Here are some of the problems with prior art associated with extracting nickel from laterite areas:

[0020] Currently known methods cannot process the iron part A1 of the laterite nickel zone (above the oxidized part of the red and yellow limonite). This means that the iron part A1 is used by the industry operating the laterite nickel zone. 1 are considered waste / residues and are simply stored indefinitely (via dry stacking or “dry stacking”), leading to serious ecological problems and high operational losses.

[0021] Furthermore, the saprolite fraction A3 of the laterite zone is currently used only to extract Class II nickel (ferronickel), which is a reduced purity nickel used primarily for the production of stainless steel. There are currently no known processes that enable the recovery of high purity Class I nickel from the saprolite fraction A3 of the laterite nickel zone, which means that at least a portion of this saprolite fraction is being used by the industry. 2 Treated as a residue / waste of the process, it is also simply deposited in post-processing and causes ecological problems and operational losses.

[0022] Furthermore, none of the methods currently known in the prior art can efficiently extract other materials of interest from laterite areas, being limited to the extraction of Class I or Class II nickel. Laterite areas are known to have other economically relevant materials (such as magnesium for example), but these materials cannot be extracted by currently known methods, so that they are discarded or dumped after processing the residue / waste.

[0023] It is further emphasized that the oxidized fraction A2 of the laterite area can currently only be processed by processes for the extraction of nickel hydroxide and cobalt, such as HPAL and CARON. Said processes cannot process the saprolite fraction A3 of the laterite area. Said processes also cannot process the nickel fraction rich in magnesium, since extraction is not feasible from an economic point of view.

[0024] It is also important to note that there are currently no methods that are able to extract materials of interest from the oxidic fraction A2 and the saprolite fraction A3 of the laterite zone. 3 An attempt has been made to apply the "heap leaching" method to the oxidic and saprolitic fractions, but this method is costly and inconvenient to operate because it requires the depositing of large amounts of material and leaching by percolation. This method also does not allow the treatment of the upper iron fraction A1 of the laterite zone.

[0025] As regards the residues / wastes themselves, the processes known in the prior art generate at least three types of residues / wastes:

[0026] (A) The first type of residue / waste is the upper ferrous part A1 of the laterite zone itself, since none of the known methods can operate efficiently on this part.

[0027] (B) The third type of residue / waste is the rest of the interesting materials from the oxidized portion A2 of the laterite area, since currently existing processes (e.g. HPAL, CARON) cannot extract any materials other than Class I nickel from the laterite area. Therefore, other economically interesting materials (e.g. magnesium) are discarded.

[0028] (C) The second type of residue / waste is the remainder from processing the saprolite fraction A3 processed for the production of Class II nickel. Since known hydrometallurgical processes are not capable of extracting Class I nickel from the saprolite fraction of the laterite zone, the remainder of the material of interest from this fraction is discarded at the end of the process.

[0029] Based on the above explanation, another problem is noted in the prior art, namely, the use of heat from polluting sources such as coal, the combustion of which produces CO2, which is known to be harmful to the environment.

[0030] Additionally, another problem has been noted in the prior art, namely, the use of sulfuric acid in the process of recovering materials derived from nickel ore, thereby producing contaminated residues, contrary to the process of the present patent.

[0031] In this type of process, sulfuric acid has a low selectivity for leaching and its relatively low vapor pressure prevents its regeneration in these processes and requires neutralization and subsequent treatment for its disposal.

[0032] References

[0033] 1. Carolina das Graciano. Tecnológica de Minério de Niquel Laterítico. Orientador: Leandro Rocha Lemos. 2019 (Mestrado em Engenharia Metalúrgica,Materiais e de Minas)-UNIVERSIDADEFEDERAL DE MINAS GERAIS,[Sl],2019.

[0034] 2.DA COSTA, Paulo Rodrigues. da escória de ferro-niquelpara como enrocamento de diques galgáveis ​​drenantes.Orientador:Gilberto Fernandes.2019. (Mestrado em Geotecnia)-Universidade Federal de Ouro Preto,Ouro Perto,2019.

[0035] 3. OXLEY, Anne et al. Why heap leach nickel laterites? Minerals Engineering, [Sl], pp. 1-8, 15 Mar. 2016.

[0036] Purpose of the Invention

[0037] Therefore, a first object of the present invention is to provide a method related to the processing of nickel ores, including the saprolitic fraction, so as to enable the recovery of marginal ores from ferronickel producing ores, as well as materials not currently exploited from deposits of this type, thus enabling the use of this part of the deposit. Companies producing ferronickel deposit this laterite fraction and mainly use the saprolitic fraction of the deposit.

[0038] A second object of the present invention is to provide methods related to nickel ore processing which, compared with the prior art, allow a reduction in the use of heating of fossil origin, thereby reducing the CO2 emissions typical of methods of this type.

[0039] A third object of the present invention is to provide methods related to nickel ore processing which enable the recovery of economically relevant materials.

[0040] A fourth object of the present invention is to provide a method for obtaining a nickel concentrate comprising suitable characteristics to enable subsequent efficient chemical processing.

[0041] A fifth object of the present invention is to provide an improved method of processing nickel ore starting from nickel concentrate by specific steps to increase the efficiency of the process.

[0042] A sixth object of the present invention is to provide a method of processing nickel concentrate for recovery of strategic materials such as, but not exclusively, iron phosphate (FePO4) and nickel and cobalt hydroxide (HNC) or commercially known as mixed hydroxide precipitate (MHP). Summary of the invention

[0043] The present invention relates to a method for obtaining a nickel concentrate, the method comprising the steps of: scrubbing the nickel ore; sorting the nickel ore into at least one fine fraction and one coarse fraction by size; magnetically sorting the coarse fraction to obtain a magnetic fraction; grinding the magnetic fraction to obtain a fine magnetic fraction; and combining the fine fraction with the fine magnetic fraction to obtain a nickel concentrate.

[0044] In one possible embodiment of the method for obtaining a nickel concentrate, the scrubbing step is performed using a twin-rotor mill, a rod mill or a scrubber-type device.

[0045] In another possible embodiment of the method for obtaining a nickel concentrate, the scrubbing step is carried out for between 2 and 50 minutes.

[0046] In another possible embodiment of the method for obtaining a nickel concentrate, the size sorting step obtains a fine fraction with a particle size of less than 75 μm and a coarse fraction with a particle size of more than 75 μm.

[0047] In another possible embodiment of the method for obtaining nickel concentrate, the method comprises a comminution step which is carried out until the size of the processed material is below 2".

[0048] The present invention further includes a method for processing nickel concentrate, which method includes the steps of: mixing the nickel concentrate with hydrochloric acid; heating the nickel concentrate until more than 90% of the nickel and cobalt contained in the nickel concentrate are converted into their soluble chloride forms, and until the desired conversion of the iron, chromium and titanium contained in the nickel concentrate into their insoluble oxide forms is achieved; leaching the nickel concentrate with water to dissolve the nickel and cobalt contained in the nickel concentrate; and obtaining a liquor rich in nickel, cobalt, iron and magnesium.

[0049] In one possible embodiment of the method for processing nickel concentrate, the heating step is performed by microwave radiation.

[0050] In one possible embodiment of the method for processing nickel concentrate, the leaching step is assisted by microwave radiation.

[0051] In another possible embodiment of the method for processing nickel concentrate, the method comprises a step of regenerating the hydrochloric acid used in the first leaching step by evaporating the hydrochloric acid in the heating step, condensing the hydrochloric acid vapor, and returning the condensed hydrochloric acid to the leaching step.

[0052] In another possible embodiment of the method for processing nickel concentrate, the first leaching step comprises adding 0.1 to 5 ml / g of hydrochloric acid per gram of nickel concentrate.

[0053] In another possible embodiment of the method of processing nickel concentrate, the heating step comprises heating for a period of time ranging from 15 to 30 minutes.

[0054] In another possible embodiment of the method for processing nickel concentrate, the second leaching step comprises microwave irradiation at a temperature between 20°C and 60°C.

[0055] In another possible embodiment of the method for processing nickel concentrate, the method comprises a filtering step of the liquor in order to obtain an insoluble oxide form containing iron, chromium and titanium.

[0056] In another possible embodiment of the method for processing nickel concentrate, the method comprises a precipitation step for extracting the iron contained in the LI liquor, which step is carried out by adding at least one phosphate source to the liquor in a stoichiometric ratio.

[0057] In another possible embodiment of the method for processing nickel concentrate, the method comprises the following steps: using MnO2 and KMnO4 to precipitate the manganese product of the precipitation step (240) for extracting iron contained in the LI liquor; and precipitating MHP, adding magnesium oxide.

[0058] In another possible embodiment of the method for processing nickel concentrate, the method comprises the steps of: adding a solvent to the liquor to obtain a liquor mainly comprising nickel and cobalt; stripping the solvent by adding hydrochloric acid to the liquor; and returning the solvent to the extraction step.

[0059] In another possible embodiment of the method for processing nickel concentrate, the method comprises the step of adding magnesium oxide to the liquor to obtain nickel hydroxide and cobalt.

[0060] In another possible embodiment of the method for processing nickel concentrate, the method comprises a step of thermal hydrolysis of the liquor for extracting magnesium oxide and hydrochloric acid.

[0061] In another possible embodiment of the method for processing nickel concentrate, the method comprises the steps of: mixing a coarse magnetic fraction rich in chromium with H2O2; and irradiating the mixture by microwaves for a time required to convert more than 90% of the chromium phase into sodium chromate.

[0062] The present invention further includes a method for recovering nickel ore derivatives, which includes the steps of the method for obtaining nickel concentrate as mentioned above in any one of its feasible embodiments, and further includes the steps of the method for processing nickel concentrate as mentioned above in any one of its feasible embodiments.

[0063] BRIEF DESCRIPTION OF THE DRAWINGS

[0064] The accompanying drawings show:

[0065] Figure 1 - is a schematic representation of a laterite zone divided into a ferruginous part A1, an oxidic part A2 and a saprolite part A3.

[0066] Figure 2 - is a flow chart of a method for obtaining nickel concentrate according to a feasible embodiment of the present invention;

[0067] Figure 3 - is a flow chart of a method for processing nickel concentrate according to another possible embodiment of the present invention;

[0068] Figure 4 - is a first graph relating to the recovery of iron (%) obtained by the process of the invention as a function of the amount of hydrochloric acid used (in L / kg) and the microwave irradiation time (in minutes); and

[0069] Figure 5 - is a second graph relating to the nickel recovery (%) obtained by the process of the invention as a function of the amount of hydrochloric acid used (in L / kg) and the microwave irradiation time (in minutes).

[0070] Figure 6 - is a third graph relating to the recovery of iron (%) obtained by the process of the invention as a function of the amount of hydrochloric acid used (in L / kg) and the microwave irradiation time (in minutes).

[0071] Figure 7 - is a fourth graph relating to the nickel recovery (%) obtained by the process of the present invention, which is related to the amount of hydrochloric acid used (in L / kg) and the microwave irradiation time (in minutes).

[0072] Detailed description with drawings

[0073] First, it should be emphasized that the term "preferred" used herein should not be understood as "necessary" or "mandatory". The term "preferred" is intended to describe an embodiment of the present invention that has a specific efficiency among multiple feasible embodiments, and the scope of the present invention is limited only by the features that are absolutely necessary to obtain the proposed technical effect.

[0074] For the purpose of understanding the present invention, the term "nickel ore" should be understood as any source of nickel, natural or otherwise, pure or pre-processed, unsulfated.

[0075] The present invention proposes methods for recovering materials derived from nickel ores, which methods involve obtaining a nickel concentrate and processing the concentrate to recover the material of interest.

[0076] Regarding the method for obtaining nickel concentrate, a possible implementation method is described below:

[0077] Method for obtaining nickel concentrate

[0078] Regarding obtaining nickel concentrate, in one possible implementation, the method discussed generally but not necessarily comprises the following steps:

[0079] - Optionally, perform a preliminary processing step 100A;

[0080] - Optionally, drying, crushing and grinding the nickel ore 100B;

[0081] - Dry or wet scrubbing of nickel ore 100;

[0082] - size sorting 110 the nickel ore into at least one fine fraction FF and one coarse fraction CF;

[0083] - magnetically separating 120 the coarse fraction CF to obtain a magnetic fraction MF,

[0084] - scrubbing 130 the coarse fraction CF to obtain a fine magnetic fraction FMF; and

[0085] - combining 140 the fine fraction FF with the fine magnetic fraction FMF to obtain a nickel concentrate NOC.

[0086] The details of each of these steps are described below:

[0087] Initial processing steps:

[0088] In one possible embodiment, and optionally, preliminary processing steps 100A may be used, such as feeding nickel ore into a feed bin, and other steps necessary to prepare the logistics of the material for subsequent steps.

[0089] Drying and crushing:

[0090] In a possible embodiment, and optionally, the use may consist of a drying and comminution 100B step of the nickel ore, the purpose of which is to obtain particles with a uniform particle size, which facilitates the subsequent processing of the material. The comminution may be carried out, for example, by means of a mineral screener or a cone-type crusher. The grinding may be carried out, for example, in a rod mill or a double roller mill. The crushing 100B is preferably carried out until the size of the processed material is less than 2", preferably reaching a range of less than 1 / 4".

[0091] The ore is then ready for a scrubbing step 100 .

[0092] Scrubbing steps:

[0093] The purpose of the scrubbing step 100 is mainly to break up the crust of silicate minerals encapsulating nickel and the nickel-iron agglomerate of the mining product, thereby making it possible to obtain nickel-containing particles with a large surface area, which is beneficial for the subsequent processing of the material, effectively enriching the nickel content contained in the fine-grained fraction of the nickel ore.

[0094] In other words, the scrubbing step 100 advantageously decomposes the ore particles, which are chemically precipitated materials due to surface alteration and are essentially composed of goethite, in addition to cleaning them from the surface. These fine particles, which are generated by chemical precipitation, accumulate on the surface of larger particles and are released by scrubbing, will be concentrated into the finer fraction of the ore. This step makes the finer iron fraction suitable for leaching and the coarse fraction ready for magnetic separation because the mineral surfaces of these coarse particles will be clean. This is crucial so that both the leaching and magnetic separation processes occur with high efficiency.

[0095] In short, after this cleaning and size sorting by scrubbing 100, the nickel-containing ore particles have a larger surface area, thereby advantageously facilitating their subsequent processing. In addition, the coarse fraction is free of these particles, thereby achieving efficient magnetic sorting thereof.

[0096] For illustrative purposes, the following Tables 1 to 4 show comparative tests between the increase in scrubbing time (scrubbing step 100) and the nickel content of the fine fraction obtained:

[0097]

[0098]

[0099]

[0100]

[0101]

[0102] Tables 1 to 4 - Comparison between increase in scrubbing time (5 minutes, 20 minutes) and nickel content of the fine fraction obtained.

[0103] In the above table, from those samples subjected to scrub 100, the contents of all oxidation profiles classified by zones (named Zone 1, Zone 2, Zone 3, and Zone 4, respectively, in Table 5) increased with increasing scrub exposure time.

[0104] In this sense, scrubbing 100 releases and concentrates the chemically deposited iron material covering the particles and the nickel-containing mineral particles covering other particles into the fine fraction FF. In addition, it is important to note that the concentration of nickel in the fine fraction FF by extracting fine particles rich in goethite and nickel is also caused by the crystallization stage of goethite. The lower the crystallinity (the crystal structure is immature and more open), the greater the tendency to absorb Ni in the structure, so scrubbing will tend to decompose these younger and brittle goethites, which are concentrated in the fines and carry a larger amount of nickel in their structure. In contrast, in the upper more mature layer, goethite undergoes various dissolution and recrystallization stages ("aging"), which tend to expel nickel from the structure, thereby forming crystalline goethite with a lower nickel content.

[0105] It was observed that the distribution of nickel in all fractions tested increased in the fine fraction FF with increasing exposure time to the scrubbing device. The following table shows the mineral composition of nickel ore in the fine fraction after 20 minutes of scrubbing, where a considerable concentration of goethite containing iron and nickel can be observed:

[0106]

[0107] Table 5 - Mineral composition of nickel ore after 20 minutes of scrubbing

[0108] Preferably, scrubbing 100 with shear force should occur for between 2 and 50 minutes, more preferably between 10 and 25 minutes. The scrubbing 100 may occur in equipment such as a twin rotor mill, a rod mill or a scrubber.

[0109] After scrubbing 100, the method continues with the step of sorting by size 110, as described above.

[0110] Steps for sorting by size:

[0111] The purpose of the size sorting step 110 is to perform a particle size cut in the material subjected to scrubbing 100 so that the material can be sorted into a fine fraction FF and a coarse fraction CF, and then to sort the magnetic fraction MF from the coarse fraction CF of the material, with the aim of obtaining a magnetic fraction for subsequent chemical treatment and a non-magnetic fraction rich in PGM and rare earths.

[0112] More specifically, the size sorting step 110 is preferably carried out by an air cyclone or a hydrocyclone device, depending on the dry or wet processing situation. The size sorting device is configured to sort a fine fraction FF from a coarse fraction CF of the fed material. Preferably, the sorting that occurs in the cyclone device sorts the material into a fine fraction FF with a size of less than 75 μm, preferably less than 30 μm and more preferably less than 20 μm, and into a coarse fraction CF with a size of greater than 75 μm, preferably greater than 30 μm and more preferably greater than 20 μm.

[0113] After sorting the fine fraction FF and the coarse fraction CF from the material, the fine fraction FF is sorted for subsequent chemical processing and the coarse fraction CF continues to the magnetic sorting step, as described above.

[0114] Magnetic separation steps:

[0115] The purpose of the magnetic sorting step 120 is to sort the magnetic fraction MF from the coarse fraction CF obtained in the size sorting step 110 so that the magnetic fraction MF extracted from the coarse fraction CF can be subsequently chemically processed together with the fine fraction FF extracted in the size sorting step 110 .

[0116] The magnetic separation is preferably carried out, for example, by means of a magnetic separator metso or outotec.

[0117] The non-magnetic fraction NMF extracted by the magnetic separator is withdrawn from the process of the invention. However, it is important to note that the non-magnetic fraction NMF is mainly represented by silicates and may also include PGMs (gold, silver and platinum group metals) and rare earths, which advantageously show the potential for processing by a parallel process.

[0118] The magnetic fraction MF extracted from the coarse fraction CF by the magnetic separator is then continued to the scrubbing step 130 as described above.

[0119] Grinding steps of magnetic fraction:

[0120] The magnetic fraction MF extracted in the magnetic sorting step 120 is directed to a crushing device such as a ball mill to undergo a grinding step 130 to below 150 μm, more preferably below 75 μm and even more preferably below 20 μm.

[0121] The purpose of said step is to reduce the particle size of the magnetic fraction MF, preferably to a size less than 20 μm, consistent with the fraction FF obtained in the scrubbing step 100 , thereby obtaining a fine magnetic fraction FMF for subsequent combination with the fine fraction FF obtained in the size sorting step 110 .

[0122] After obtaining the fine magnetic fraction FMF, the next step is to combine it with the fine fraction FF, as described above.

[0123] If the magnetic fraction is rich in Cr2O3 originating from chromite or iron spinel, the magnetic fraction can also be processed using microwave radiation. In this case, the coarse-grained magnetic fraction rich in chromium is mixed with NaOH in a stoichiometric ratio of between 100% and 200% m / m, preferably between 110% and 150% m / m, even more preferably between 125% and 135% m / m, and a stoichiometric amount of H2O2 relative to chromium of 100% to 200% m / m, more preferably between 150% and 180% m / m, and heated with microwaves for the time required to convert more than 90% of the chromium phase into sodium chromate, preferably for a time of between 2 and 15 minutes and more preferably for a time of between 3 and 5 minutes, following the following equation:

[0124]

[0125] The sodium chromate in solution can then be filtered and separated from the rest of the coarse magnetic fraction.

[0126] Steps for combining the fine magnetic fraction with the fine fraction:

[0127] In this combined step 140 , the fine magnetic fraction FMF is added to the fine fraction FF to form a final material (hereinafter referred to as “nickel concentrate” NOC) which can be chemically processed as seen previously.

[0128] The two fractions, fines FF and magnetic fines FMF, may be combined by any suitable means including simple mechanical mixing of the two.

[0129] Moreover, the nickel concentrate represents approximately 60% of the volume of the initial nickel ore, which in itself already implies a high sorting efficiency of the material actually of interest for subsequent processing, despite neglecting the non-magnetic fraction extracted from the process, which can moreover subsequently be exploited by other processes for other equally interesting materials it may contain.

[0130] In view of the above, the method for obtaining nickel concentrate proposed in this article advantageously produces a nickel concentrate in which the nickel-rich ore particles have a large surface area because goethite (FeO(OH)) and hematite (Fe2O3) and other nickel-containing minerals are mainly decomposed from the ore particles, which ensures a nickel concentrate that is particularly desirable for subsequent high-efficiency chemical processing.

[0131] After presenting a possible embodiment of the method for obtaining nickel concentrate NOC, the present invention also relates to a processing method of nickel concentrate for obtaining derivatives of interest, which processing method will be explained in further detail below.

[0132] Method for processing nickel concentrate

[0133] Regarding processing nickel concentrate to obtain a LI-rich liquid, in one possible embodiment, the method discussed generally but not necessarily comprises the following steps:

[0134] - Mixing nickel concentrate NOC with hydrochloric acid 200;

[0135] - heating or irradiating 210 the nickel concentrate NOC until the desired conversion of the nickel and cobalt contained in the nickel concentrate into the form of their soluble chlorides is achieved, and until the desired conversion of the iron, chromium and titanium contained in the nickel concentrate into the form of their insoluble oxides is achieved;

[0136] - optionally, regenerating 210A the hydrochloric acid used in the previous leaching step 200 by evaporating said hydrochloric acid in a heating or irradiation step 210 and subsequently condensing it and returning it to the leaching step 200; and

[0137] - leaching 220 the nickel concentrate NOC with water to dissolve the nickel and cobalt contained in the nickel concentrate NOC, the leaching optionally being assisted by microwave radiation; and

[0138] - Obtain 230 LI liquid mainly rich in nickel, cobalt, iron, manganese and magnesium.

[0139] The above-mentioned steps will be described in detail below.

[0140] Steps for mixing nickel concentrate with hydrochloric acid

[0141] The mixing step 200 involves mixing the nickel concentrate with hydrochloric acid, for example in a ribbon blender or pug-mill type device, or in any device that likewise homogeneously mixes liquids with solids.

[0142] It is very important to emphasize that the use of applied hydrochloric acid for blending nickel concentrates proves to be more efficient and more advantageous than the use of sulfuric acid commonly used in the prior art for at least the following reasons:

[0143] (i) Compared with other methods, the hybrid method proposed herein requires less hydrochloric acid to prepare hydrochloric acid concentrate; and

[0144] (ii) The vapour pressure of hydrochloric acid is relatively greater than that of sulphuric acid, which is beneficial for the process proposed herein because it enables the regeneration of hydrochloric acid to be facilitated and its use in a cyclic manner, as will be seen below.

[0145] Preferably, hydrochloric acid is added to the nickel concentrate in an amount of 0.1 to 5 ml / g, more preferably 0.8 to 2.0 ml / g, per gram of treatment material.

[0146] After mixing 200, a heating or irradiation step 210 of the concentrate is performed, as described above.

[0147] Heating steps

[0148] After the mixing 200 is completed, a large amount of nickel concentrate is thus obtained, which is sent to a device for heating or irradiating 210 the material, specifically in this case. The heating can be carried out by radiation, convection, induction, thermal conduction, or any other form of heating suitable for the purpose. Preferably, microwave radiation is used. However, other devices can be used, such as, for example, infrared or radio induction devices.

[0149] The purpose of the heating is to convert the nickel and cobalt of the nickel concentrate into their soluble chloride forms, and to convert the iron, chromium and titanium of the nickel concentrate into insoluble oxide forms. The conversion occurs according to the following equation:

[0150] NiO (固态) +2HCl (水性) + Energy - → NiCl 2(水性) +H2O

[0151] FeOOH (固态) +3HCl (水性) + Energy → FeCl 3(水性) +2H2O

[0152] 2FeCl3+3H2O+energy→Fe2O 3(固体) +6HCl

[0153] or through the following mechanisms,

[0154] 4FeCl3+3O2+energy→2Fe2O 3(固态) +6Cl2

[0155] FeOOH (固态) +O2+energy-→2Fe2O 3(固态) +2H2O

[0156] Thus, the heating or irradiation 210 should be performed until a desired conversion level (e.g., above 90%) of the nickel and cobalt contained in the nickel concentrate to their soluble chloride forms is achieved, and until a desired conversion level of the iron, chromium and titanium contained in the nickel concentrate to their insoluble oxide forms is achieved. By way of illustration, in an arrangement using microwave radiation, the heating or irradiation 210 may occur, for example, for 5 to 50 minutes, more preferably 10 to 30 minutes, or until the combined temperature reaches 150 to 200 degrees Celsius and is maintained for about 5 to 40 minutes, preferably 15 to 30 minutes, preferably 20 minutes.

[0157] It should be emphasized that the heating or radiation 210 is preferably carried out in a manner that transfers energy, rather than heat, to the material, so that the heating vibrates each of the minerals contained in the material at a specific frequency that depends on the constant dielectric of each mineral. This energy transfer in the form of vibrations causes phase changes in the ore.

[0158] Likewise, goethite transforms to hematite when subjected to, for example, radiation in the presence of oxygen, such that this structural transformation draws nickel to the surface of the mineral, advantageously making the nickel more accessible for subsequent leaching.

[0159] It is also important to note that, although preferred times are described above for the heating or irradiation step 210 described herein, the heating time for transferring energy to the nickel ore greatly affects the subsequent processing steps of the nickel concentrate, particularly for recovering iron and nickel. The crystal structures of nickel- and cobalt-carrying minerals such as goethite and olivine, which will be crushed so that the nickel is exposed, have an open atomic structure that allows hydrochloric acid to penetrate. The permeability can be amplified, for example, by electromagnetic waves irradiated by microwaves, thereby leaching nickel and cobalt from these structures to form stable chlorides, because part of the leached iron forms an unstable chloride that will quickly convert to the form of insoluble hematite, and the part of the iron that is not leached by the hydrochloric acid reacts with oxygen from the air to also form insoluble hematite.

[0160] To illustrate this point, Figure 4 and Figure 5 A graph is disclosed correlating microwave irradiation time (Microwave Time (min.)), the amount of acid used in the leaching step 200 (Hydrochloric acid (L / kg)) and the percentage of material recovered from the nickel concentrate in subsequent processing steps ((Iron Recovery (%)) and (Nickel Recovery (%)) respectively).

[0161] pass Figure 4 It was noted that the longer the nickel ore remained under irradiation, the less iron was recovered in subsequent processing methods. Figure 5 The results showed that the longer the nickel ore was exposed to microwaves, the more nickel was recovered.

[0162] In this case, it is clear that the heating time or the radiation 210 should take into account the element of interest to be extracted, or even find a balance between the two based on the desired application.

[0163] To further illustrate this possibility, Figure 6 and Figure 7 In the above, the selectivity of the nickel recovery method for the main liquor contaminant iron can also be noted. In addition to the selectivity, the amount of dissolved iron can also be controlled by the time of microwave irradiation and the acid concentration used, which brings unique versatility to the method. For example, at a time equal to 20 minutes and a concentration of 2 liters of acid per kg of sample, the nickel recovery rate is close to 100% and the iron recovery rate is almost negligible. In addition, the iron present in the liquor will precipitate in the form of phosphate and will therefore become a coproduct of nickel and cobalt production.

[0164] That is to say, the preferred (but not mandatory) use of microwave radiation to irradiate nickel ore in this step brings a series of advantages to the method for obtaining nickel concentrate, as well as the overall processing method of nickel ore. Some advantages are described below in a non-exhaustive manner:

[0165] (i) By irradiation with microwaves, the dissolution of iron can be properly controlled, and thus enables the elements to be extracted from the nickel ore to be controlled, as has been explained above.

[0166] (ii) The use of microwave radiation enables high conversions of nickel and cobalt (above 85%) to be obtained, and such conversion levels cannot be achieved by conventional ovens.

[0167] (iii) Microwaves enable the conversion of elements contained in nickel ores at ambient pressure, whereas prior art processes (eg, the HPAL process) operate at high pressure but achieve lower efficiency and selectivity.

[0168] (iv) The use of microwaves enables the regeneration of the hydrochloric acid used in the processing of nickel concentrates, as seen earlier, since this acid is highly sensitive to microwaves and has a very high vapour pressure.

[0169] In any case, it should be emphasized that the use of radiation and also by means of microwaves is not essential for carrying out the method of the invention, so that, as has been exemplified previously, other forms of heating may be utilized.

[0170] After this first heating or irradiation 210 , the next optional step is to regenerate the hydrochloric acid used in the immediately preceding mixing step 200 .

[0171] Steps to regenerate hydrochloric acid

[0172] After the aforementioned heating or irradiation 210, about 20% to 90% of the hydrochloric acid originating from the mixing 200 remains in the material, while the other 80% to 10% is evaporated to a high hydrochloric acid vapor pressure value depending on the residence time.

[0173] Considering that the inventive process presented herein operates at ambient pressure, this allows the hydrochloric acid to evaporate and be easily captured and condensed for regeneration.

[0174] Therefore, in a possible and optional embodiment of the process of the invention, the following step can advantageously be carried out: regenerating the hydrochloric acid 210A, involving capturing the acid vapor produced in the heating 210 and its subsequent condensation, and then directing or returning the acid to the mixing step 200.

[0175] In other words, by this possible embodiment of the invention, most of the hydrochloric acid used is regenerated and recycled, so that an efficient process with low hydrochloric acid consumption for mixing 200 is obtained.

[0176] Whether or not this step of regenerating the hydrochloric acid has been performed, the next stage is the leaching step 220 as described above.

[0177] Microwave-assisted leaching step

[0178] After the heating or irradiation step 210, with or without subsequent regeneration of the hydrochloric acid, the nickel concentrate undergoes leaching 220, which may be assisted or supplemented by simultaneous microwave irradiation.

[0179] The leaching step 220 consists of the following operations: mixing the nickel concentrate irradiated from the previous heating or irradiation step 210 with water to dissolve the nickel and cobalt inside the concentrate. In addition, in this leaching step 220, microwave irradiation may be performed in some specific applications to accelerate the leaching method. In this case, the irradiation performed in this step is preferably performed at low temperature, more preferably between 20°C and 100°C, more preferably between 30°C and 50°C.

[0180] It should be emphasized that microwave irradiation to assist the leaching 220 is optional and not mandatory, and whether it is desirable depends on the type of application. Furthermore, the irradiation step performed simultaneously with the leaching 220 should not be mistaken as being immediately preceded by the heating or irradiation step 210 .

[0181] By this leaching step 220, whether assisted by microwave radiation or not, a nickel concentrate is obtained for obtaining a LI liquor rich in nickel, cobalt, iron, manganese and magnesium, containing materials of interest for subsequent processing, and extracting these materials from the LI liquor.

[0182] Advantageously, the present invention solves the problem of using heat from polluting sources such as coal, which produces CO2 when burned, which is known to be harmful to the environment; while using hydrochloric acid rather than sulfuric acid, which provides greater nickel recovery with less acid usage, achieving over 90% recovery at a 1,125:1 ml / g ratio.

[0183] Furthermore, in a preferred embodiment, unlike, for example, the HPAL process of the prior art, the inventive method of processing nickel concentrate enables leaching to be performed at ambient pressure due to irradiation by microwaves.

[0184] By way of illustration, as has been stated previously the HPAL process requires high temperatures to convert nickel ore, which requires heating under high pressure, not only to achieve the required high temperatures, but also to keep the iron insoluble in the HPAL process. In its preferred embodiment, using microwave radiation, the process of the present invention does not require high temperatures or high pressures and can be carried out at ambient pressure.

[0185] As an example, the following table presents a liquid recovery test under different conditions. The first table (Table 6) indicates the compositions tested, and the second table (Table 7) indicates the recovery results obtained in the test.

[0186]

[0187] Table 6 - Composition of the liquids tested.

[0188]

[0189] Table 7 - Recoveries obtained from the tests.

[0190] The "Test" column of the table above indicates the tests carried out with liquors of different compositions. The rows concerning "Theoretical liquor" are hypothetical, taking into account that the entire content of the nickel ore has been dissolved. The rows indicating the numbers 001 to 011 refer to the contents of the liquor tested after the conversion steps, in this case microwave, and microwave time (in minutes), hydrochloric acid content (liters / kg) and leaching with water.

[0191] For example, by comparing the liquid of method 004 with the liquid of method 006, it can be seen that the microwave heating time greatly changes the dissolution of iron, and the recovery rate of iron decreases from 63.685% of the liquid of method 004 to 5.022% of the liquid of method 006, while the recovery rates of nickel and cobalt remain high.

[0192] In another example, the liquor of method 009 has a higher nickel and cobalt recovery, and a lower iron recovery, and also has a liquor free of contaminants. The largest amount of content such as silica can be extracted, for example, by filtering with diatomaceous earth, and the other contaminant manganese can be sorted by precipitation and filtration at pH 7, thereby producing a liquor rich in only nickel and cobalt.

[0193] After obtaining the LI liquor enriched with materials of interest, these materials of interest can be extracted from the liquor through a series of additional steps, which will be explained later.

[0194] Step of filtering the co-products (containing oxides of iron, chromium and titanium)

[0195] After obtaining the LI liquor, in one embodiment, filtration 230 may be performed, wherein the insoluble oxide forms containing iron, chromium, and titanium are thickened, filtered, and separated from the rich liquor. The filtration may be performed, for example, by a filter press, and produces a first co-product CO containing primarily iron oxide (Fe2O3), silicon dioxide (SiO2), and chromium oxide (Cr2O3), suitable for additional subsequent separation and processing if these materials are of interest. Of course, it is important to note that the extracted insoluble form may contain lower levels of other materials, but primarily contains oxides containing iron, chromium, and titanium.

[0196] Iron phosphate precipitation and filtration steps

[0197] After the filtering step 230, a precipitation step 240 for extracting the iron contained in the LI liquid may be performed. In this case, for example, a precipitation tank is used, and the LI liquid from a phosphate source (e.g., phosphoric acid, sodium phosphate, ammonium phosphate, etc.) is added thereto in a stoichiometric ratio to force the iron contained in the LI liquid to selectively precipitate in the form of iron phosphate, and it is optional to use iron phosphate as a seed to promote its precipitation.

[0198] With regard to the steps involved in obtaining ferric phosphate, it should be emphasized that iron is one of the most significant interferents and it may be a co-product depending on the way it precipitates. For example, ferric phosphate (FePO4) is insoluble in hydrochloric acid media at low pH.

[0199] It is noteworthy that nickel remains dissolved in a wide pH range of 0 to 7, and beyond this range it precipitates primarily in the form of nickel hydroxide at pH 9. However, iron precipitates in the form of phosphate from pH 1.8 and remains in a solid phase at high pH. Due to this difference in precipitation conditions noted between nickel and iron, it is possible to selectively precipitate iron in the form of phosphate, which is a product with added value.

[0200] In this sense, precipitation preferably takes place in a stoichiometric ratio of 200% hydrogen peroxide and 150% phosphoric acid relative to the Fe ions in solution.

[0201] It is used in excess to increase the pH of the solution to maintain the iron phosphate in the solid phase. In this context, by way of illustration, after precipitation at 80°C for 2 hours, advantageously more than 97% of a precipitate is obtained, wherein the iron phosphate content is more than 95% without co-precipitation of nickel and cobalt.

[0202] Furthermore, after precipitation with phosphoric acid (H3PO4), it was noted that the LI solution turned greenish-blue due to the nickel and cobalt ions in solution. In contrast, iron phosphate (FePO4) formed a high purity white precipitate.

[0203] That is, after precipitation of iron phosphate, the LI liquor or a portion thereof containing the precipitated iron phosphate is passed through a filter press to filter 241 the iron phosphate, thereby obtaining the iron phosphate as a product of interest.

[0204] The purification step is performed by precipitation extraction.

[0205] After the step of removing the iron in the precipitate as phosphate, the main contaminants of the solution are manganese and magnesium. Manganese can precipitate with the nickel and cobalt in the solution in which it is located, which requires a step of purifying the liquor, such as extraction by solvent or selective precipitation of manganese. Magnesium does not precipitate with MHP, and therefore the liquor does not need to have a low concentration of magnesium.

[0206] Manganese can be precipitated after iron, using MnO2 as precipitant, KMnO4 concentration between 0.2 mol / L and 2 mol / L, preferably between 0.4 and 0.6 mol / L, at a temperature between 10°C and 40°C, more preferably between 20°C and 35°C, for 30 to 120 minutes, more preferably between 60 and 90 minutes, while stirring. After removing and filtering the solid products from the two main co-products (iron in the form of phosphate and manganese in the form of oxide), MHP can be precipitated by adding magnesium oxide until the pH is between 5 and 10, preferably between 6 and 8. The precipitated MHP should be filtered and the magnesium-rich solution sent to a "spray roaster" for regeneration of hydrochloric acid and precipitation of magnesium oxide present in the solution in the form of chloride.

[0207] Steps of extracting with a solvent and stripping the solvent

[0208] After the steps of precipitating 240 and filtering 241 the iron phosphate from the LI liquor, a step of purifying the LI liquor by extracting 250 certain materials therefrom (e.g. magnesium and trace iron from the previous step) with a solvent, with the aim of retaining only certain amounts of nickel and cobalt in the LI liquor, may be performed. Thus, a solvent (e.g. Cyanex 301) is added to the LI liquor, preferably in a ratio of two parts organic to one part liquid, at a temperature of 10 to 80 degrees Celsius, more preferably at 20 to 40 degrees Celsius, more preferably at 30 degrees Celsius, with a contact time of 5 to 50 minutes, preferably 20 to 40 minutes, preferably 30 minutes. The extraction step preferably occurs in a countercurrent manner in 1 to 6 steps, more preferably in 2 to 4 steps, more preferably in 3 steps, and may occur in both a mixing tank and a pulse column.

[0209] Subsequently, the solvent is stripped 251 by adding hydrochloric acid to the LI liquor, preferably 0.5 parts of hydrochloric acid at a concentration of 10 mol / L per part of organic matter. The solvent SO is returned to the extraction step 250 and the LI liquor is purified to contain mainly nickel and cobalt.

[0210] With respect to the steps listed above, extraction with a solvent is a liquid-liquid extraction technique that uses the immiscibility of the phases to transfer material from the aqueous phase (LI fluid) to the organic phase.

[0211] Preferably, the solvent used is Cyanex 301, an extractant having phosphorothioate organic functional groups and having a high selectivity for extracting nickel and cobalt.

[0212] For example, it should be noted that for the conditions of 2 mol / L Cyanex 301 in isoparaffin, a temperature of 50°C and a natural pH of 1.8, a 97% extraction of nickel ions was obtained after three extraction stages under these conditions. A 99% extraction of cobalt ions was obtained after two extraction stages under these conditions.

[0213] As another example, the above conditions are observed for stripping in an organic phase rich in nickel and cobalt, wherein the residence time for extraction for desorption is 10 to 50 minutes, preferably 20 to 40 minutes, more preferably 30 minutes; wherein the concentration of hydrochloric acid is preferably 1 to 10 mol / L, preferably 2 to 6 mol / L, more preferably 3 mol qL; the temperature is preferably 20°C to 60°C, more preferably 30°C to 40°C; wherein the aqueous phase to organic phase ratio (A:O) is preferably 1:0.5 to 1:5, more preferably (A:O) is 1:1 to 1:3, more preferably the ratio (A:O) is 1:2. It should be noted that the extraction by solvent produces an acid phase rich in nickel and cobalt.

[0214] Nickel and cobalt precipitation steps

[0215] Once the nickel and cobalt rich LI liquor is obtained, magnesium oxide (calcined magnesium oxide) is added to the LI liquor in a precipitation tank in order to extract these materials of interest from the liquor.

[0216] Preferably, magnesium oxide is added until the pH of the solution is 9, and then precipitation is performed. The products of the precipitation 260 that occurs under these conditions are nickel hydroxide and cobalt HNC, which can be extracted from the LI liquid, for example, by filtering 261 through a filter press. By way of illustration, precipitation can be performed with magnesium oxide (MgO) by adding 0.1 to 1 kg of magnesium oxide per kg of a mixture of nickel plus cobalt at a temperature of 20° C. to 80° C., more preferably 30° C. to 60° C., more preferably 40° C., for 1 to 5 hours, more preferably 2 to 4 hours, more preferably 3 hours. Advantageously, it was found that both nickel and cobalt were precipitated by more than 99%. After the precipitation step with magnesium oxide, the precipitate of nickel hydroxide and cobalt can be subjected to decantation and filtration steps to obtain nickel hydroxide and cobalt.

[0217] It should be emphasized that nickel and cobalt hydroxides are products widely used in the battery industry, but if desired, the new separation steps can be used to obtain nickel and cobalt in their separate forms and subsequently reduced to the electrolytic metal form.

[0218] Said steps may involve, for example, separation of nickel and cobalt by solvent separation followed by extraction of the nickel and cobalt by electrolysis.It should further be emphasized that the nickel obtained by the process described herein refers to high purity nickel, ie Type I nickel.

[0219] Thermal hydrolysis step for extraction or regeneration

[0220] After the nickel hydroxide and cobalt are extracted from the LI liquor, the liquor contains residual magnesium chloride and hydrochloric acid. If it is desired to extract or regenerate these elements, a thermal hydrolysis step 270 of the LI liquor can be used, which is preferably carried out by a "spray roaster" device or similar device.

[0221] The magnesium oxide added to the liquor in the previous step is precipitated and the hydrochloric acid is extracted, thereby enabling the regeneration and reuse of both, included in the above-mentioned steps of the method described herein.

[0222] Advantageously, therefore, this embodiment of the process of the invention further differs from the prior art in that it provides for the regeneration of both magnesium oxide and hydrochloric acid, thereby obtaining a cyclic loading.

[0223] Having described the methods of obtaining nickel concentrate and processing the nickel concentrate, it will be apparent that a method of recovering materials of interest from the nickel ore, if desired, may be obtained by combining these two methods into one continuous process.

[0224] Furthermore, it is demonstrated that the process proposed herein is able to bring numerous benefits of an economic and ecological nature to a range of materials of interest to be recovered from nickel ores. The following advantages can be cited non-exhaustively:

[0225] (A) enabling the recovery of residues and materials not currently exploited from such nickel ore, thereby enabling the removal of such residues from nature;

[0226] (B) eliminate the use of fossil-based heating, reducing CO2 emissions typical of processes of this type; and

[0227] (C) Recover economically relevant materials.

[0228] More specifically, the advantages which can be pointed out in a non-exhaustive manner by using the invention are:

[0229] (I) efficiently processing nickel ores, a type of deposit known to have been largely neglected by the industry due to the inefficiencies of then-existing recovery methods;

[0230] (II) recovering multiple seed products from nickel ore;

[0231] (III) controlling the solubility of iron in the nickel ore and, therefore, the daughter products to be extracted;

[0232] (IV) eliminating the need to convert elements from nickel ore through an oven, completely eliminating the emission of polluting gases from the process;

[0233] (v) using hydrochloric acid, which has a greater leaching efficiency than sulfuric acid and has a greater vapor pressure, which enables the efficiency of the process and the possibility of regeneration to be increased; and

[0234] (VI) In some embodiments, the possibility of regenerating the hydrochloric acid and manganese oxide provides the potential for economy in the amount of materials used.

[0235] Having described an example of a preferred embodiment, it should be understood that the scope of the present invention encompasses other possible variations, being limited only by the content of the appended claims, including potential equivalents.

Claims

1. A method for obtaining nickel concentrate, characterized in that The method comprises the following steps: -Scrub (100) nickel ore; - size sorting (110) the nickel ore into at least one fine fraction (FF) and a coarse fraction (CF); - subjecting the coarse fraction (CF) to magnetic separation (120) to obtain a magnetic fraction (MF); - grinding (130) the magnetic fraction (MF) to obtain a fine magnetic fraction (FMF); and - combining (140) said fine fraction (FF) with said fine magnetic fraction (FMF) to obtain a nickel concentrate (NOC).

2. The method for obtaining nickel concentrate according to claim 1, characterized in that The scrubbing step (100) is performed by means of a twin rotor mill, a rod mill or a "scrubber" type device.

3. The method for obtaining nickel concentrate according to claim 1, characterized in that The scrubbing step (100) occurs for between 2 minutes and 50 minutes.

4. The method for obtaining nickel concentrate according to claim 1, characterized in that The step of size sorting (110) produces a fine fraction (FF) having a particle size of less than 75 μm and a coarse fraction (CF) having a particle size of greater than 75 μm.

5. The method for obtaining nickel concentrate according to claim 1, characterized in that It includes a comminution step (100B) which is performed until the size of the processed material is less than 2".

6. A method for processing nickel concentrate, characterized in that The following steps are involved: - mixing nickel ore concentrate (NOC) with hydrochloric acid (200), - irradiating (210) the nickel concentrate (NOC) by microwaves until more than 90% of the nickel and cobalt contained in the nickel concentrate are converted into their soluble chloride forms, and until the desired conversion of the iron, chromium and titanium contained in the nickel concentrate into their insoluble oxide forms is achieved; - leaching (220) the nickel concentrate (NOC) with water to dissolve nickel and cobalt contained in the nickel concentrate (NOC); and - Obtaining (230) a liquid (LI) rich in nickel, cobalt, iron and magnesium.

7. The method for processing nickel concentrate according to claim 6, characterized in that The leaching step (220) is assisted by microwave radiation.

8. The method for processing nickel concentrate according to claim 6, characterized in that The method comprises the step of regenerating (210A) the hydrochloric acid used in the first leaching step (200), the step comprising evaporating the hydrochloric acid in the heating step (210), condensing the hydrochloric acid vapor, and returning the condensed hydrochloric acid to the leaching step (200).

9. The method for processing nickel concentrate according to claim 6, characterized in that The first leaching step (200) comprises adding 0.1 ml / g to 5 ml / g of hydrochloric acid per gram of nickel concentrate.

10. The method for processing nickel concentrate according to claim 6, characterized in that The heating step (210) includes heating for a period of time ranging from 5 minutes to 50 minutes.

11. The method for processing nickel concentrate according to claim 6, characterized in that The second leaching step (220) comprises microwave irradiation at a temperature between 20°C and 100°C.

12. The method for processing nickel concentrate according to claim 6, characterized in that A filtering step (230) of the liquid (LI) is included to obtain insoluble oxide forms containing iron, chromium and titanium.

13. The method for processing nickel concentrate according to claim 6, characterized in that The method comprises a precipitation step (240) for extracting the iron contained in the LI liquid, wherein the precipitation step (240) is performed by adding at least one phosphate source to the liquid (LI) in a stoichiometric ratio.

14. The method for processing nickel concentrate according to claim 13, characterized in that The following steps are involved: - using MnO2 and KMnO4 to precipitate the manganese product of the precipitation step (240) for extracting the iron contained in the LI liquid, - Precipitation of MHP, addition of magnesium oxide.

15. The method for processing nickel concentrate according to claim 6, characterized in that The following steps are involved: - adding (250) a solvent (SO) to the liquid (LI) to obtain a liquid (LI) mainly comprising nickel and cobalt; - stripping (251) the solvent (SO) by adding hydrochloric acid to the liquid (LI); and - Returning the solvent (SO) to the extraction step (250).

16. The method for processing nickel concentrate according to claim 15, characterized in that The process comprises a thermal hydrolysis step (270) of the liquid (LI) to extract magnesium oxide and hydrochloric acid.

17. The method for processing nickel concentrate according to claim 6, characterized in that The method comprises the step of adding (340) magnesium oxide to the liquid (LI) to obtain nickel hydroxide and cobalt (HNC).

18. The method for processing nickel concentrate according to claim 6, characterized in that The following steps are involved: - mixing the coarse magnetic fraction rich in chromium with H2O2; as well as - The time required for more than 90% of the chromium phase to be converted into sodium chromate by continuous microwave irradiation of the mixture.

19. A method for recovering derivatives from nickel ore, characterized in that The method comprises the steps of obtaining a nickel concentrate according to any one of claims 1 to 5, and further comprises the steps of processing a nickel concentrate according to any one of claims 6 to 18.