Polyurethane fiber and preparation method thereof

By developing protein polyurethane alloy fibers, using wet spinning process and specific polyol components, the environmental and animal welfare problems of traditional leather production are solved, providing alternative materials with excellent performance, meeting the demand for high-performance fabrics.

CN119013444APending Publication Date: 2024-11-22MODERN MEADOW INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033971.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-18
Filing Date
2023-04-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The environmental pollution, animal welfare issues and reduced supply of traditional leather production have led to an increase in demand for alternative materials.

Method used

Develop polyurethane fibers suitable for textile and fabric applications, including protein polyurethane alloys, prepared by wet spinning process using a combination of polyol components such as polyether polyols, polyester polyols and polycarbonate polyols, combined with organic solvents such as tetrahydrofuran and butyl acetate form fibers with excellent mechanical properties and aesthetic properties.

Benefits of technology

It provides materials that replace traditional leather with excellent toughness, modulus, elongation and color fastness, suitable for a variety of fabric applications, reducing dependence on animal leather and reducing environmental footprint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005082422630000181
    Figure BDA0005082422630000181
  • Figure HDA0005082422640000011
    Figure HDA0005082422640000011
  • Figure HDA0005082422640000021
    Figure HDA0005082422640000021
Patent Text Reader

Abstract

The fibers comprise a polyurethane or a protein polyurethane alloy. The fibers comprise a core defined by the polyurethane or the protein polyurethane alloy. These fibers comprising a protein polyurethane alloy comprise a protein dissolved within a polyurethane. In some embodiments, the fibers may be prepared by wet spinning a blended mixture of the polyurethane or the protein polyurethane alloy and an organic solvent. In alternative embodiments, the fibers can be prepared by wet spinning a blended mixture of the polyurethane or the protein polyurethane alloy with an aqueous solution of polyethylene oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] References to sequence listings submitted electronically

[0002] The contents of the sequence listing submitted electronically in the XML file (name: 4431_084PC01_Seqlisting_ST26.xml; size: 2,709 bytes; and creation date: April 10, 2023) submitted with this application are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates to polyurethane fibers. In some embodiments, the polyurethane fibers may be wet-spun polyurethane fibers. In some embodiments, the polyurethane fibers may include a protein polyurethane alloy comprising one or more proteins dissolved in the polyurethane. In some embodiments, these fibers may be used to prepare textiles or fabric articles, such as textiles or fabric articles typically prepared from natural leather. Background Art

[0004] Leather is a common product used in many industries, including: the furniture industry, where leather is often used as a furniture upholstery material; the apparel industry, where leather is used to make pants and jackets; the footwear industry, where leather is used to make casual and dress shoes; the luggage industry; the handbags and accessories industry; and the automotive industry. The global trade value of leather is high, and the demand for leather products continues to grow. Although leather seems to be everywhere, there are various costs, restrictions, and social issues associated with producing natural leather. First, natural leather is made from animal skins, so livestock must be raised and slaughtered. Raising livestock requires large amounts of feed, pasture, water, and fossil fuels, and can cause air and waterway pollution, such as through greenhouse gases such as methane. Leather production also raises social issues related to the treatment of animals. In recent years, the supply of traditional high-quality leather has also seen a considerable decline. For at least these reasons, it is desirable to find alternative ways to meet the demand for leather.

[0005] In addition, other fabric materials, such as cotton and spandex, are used in many industries, including the furniture industry and the clothing industry. The demand for such fabric materials is high, and there is a continuous need for improved fabric materials. Summary of the invention

[0006] The present disclosure provides polyurethane fibers suitable for use in a variety of applications, including textile or fabric applications. In some embodiments, the fibers may include a protein polyurethane alloy that provides the fibers with desirable properties for a variety of applications.

[0007] A first embodiment (1) of the present disclosure is directed to a protein polyurethane alloy construct comprising a protein dissolved in a polyurethane, wherein the construct is in the form of a fiber, and wherein the core of the fiber is defined by the protein polyurethane alloy.

[0008] In a second embodiment (2), the fiber according to the first embodiment (1) is a wet spun fiber.

[0009] In the third embodiment (3), the protein according to the first embodiment (1) or the second embodiment (2) is selected from the group consisting of soy protein, collagen, gelatin, bovine serum albumin, pea protein, egg white albumin, casein, peanut protein, edema globulin, whey protein, karanja protein, hemp protein, enzymes and cellulases.

[0010] In a fourth embodiment (4), the protein according to the first embodiment (1) or the second embodiment (2) is soybean protein.

[0011] In a fifth embodiment (5), the soybean protein according to the fourth embodiment (4) is a soybean protein isolate.

[0012] In a sixth embodiment (6), the protein polyurethane alloy construct according to any one of embodiments (1) to (5) further comprises a dye.

[0013] In a seventh embodiment (7), the fiber according to any one of embodiments (1) to (6) has a length greater than or equal to about 5 mm.

[0014] In an eighth embodiment (8), the fiber according to any one of embodiments (1) to (7) has an effective diameter in the range of about 1 micrometer to about 1 centimeter.

[0015] In a ninth embodiment (9), the fiber according to any one of embodiments (1) to (8) has an aspect ratio greater than or equal to about 10, the aspect ratio being defined as the ratio of the length of the fiber to the effective diameter of the fiber.

[0016] In a tenth embodiment (10), the aspect ratio according to the ninth embodiment (9) is in the range of about 10 to about 1000.

[0017] In an eleventh embodiment (11), the fiber according to any one of embodiments (1) to (10) has a modulus greater than or equal to about 0.1 cN / tex.

[0018] In a twelfth embodiment (12), the modulus of the fiber according to any one of embodiments (1) to (10) is in the range of 0.1 cN / tex to about 10 cN / tex.

[0019] In a thirteenth embodiment (13), the maximum elongation of the fiber according to any one of embodiments (1) to (12) is greater than or equal to about 100%.

[0020] In a fourteenth embodiment (14), the maximum elongation of the fiber according to any one of embodiments (1) to (12) is in the range of about 100% to about 1000%.

[0021] In a fifteenth embodiment (15), the fiber according to any one of embodiments (1) to (14) has a tenacity greater than or equal to about 1 cN / tex.

[0022] In a sixteenth embodiment, the fiber according to any one of embodiments (1) to (14) has a tenacity in the range of about 1 cN / tex to about 20 cN / tex.

[0023] In a seventeenth embodiment (17), the protein polyurethane alloy construct according to any one of embodiments (1) to (16) comprises a dye and dye penetration of greater than or equal to about 5% of the fiber effective radius.

[0024] In an eighteenth embodiment (18), the dye penetration according to the seventeenth embodiment (17) is greater than or equal to about 50% of the effective radius of the fiber.

[0025] In a nineteenth embodiment (19), the dye penetration according to the seventeenth embodiment (17) is greater than or equal to about 90% of the effective radius of the fiber.

[0026] In a twentieth embodiment (20), the polyurethane according to any one of embodiments (1) to (19) comprises a polyol component selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, and combinations thereof.

[0027] The twenty-first embodiment (21) of the present disclosure relates to a fiber bundle comprising a plurality of protein polyurethane alloy constructs according to any one of embodiments (1) to (20).

[0028] The twenty-second embodiment (22) of the present disclosure relates to a method for preparing protein polyurethane alloy fibers, the method comprising extruding a blended mixture comprising a protein dissolved in a polyurethane and an organic solvent into protein polyurethane alloy fibers.

[0029] In a twenty-third embodiment (23), the method according to the twenty-second embodiment (22) comprises blending the protein with a polyurethane in an aqueous solution to form a blended mixture comprising the protein dissolved in the polyurethane, and adding an organic solvent to the blended mixture.

[0030] In the twenty-fourth embodiment (24), extruding the blended mixture into the protein polyurethane alloy fiber according to the twenty-second embodiment (22) or the twenty-third embodiment (23) comprises wet spinning the blended mixture.

[0031] In a twenty-fifth embodiment (25), the organic solvent according to any one of embodiments (21) to (24) is an ether-containing solvent or an ester-containing solvent.

[0032] In a twenty-sixth embodiment (26), the organic solvent according to the twenty-fifth embodiment (25) is an ether-containing solvent, and the ether-containing solvent is tetrahydrofuran.

[0033] In the twenty-seventh embodiment (27), the organic solvent according to the twenty-fifth embodiment (25) is an ether-containing solvent, and the ether-containing solvent is diethyl ether.

[0034] In a twenty-eighth embodiment (28), the organic solvent according to the twenty-fifth embodiment (25) is an ether-containing solvent, and the ether-containing solvent is a polyether.

[0035] In a twenty-ninth embodiment (29), the organic solvent according to the twenty-fifth embodiment is an ester-containing solvent, and the ester-containing solvent is butyl acetate.

[0036] In a thirtieth embodiment (30), the blended mixture according to any one of embodiments (22) to (29) further comprises a dye.

[0037] In the thirty-first embodiment (31), the method according to any one of embodiments (22) to (29) or embodiments (22) to (30) further comprises dyeing the protein polyurethane alloy fiber.

[0038] In a thirty-second embodiment (32), the polyurethane according to any one of embodiments (22) to (31) is a water-dispersible polyurethane.

[0039] In a thirty-third embodiment (33), the polyurethane according to any one of embodiments (22) to (32) comprises a polyol component selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, and combinations thereof.

[0040] The thirty-fourth embodiment (34) of the present disclosure is directed to a method for wet-spinning polyurethane fibers, the method comprising blending a water-dispersible polyurethane and an organic solvent to form a blended mixture, and wet-spinning the blended mixture to form polyurethane fibers.

[0041] In a thirty-fifth embodiment (35), the polyurethane fiber according to the thirty-fourth embodiment (34) is substantially free of protein.

[0042] In the thirty-sixth embodiment (36), the organic solvent according to the thirty-fourth embodiment (34) or the thirty-fifth embodiment (35) is an ether-containing solvent or an ester-containing solvent.

[0043] In the thirty-seventh embodiment (37), the organic solvent according to the thirty-sixth embodiment (36) is an ether-containing solvent, and the ether-containing solvent is tetrahydrofuran.

[0044] In the thirty-eighth embodiment (38), the organic solvent according to the thirty-sixth embodiment (36) is an ether-containing solvent, and the ether-containing solvent is diethyl ether.

[0045] In the thirty-ninth embodiment (36), the organic solvent according to the thirty-sixth embodiment (36) is an ether-containing solvent, and the ether-containing solvent is a polyether.

[0046] In a fortieth embodiment (40), the organic solvent according to the thirty-sixth embodiment (36) is an ester-containing solvent, and the ester-containing solvent is butyl acetate.

[0047] In the forty-first embodiment (41), the blended mixture according to any one of embodiments (34) to (40) further comprises a dye.

[0048] In a forty-second embodiment (42), the method according to any one of embodiments (34) to (40) or embodiments (34) to (41) further comprises dyeing the polyurethane fiber.

[0049] In a forty-third embodiment (43), the polyurethane fiber according to any one of embodiments (34) to (42) has a length greater than or equal to about 5 mm.

[0050] In a forty-fourth embodiment (44), the modulus of the polyurethane fiber according to any one of embodiments (34)-(43) is greater than or equal to about 0.1 cN / tex.

[0051] In a forty-fifth embodiment (45), the maximum elongation of the polyurethane fiber according to any one of embodiments (34) to (44) is greater than or equal to about 100%.

[0052] In the forty-sixth embodiment (46), the polyurethane fiber according to any one of embodiments (34) to (45) has a tenacity greater than or equal to about 1 cN / tex.

[0053] The forty-seventh embodiment (47) of the present disclosure relates to a method for preparing protein polyurethane alloy fibers, the method comprising extruding a blended mixture into protein polyurethane alloy fibers, the blended mixture comprising a protein dissolved in a polyurethane and an aqueous solution of polyethylene oxide.

[0054] In a forty-eighth embodiment (48), the method according to the forty-seventh embodiment (47) comprises blending the protein with a polyurethane in an aqueous solution to form the blended mixture comprising the protein dissolved in the polyurethane, and adding the aqueous polyethylene oxide solution to the blended mixture.

[0055] In the forty-ninth embodiment (49), extruding the blended mixture into the protein polyurethane alloy fiber according to the forty-seventh embodiment (47) or the forty-eighth embodiment (48) comprises wet spinning the blended mixture.

[0056] In a fiftieth embodiment (50), the blended mixture according to any one of embodiments (47) to (49) further comprises a dye.

[0057] In a fifty-first embodiment (51), the method according to any one of embodiments (47) to (49) or embodiments (47) to (50) further comprises dyeing the protein polyurethane alloy fiber.

[0058] In a fifty-second embodiment (52), the polyurethane according to any one of embodiments (447) to (51) is a water-dispersible polyurethane.

[0059] The fifty-third embodiment (53) of the present disclosure relates to a method for wet-spinning polyurethane fibers, which comprises blending a water-dispersible polyurethane and an aqueous solution of polyethylene oxide to form a blended mixture, and wet-spinning the blended mixture to form polyurethane fibers.

[0060] In a fifty-fourth embodiment (54), the polyurethane fiber according to the fifty-third embodiment (53) is substantially free of protein.

[0061] In the fifty-fifth embodiment (55), the blended mixture according to the fifty-third embodiment (53) or the fifty-fourth embodiment (54) further comprises a dye.

[0062] In the fifty-sixth embodiment (56), the method according to the fifty-third embodiment (53), the fifty-fourth embodiment (54), or any one of embodiments (53) to (55) further comprises dyeing the polyurethane fiber.

[0063] In a fifty-seventh embodiment (57), the polyurethane fiber according to any one of embodiments (53) to (56) has a length greater than or equal to about 5 mm.

[0064] In a fifty-eighth embodiment (58), the modulus of the polyurethane fiber according to any one of embodiments (53) to (57) is greater than or equal to about 0.1 cN / tex.

[0065] In a fifty-ninth embodiment (59), the maximum elongation of the polyurethane fiber according to any one of embodiments (53) to (58) is greater than or equal to about 100%.

[0066] In a sixtieth embodiment (60), the polyurethane fiber according to any one of embodiments (53) to (59) has a tenacity greater than or equal to about 1 cN / tex. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] The accompanying drawings incorporated herein form a part of this specification and illustrate embodiments of the present disclosure. These drawings, together with the specification, are further used to explain the principles of the embodiments of the present disclosure and enable those skilled in the relevant art to implement and use the embodiments of the present disclosure. These drawings are intended to be exemplary and non-restrictive. Although the present disclosure is generally described in the context of these embodiments, it should be understood that the scope of the present disclosure is not intended to be limited to these specific embodiments. In the accompanying drawings, similar reference numerals indicate identical or functionally similar elements.

[0068] Figure 1 Fibers according to some embodiments are shown.

[0069] Figure 2 Fibers along the Figure 1 Cross section along line 2-2'.

[0070] Figure 3 Fiber bundles according to some embodiments are shown. DETAILED DESCRIPTION

[0071] The indefinite articles "a", "an" and "the" include plural referents unless clearly contradicted or the context clearly dictates otherwise.

[0072] The term "comprising" is an open transition phrase. The list of elements following the transition phrase "comprising" is a non-exclusive list, such that elements other than those specifically recited in the list may be present. The phrase "consisting essentially of limits the composition of a component to the specified materials and materials that do not materially affect the basic and novel characteristics of the component. The phrase "consisting of limits the composition of a component to the specified materials and excludes any materials not specified.

[0073] When quoting the numerical range including the upper limit and the lower limit herein, unless otherwise specified in a particular case, the range is intended to include its endpoints, and all integers and fractions within the range. When limiting the range, it is not intended that the disclosure or claims be limited to the specific values ​​cited. In addition, when equivalents, concentrations or other values ​​or parameters are given with a range, one or more ranges or are given with a list of upper and lower limits, it should be understood to specifically disclose all ranges or values ​​formed by any paired upper range limit and any lower range limit, regardless of whether such pairs are disclosed individually. Finally, when the term "about" is used to describe the endpoint of a value or range, the disclosure should be understood to include the specific value or endpoints mentioned. Regardless of whether the endpoint of a numerical value or range is described as "about", the endpoint of a numerical value or range is intended to include two embodiments: one is modified by "about", and one is not modified by "about".

[0074] As used herein, the term "about" refers to a value within the range of ±10% of the stated value. For example, about 3 MPa may include any value between 2.7 MPa and 3.3 MPa. That is, if a percentage is listed and the value of the percentage cannot be higher than 100%, such as 100% by weight or 99% by weight, "about" does not modify the percentage to include values ​​higher than 100%.

[0075] As used herein, "bio-based polyurethane" is a polyurethane in which at least a portion of the polyurethane (eg, the structural units of polyols (such as diols) and diacids (such as succinic acid)) is derived from biomaterials such as corn starch.

[0076] As used herein, the term "substantially free" means that a component is present in a detectable amount of no more than about 0.1% by weight.

[0077] As used herein, the term "free of" means that the component is not present in the blend or material (eg, protein polyurethane alloy), even in trace amounts.

[0078] As used herein, "collagen" refers to a family of at least 28 different naturally occurring collagen types, including but not limited to I, II, III, IV, V, VI, VII, VIII, IX, X, XI, XII, XIII, XIV, XV, XVI, XVII, XVIII, XIX and XX collagen. As used herein, the term collagen also refers to collagen prepared using recombinant technology. The term collagen includes collagen, collagen fragments, collagen-like proteins, triple helical collagen, α chains, monomers, gelatin, trimers and combinations thereof. The recombinant expression of collagen and collagen-like proteins is known in the art (see, for example, Bell, EP 1232182B1, Bovine collagen and method for producing recombinant gelatin; Olsen et al., U.S. Patent 6,428,978, and Van Heerde et al., U.S. Patent 8,188,230, these patent documents are incorporated herein by reference in their entirety). Unless otherwise indicated, any type of collagen, whether naturally occurring or prepared using recombinant technology, can be used in any of the embodiments described herein. That is, in some embodiments, the collagen described herein can be prepared using bovine type I collagen. Collagen is characterized by a repeating triplet of amino acids, -(Gly-XY)n-, such that approximately one-third of the amino acid residues in collagen are glycine. X is typically proline, and Y is typically hydroxyproline. Thus, the structure of collagen can consist of three interwoven peptide chains of varying lengths. Different animals can produce different amino acid compositions of collagen, which can result in different properties (and differences in the resulting leather).

[0079] Any type of collagen, truncated collagen, unmodified or post-translationally modified or amino acid sequence modified collagen can be used as part of the protein polyurethane alloy.

[0080] In some embodiments, the collagen can be a plant-based collagen. For example, the collagen can be a plant-based collagen prepared by CollPlant.

[0081] In some embodiments, the collagen solution can be fibrillated into collagen fibrils. As used herein, collagen fibrils refer to nanofibers composed of tropocollagen or tropocollagen-like structures (which have a triple helical structure). In some embodiments, triple helical collagen can be fibrillated to form nanofibers of collagen.

[0082] In some embodiments, recombinant collagen can include collagen fragments of the amino acid sequence of the native collagen molecule that can form procollagen (trimeric collagen). Recombinant collagen can also include collagen or truncated collagen with at least 70%, 80%, 90%, 95%, 96%, 97%, 98% or 99% homogeneity or similarity with the native collagen amino acid sequence (or with its fibril-forming region or with the segment that substantially comprises [Gly-XY]n). In some embodiments, the collagen fragment can be the 50kDa part of native collagen. The native collagen sequence includes the amino acid sequence of CollA1, CollA2 and Col3A1, which is described in Accession Nos. NP_001029211.1, NP_776945.1 and NP_001070299.1, and these sequences are incorporated herein by reference. In some embodiments, the collagen fragment may be a portion of human collagen alpha-1(III) (Col3A1; Uniprot #P02461, Entrez Gene ID #1281).

[0083] In some embodiments, the collagen fragment can have an amino acid sequence listed as SEQ ID NO: 1. In some embodiments, the collagen fragment can have at least about 80%, at least about 85%, at least about 87.5%, at least about 90%, at least about 91%, at least about 92%, at least about 93%, at least about 94%, at least about 95%, at least about 96%, at least about 97%, at least about 98%, at least about 99%, or 100% sequence identity or similarity to SEQ ID NO: 1.

[0084] Methods for producing recombinant collagen and recombinant collagen fragments are known in the art. For example, U.S. Publication Nos. 2019 / 0002893, 2019 / 0040400, 2019 / 0093116, and 2019 / 0092838 provide methods for producing collagen and collagen fragments, which can be used to produce recombinant collagen and recombinant collagen fragments disclosed herein. The contents of these four disclosures are incorporated herein by reference in their entirety.

[0085] As used herein, "fiber" refers to a construct having a length substantially greater than its effective diameter. "Fiber" can be a filament, line, yarn, cable, string, fiber bundle, line band, strip, monofilament, braid, rope or any other form of material that can be wound. In some embodiments, fiber can have a length at least ten times greater than its effective diameter. In some embodiments, fiber can have a length at least 100 times greater than its effective diameter. In some embodiments, fiber can have a length at least 200 times greater than its effective diameter. In some embodiments, fiber can have a length at least 300 times greater than its effective diameter. In some embodiments, fiber can have a length at least 500 times greater than its effective diameter.

[0086] "Effective diameter" is used herein to describe the diameter of a fiber, but the term should not be interpreted as requiring a fiber to have a circular diameter or shape. In contrast, a fiber may have a non-circular shape, and in such embodiments, the term "effective diameter" is intended to refer to the maximum cross-sectional dimension of the shape. For example, the "effective diameter" of a fiber with an elliptical cross-sectional shape would be the length of the major axis of the elliptical shape. For fibers with an effective diameter that varies along the length of the fiber, the effective diameter is the maximum effective diameter. "Effective radius" is defined as half of the effective diameter of the fiber.

[0087] As used herein, the term "core" and the phrase "core of a fiber" mean a region of a fiber located along the cross-sectional center of a fiber. Unless otherwise specified, a region of a fiber located along the cross-sectional center of a fiber is a region having a cross-sectional center defined by the cross-sectional center of the fiber and having an effective diameter less than or equal to 50% of the effective diameter of the fiber. In some embodiments, a region of a fiber located along the cross-sectional center of a fiber may be a region having a cross-sectional center defined by the cross-sectional center of the fiber and having an effective diameter less than or equal to 20% of the effective diameter of the fiber. In some embodiments, a region of a fiber located along the cross-sectional center of a fiber may be a region having a cross-sectional center defined by the cross-sectional center of the fiber and having an effective diameter less than or equal to 10% of the effective diameter of the fiber.

[0088] As used herein, the term "wet spinning" refers to a process for preparing fibers, which comprises mixing an aqueous polymer dispersion and optionally a protein in a suitable solvent to produce a polymer mixture (or polymer-protein mixture), and extruding the polymer or polymer-protein mixture through a needle or spinneret into a liquid coagulation bath, in which the polymer or polymer-protein mixture coagulates to form fibers.

[0089] As used herein, the term "wet-spun fibers" refers to fibers produced using wet spinning.

[0090] As used herein, the term "dye penetration" means the distance from the outer surface of the fiber at which the dye is visibly present in a cross section of the fiber under an optical microscope. Unless otherwise specified, dye penetration is measured in a direction perpendicular to a point on the outer surface.

[0091] Polyurethane fibers as described herein are extruded polyurethane fibers comprising one or more polyurethanes. In some embodiments, extruded polyurethane fibers as described herein are wet-spun polyurethane fibers comprising one or more polyurethanes. In some embodiments, wet-spun fibers can be spun from a polyurethane mixture comprising one or more water-dispersible polyurethanes and one or more organic solvents. In alternative embodiments, wet-spun fibers can be spun from a polyurethane mixture comprising one or more water-dispersible polyurethanes and an aqueous solution of polyethylene oxide. In some embodiments, wet-spun fibers can be spun from a polyurethane mixture comprising one or more water-dispersible polyurethanes, one or more organic solvents, and an aqueous solution of polyethylene oxide.

[0092] In some embodiments, the organic solvent is miscible with water. In some embodiments, the organic solvent can be an ether-containing solvent, such as tetrahydrofuran (THF) or dimethoxymethane. In some embodiments, the ether-containing solvent can be a polyether. The example of suitable ether-containing solvents includes but is not limited to tert-amyl ethyl ether, cyclopentyl methyl ether, di-tert-butyl ether, di(propylene glycol) methyl ether, dibutyl ether, ether, diisopropyl ether, dimethoxyethane, dimethoxymethane, 1,4-dioxane, ethyl tert-butyl ether, methoxyethane, 2-(2-methoxyethoxy) ethanol, methyl tert-butyl ether, 2-methyltetrahydrofuran, morpholine, propylene glycol methyl ether, tetrahydrofurfuryl alcohol, tetrahydropyran, 2,2,5,5-tetramethyltetrahydrofuran and polyethylene glycol.

[0093] In some embodiments, the organic solvent may be an ester-containing solvent, such as butyl acetate. Other suitable examples of ester-containing solvents include, but are not limited to, ethyl acetate, propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, and ethyl acetate, hexyl acetate.

[0094] In some embodiments, the organic solvent may include an ether-containing solvent and an ester-containing solvent.

[0095] Surprisingly, the presence of organic solvent, aqueous polyethylene oxide solution or both facilitates the formation of wet-spun polyurethane fibers made from a mixture comprising an aqueous polyurethane dispersion in a coagulation bath (see, e.g., Examples 3 and 6). In the absence of organic solvent or aqueous polyethylene oxide solution, the wet-spun aqueous polyurethane dispersion mixture described herein will not form continuous fibers, but will form discontinuous beads (see, e.g., Example 1). Without being bound by theory, it is believed that organic solvent, aqueous polyethylene oxide solution or both promote the formation of continuous fibers by increasing polymer chain entanglement, which improves spinnability. Again, without wishing to be bound by theory, it is believed that organic solvent and aqueous polyethylene oxide can increase polymer chain entanglement without causing precipitation or causing phase separation of the aqueous polyurethane dispersion, which allows for improved spinnability.

[0096] By promoting the formation of wet-spun polyurethane fibers, organic solvents, aqueous polyethylene oxide solutions, or both may also promote the formation of wet-spun polyurethane fibers from aqueous polyurethane dispersion mixtures containing other components that are miscible in the polyurethane dispersion mixture. For example, in some embodiments, the wet-spun polyurethane fibers may contain one or more proteins dissolved in the polyurethane of the fiber. In such embodiments, the wet-spun polyurethane fibers contain a "protein polyurethane alloy" as described herein.

[0097] The wet-spun polyurethane fibers described herein provide advantages over other polymer fibers, including other polyurethane fibers prepared using different methods such as different wet-spinning methods or dry-spinning methods. The wet-spun polyurethane fibers described herein may have a length suitable for producing various fabric materials (including woven, nonwoven and knitted materials). The wet-spun polyurethane fibers described herein may have mechanical / performance properties, aesthetic properties and / or thermal properties, which make them useful for producing materials with properties similar to or superior to natural leather or other common fabric materials. Fiber mechanical / performance properties include, but are not limited to, toughness (strength), modulus, elongation at break, water resistance, air permeability, and the ability to dye with reactive dyes and maintain color when rubbed (color fastness). Fiber aesthetic properties may include, but are not limited to, dyeability, aging, color, color depth, and color pattern. Fiber thermal properties include, but are not limited to, heat resistance and resistance to hardening or softening in a significantly wide temperature range (e.g., 25°C to 100°C).

[0098] Figure 1 and Figure 2 A wet-spun polyurethane fiber 100 is shown according to some embodiments. The fiber 100 includes an outer surface 102 and a core 106 about a cross-sectional center 104 of the fiber 100. The dimensions of the fiber 100 can be defined by one or more of a length 110 of the fiber 100, an effective diameter 112 of the fiber 100, or an aspect ratio of the fiber 100, which is defined as the ratio of the length 110 to the effective diameter 112.

[0099] In some embodiments, the length 110 of the fiber 100 may be greater than or equal to about 5 millimeters. In some embodiments, the length 110 of the fiber 100 may be in the range of about 5 millimeters to about 1000 meters, including subranges. For example, in some embodiments, the length 110 may be in the range of about 5 millimeters to about 500 meters, about 5 millimeters to about 200 meters, about 10 millimeters to about 1000 meters, or about 100 millimeters to about 1000 meters. In some embodiments, the length 110 of the fiber 100 may be greater than 1000 meters.

[0100] In some embodiments, the effective diameter 112 of the fiber 100 can be in the range of about 1 mm to about 1 cm, including subranges. For example, in some embodiments, the effective diameter 112 of the fiber 100 can be in the range of about 1 micron to about 5 mm, about 1 micron to about 1 mm, about 1 micron to about 500 microns, about 1 micron to about 100 microns, about 100 microns to about 1 cm, about 500 microns to about 1 cm, about 1 mm to about 1 cm, or about 5 mm to about 1 cm.

[0101] In some embodiments, the fiber 100 can have an aspect ratio of greater than or equal to about 10. In some embodiments, the fiber 100 can have an aspect ratio in the range (including sub-ranges) of about 10 to about 1000. For example, in some embodiments, the aspect ratio of the fiber 100 can be in the range of about 10 to about 750, about 10 to about 500, about 10 to about 250, or about 10 to about 100.

[0102] In some embodiments, the fiber 100 may include one or more protein polyurethane alloys. In such embodiments, the protein polyurethane alloy may define the core 106 of the fiber 100. In some embodiments, the fiber 100 may include greater than or equal to 80% by weight of the protein polyurethane alloy. In some embodiments, the fiber 100 may include greater than or equal to 85% by weight of the protein polyurethane alloy. In some embodiments, the fiber 100 may include greater than or equal to 90% by weight of the protein polyurethane alloy. In some embodiments, the fiber 100 may include greater than or equal to 95% by weight of the protein polyurethane alloy. In some embodiments, the fiber 100 may consist essentially of the protein polyurethane alloy (i.e., consisting only of an alloy having less than about 1% by weight of impurities or other components).

[0103] The protein polyurethane alloys used for the fibers 100 described herein include proteins dissolved in one polyurethane or multiple polyurethanes. In certain embodiments, the protein polyurethane alloys described herein may include proteins that are miscible with only one of the multiple phases of the polyurethane or multiple polyurethanes blended therewith. For example, in some embodiments, the protein polyurethane alloys may include proteins that are miscible with only the hard phase of the polyurethane or multiple polyurethanes having both hard and soft phases.

[0104] The protein used in the protein polyurethane alloy disclosed herein can be a lysine-containing protein. In some embodiments, the protein can be soy protein. In some embodiments, the protein can be soy protein isolate. In some embodiments, the protein can be collagen. In some embodiments, the protein can be gelatin. In some embodiments, the protein can be bovine serum albumin. In some embodiments, the protein can be pea protein. In some embodiments, the protein can be egg white albumin. In some embodiments, the protein can be casein. In some embodiments, the protein can be peanut protein. In some embodiments, the protein can be edema protein. In some embodiments, the protein can be whey protein. In some embodiments, the protein can be karanja protein. In some embodiments, the protein can be hemp protein. In some embodiments, the protein can be an enzyme. In some embodiments, the protein can be a cellulase.

[0105] Suitable water-dispersible polyurethanes for use in fibers comprising protein polyurethane alloys described herein include those comprising at least two phases, including a "soft phase" and a "hard phase". The soft phase is formed by polyol segments within the polyurethane that are separated from the urethane-containing phase due to polarity differences. The urethane-containing phase is referred to as the hard phase. This phase separation is known in the art and is the basis of many of the properties of polyurethanes.

[0106] The soft phase is typically elastomeric at room temperature and typically has a softening point or glass transition temperature (Tg) below room temperature. Tg can be measured by dynamic mechanical analysis (DMA) and quantified by the peak value of tan (δ) or the onset of the drop in storage modulus. Alternatively, Tg can be measured by differential scanning calorimetry (DSC). In some cases, there may be crystallinity in the soft phase, which can be considered as a melting point, typically between 0°C and about 60°C.

[0107] The hard phase typically has a Tg or melting point above room temperature, more typically above about 80° C. Softening of the hard phase can be measured by measuring the onset of the drop in storage modulus (sometimes referred to as stiffness) as measured by DMA.

[0108] The "soft phase" of polyurethane or protein polyurethane alloy containing polyurethane comprises the polyol component of polyurethane. Its function is to become soft and flexible at a temperature higher than its Tg to give polyurethane toughness, elongation and flexibility. Typical soft segments may include polyether polyols, polyester polyols, polycarbonate polyols and mixtures thereof. The molecular weight of the soft segment is generally in the range of about 250D to greater than about 5kD. The "hard phase" for polyurethane or protein polyurethane alloy containing polyurethane comprises the urethane segment of the polymer given by the isocyanate for connecting polyols and short-chain diols such as butanediol, propylene glycol, etc. Typical isocyanates suitable for polyurethane of the present invention include but are not limited to hexamethylene diisocyanate, isophorone diisocyanate, methylene diisocyanate, phenyl diisocyanate, etc. These molecules are more polar and harder than the polyols used to prepare the soft segment. Therefore, compared with the soft segment, the hard segment is harder and has a higher softening point. The function of the hard phase is to provide properties such as strength, temperature resistance and wear resistance to polyurethane.

[0109] In some embodiments described herein, the protein may be miscible only with the hard phase, leaving the soft phase transition substantially unchanged. Without wishing to be bound by a particular theory, it is believed that when the protein is dissolved in the hard phase, it significantly increases the temperature at which the hard phase begins to soften, thereby increasing the temperature resistance of the alloy.

[0110] In a protein polyurethane alloy comprising one or more miscible proteins and polyurethanes, the one or more proteins may be dissolved in the hard phase of the one or more polyurethanes. The protein polyurethane alloy may include at least one protein that is miscible with the hard phase of one or more polyurethanes in the alloy. In some embodiments, the protein polyurethane alloy may include multiple proteins and / or multiple polyurethane hard phases that are miscible with each other. In all of these embodiments, and without wishing to be bound by a particular theory, it is believed that the protein or multiple proteins are dissolved in the hard phase of the polyurethane or multiple polyurethanes.

[0111] When blended, one or more proteins dissolved in the hard phase of one or more polyurethanes can form a homogenized mixture. In some embodiments, the protein polyurethane alloy can include multiple proteins dissolved in one or more polyurethanes, so that the protein and polyurethane form a homogenized mixture when blended and dried. Typically, the protein polyurethane alloy comprising a homogenized mixture of protein and polyurethane does not include a large amount of protein that is not dissolved in the polyurethane. That is, and in some embodiments, the protein polyurethane alloy can include a portion of the protein dispersed in the polyurethane.

[0112] In some embodiments, the protein polyurethane alloy may be transparent. In some embodiments, a transparent protein polyurethane alloy may indicate that the protein is miscible with the hard phase of the polyurethane in the alloy. As used herein, a "transparent" material refers to a material with an opacity of about 50% or less. Opacity is measured as follows: a sample of the material is placed on a white background to measure the Y tristimulus value ("compared to white Y") in reflectivity using a D65 10 degree illuminant with a spectrometer. The same sample is then placed on a black background, and the measurement is repeated to obtain "compared to black Y". The opacity percentage is calculated as "compared to black Y" divided by "compared to white Y" multiplied by 100.

[0113] 100% opacity is defined as the lowest transparency, and 0% opacity is defined as the highest transparency.

[0114] In some embodiments, the protein polyurethane alloy can be transparent and the opacity can be in the range of 0% to about 50%, including subranges. For example, the opacity of the transparent protein polyurethane alloy can be in the range of 0% to about 40%, 0% to about 30%, 0% to about 20%, 0% to about 10%, or 0% to about 5%. The transparency of the protein polyurethane alloy is evaluated before dyeing or otherwise coloring the protein polyurethane alloy.

[0115] Transparent protein polyurethane alloys can be produced by selecting and blending appropriate combinations of one or more proteins and one or more polyurethanes. Although not all combinations of proteins and polyurethanes will produce a transparent protein polyurethane alloy layer, it is within the skill of ordinary technicians to determine whether a given blend produces a transparent protein polyurethane alloy layer in accordance with the present disclosure. In embodiments involving fibers comprising the transparent protein polyurethane alloys described herein, the transparent protein polyurethane alloys can provide unique properties to the fibers. For example, compared to opaque fibers, the transparent protein polyurethane alloys can provide unique color depth when dyed.

[0116] Suitable water-dispersible polyurethanes for protein polyurethane alloys according to the embodiments described herein include, but are not limited to, aliphatic polyurethanes, aromatic polyurethanes, bio-based polyurethanes, or acrylic modified polyurethanes. Suitable polyurethanes are commercially available from manufacturers including Lubrizol, Hauthaway, Stahl, etc. In some embodiments, the polyurethane for protein polyurethane alloys may be bio-polyurethanes. In some embodiments, the polyurethane may be a polyester polyurethane. In some embodiments, the polyurethane may be a polyether polyurethane. In some embodiments, the polyurethane may be a polycarbonate-based polyurethane. In some embodiments, the polyurethane may be an aliphatic polyester polyurethane. In some embodiments, the polyurethane may be an aliphatic polyether polyurethane. In some embodiments, the polyurethane may be an aliphatic polycarbonate polyurethane. In some embodiments, the polyurethane may be an aromatic polyester polyurethane. In some embodiments, the polyurethane may be an aromatic polyether polyurethane. In some embodiments, the polyurethane may be an aromatic polycarbonate polyurethane.

[0117] In some embodiments, polyurethane may have a soft segment selected from the group consisting of: polyether polyols, polyester polyols, polycarbonate polyols and mixtures thereof. In some embodiments, polyurethane may have a hard segment comprising a diisocyanate and an optional short-chain diol. Suitable diisocyanates may be selected from the group consisting of: aliphatic diisocyanates, such as hexamethylene diisocyanate, isophorone diisocyanate; aromatic diisocyanates, such as 4,4' diphenylmethylene diisocyanate, toluene diisocyanate, phenyl diisocyanate and mixtures thereof. Suitable short-chain diols include ethylene glycol, propylene glycol, butanediol, 2,2 methyl 1,3 propanediol, pentanediol, hexanediol and mixtures thereof. In some embodiments, crosslinking agents such as polyfunctional alcohols, for example trimethylolpropane triol or diamines, such as ethylenediamine or 4,4' diaminodiphenyl diamine.

[0118] Exemplary commercial polyurethanes include, but are not limited to, L3360 and Hauthane HD-2001 from CL Hauthaway & Sons Corporation, SANCURE TM Polyurethane, BONDTHANE from Bond Polymers International TM Polyurethanes, such as UD-108, UD-250 and UD-303, are available from BASF ECO 3702 and P100 ECO, Permutex Evo EX-RC-2214 (RC-2214) purchased from Stahl, and WLF-286BP. L3360 is an aliphatic polyester polyurethane polymer aqueous dispersion having a solid content of 35%, a viscosity of 50 cps (centipoise) to 500 cps, and a density of about 8.5 lb / gal (pounds per gallon). HD-2001 is an aliphatic polyester polyurethane polymer aqueous dispersion having a solid content of 40%, a viscosity of 50 cps to 500 cps, and a density of about 8.9 lb / gal. BONDTHANE TM UD-108 is an aqueous dispersion of an aliphatic polyether polyurethane polymer having a solids content of 33%, a viscosity of 300 cps, and a density of 8.7 lb / gal. TM UD-250 is an aqueous dispersion of an aliphatic polyester polyurethane polymer having a solids content of 35%, a viscosity of 200 cps, and a density of 8.8 lb / gal. BONDTHANE TM UD-303 is an aqueous dispersion of an aliphatic polyether polyurethane polymer having a solids content of 35%, a viscosity of less than 500 cps, and a density of 8.7 lb / gal. P100ECO is a polyester polyurethane elastomer aqueous dispersion having approximately 40% solids and a viscosity of about 40 mPas. RC-2214 is an aliphatic polyether polyurethane polymer aqueous dispersion having a solids content of 58% to 60%, a viscosity of 4,000 to 15,000 cps, and a density of about 8.9 lb / gal. WLF-286BP is a bio-based waterborne aliphatic polycarbonate polyurethane anionic aqueous dispersion with 32%-36% solids content and 5 to 1,000 cps viscosity.

[0119] Exemplary bio-based polyurethanes include, but are not limited to, L3360 available from CL Hauthaway & Sons Corporation, Eco DLS, Eco DL 519, Eco DLP-R and DL-5249. Eco DLS is an anionic aliphatic polyester polyurethane polymer aqueous dispersion having a solids content of approximately 50%, a viscosity of less than 1,200 MPa·s, and a density of about 1.1 g / cc. Eco DL 519 is an anionic, aliphatic polyester polyurethane polymer aqueous dispersion. Eco DLP-R is an anionic, aliphatic polyester polyurethane polymer aqueous dispersion. DL 5249 is an anionic, aliphatic polyester polyurethane polymer aqueous dispersion.

[0120] In some embodiments, the polyurethane may include reactive groups that can crosslink with proteins. Exemplary reactive groups include, but are not limited to, sulfonates, aldehydes, carboxylic acids or esters, blocked isocyanates, and the like, and combinations thereof. In such embodiments, the polyurethane can be crosslinked with proteins in a protein-polyurethane alloy by reacting reactive groups on the protein with reactive groups present in the polyurethane.

[0121] Suitable proteins for the protein polyurethane alloys according to the embodiments described herein include, but are not limited to, collagen, gelatin, bovine serum albumin (BSA), soy protein, pea protein, egg white albumin, casein, peanut protein, edible globulin, whey protein, karanja protein, cellulase and hemp. Suitable collagens include, but are not limited to, recombinant collagen (r-collagen), recombinant collagen fragments and extracted collagen. Suitable soy proteins include, but are not limited to, soy protein isolate (SPI), soybean meal protein and soy protein derivatives. In some embodiments, soy protein isolate may be partially hydrolyzed soy protein isolate. Suitable pea proteins include, but are not limited to pea protein isolate and pea protein derivatives. In some embodiments, pea protein isolate may be partially hydrolyzed pea protein isolate.

[0122] Table 1 below lists some exemplary proteins. Gelatin is gelatin from pig skin, type A (Sigma Aldrich G2500). Collagen is extracted bovine collagen purchased from Wuxi BIOT Biology-technology Company. Bovine serum albumin Sigma Aldrich 5470 bovine serum albumin. R-collagen is recombinant collagen from Modern Meadow. Soy protein isolate is soy protein isolate purchased from MP Medicals (IC90545625). Pea protein is pea protein powder purchased from Bobs Red Mills (MTX5232). Egg white albumin is albumin from chicken egg white (Sigma Aldrich A5253). Casein is casein from milk (Sigma Aldrich C7078). Peanut protein is peanut protein powder purchased from Tru-Nut. Whey protein is whey from milk (Sigma Aldrich W1500). Other suitable soy protein isolates include, but are not limited to, soy protein isolates available from AMD (Clarisoy 100, 110, 150, 170, 180) or DuPont ( XT 55, XT 221D, XT 221D-IP and Other suitable pea protein powders include, but are not limited to, pea protein powders available from Puris (870 and 870H).

[0123] Karanja protein is a protein found in Karanja seeds harvested from the Pongamia pinnata tree (also known as the Pongamia glabra tree). See Rahman, M. and Netravali, "Green Resin from Forestry Waste Residue'Karanja (Pongamia pinnata) Seed Cake'for Biobased Composite Structures," ACS Sustainable Chem. Eng., 2: 2318-2328 (2014); see also Mandal et al., "Nutritional Evaluation of Proteins from three Non-traditionalSeeds with or without Amino Acids Supplementation in Albino Rats," Proc. Indiannatn. Sci. Acad., B50, No. 1, 48-56 (1984). Solvent extraction methods can be used to extract proteins from Karanja seeds. Same as above. In some embodiments, the Karanja protein can be a Karanja isolated protein. In such embodiments, Karanja protein isolate can be obtained by alkaline extraction and acid precipitation of defatted Karanja seed cake. See Rahman, M. and Netravali, "Green Resin from Forestry Waste Residue'Karanja (Pongamiapinnata) Seed Cake'for Biobased Composite Structures," ACS Sustainable Chem. Eng., 2:2318-2328 (2014).

[0124] Suitable cellulase proteins are listed in Table 1 below. "Cellulase-RG" protein was purchased from CREATIVE The "Cellulase-IG" protein is a laboratory grade cellulase purchased from Carolina BiologicalSupply Company.

[0125] The 50 KDa recombinant collagen fragment (50 KDa r-collagen fragment) in Table 1 is a collagen fragment comprising the amino acid sequence listed in SEQ ID NO:1.

[0126] The "Dissolution Methods" listed in Table 1 are exemplary aqueous solvents in which proteins can be dissolved in solutions that are miscible with the hard phase of the polyurethane as described herein. Proteins that are at least partially soluble in aqueous solutions are suitable for forming protein-polyurethane alloys with aqueous polyurethane dispersions.

[0127] Table 1

[0128]

[0129] In some embodiments, the protein may have one or more of the following properties: (i) a molecular weight within the ranges described herein, (ii) an isoelectric point within the ranges described below, (iii) an amino acid composition measured as grams of lysine per 100 grams of protein within the ranges described below, and (iv) protein thermal stability up to 200°C.

[0130] Protein molecular weight

[0131] In some embodiments, the molecular weight of proteins suitable for blending with polyurethanes can range from about 1 KDa to about 700 KDa, including subranges. For example, the molecular weight of the protein can be in the range of about 1 KDa to about 700 KDa, about 10 KDa to about 700 KDa, about 20 KDa to about 700 KDa, about 50 KDa to about 700 KDa, about 100 KDa to about 700 KDa, about 200 KDa to about 700 KDa, about 300 KDa to about 700 KDa, about 400 KDa to about 700 KDa, about 500 KDa to about 700 KDa, about 600 KDa to about 700 KDa, about 1 KDa to about 600 KDa, about 1 KDa to about 500 KDa, about 1 KDa to about 400 KDa, about 1 KDa to about 300 KDa, about 1 KDa to about 200 KDa, about 1 KDa to about 100 KDa, about 1 KDa to about 50 KDa, about 1 KDa to about 20 KDa, or about 1 KDa to about 10 KDa, or in any range having any two of these values ​​as endpoints, inclusive.

[0132] Protein isoelectric point

[0133] In some embodiments, the isoelectric point of a protein suitable for blending with a polyurethane may be in the range of about 4 to about 10, including subranges. For example, the isoelectric point of the protein may be in the range of about 4 to about 10, about 4.5 to about 9.5, about 5 to about 9, about 5.5 to about 8.5, about 6 to about 8, about 6.5 to about 7.5, or about 6.5 to about 7, or in a range having any two of these values ​​as endpoints, including the endpoints. In some embodiments, the isoelectric point of the protein may be in the range of about 4 to about 5.

[0134] Protein amino acid composition

[0135] In some embodiments, the protein suitable for blending with polyurethane may have an amino acid composition (referred to as "lysine weight percentage") ranging from about 0.5% by weight to about 100% by weight (including sub-ranges) measured in grams of lysine per 100 grams of protein. For example, the lysine weight percentage of the protein may be in the range of about 0.5% by weight to about 100% by weight, about 1% by weight to about 100% by weight, about 5% by weight to about 100% by weight, about 10% by weight to about 100% by weight, about 20% by weight to about 100% by weight, about 30% by weight to about 100% by weight, about 40% by weight to about 100% by weight, about 50% by weight to about 100% by weight, about 60% by weight to about 100% by weight, about 70% by weight to about 100% by weight, about 80% by weight to about 100% by weight, or about 90% by weight to about 100% by weight, or in the range of having any two of these values ​​as endpoints, including the endpoints. In some embodiments, the protein may be polylysine.

[0136] In some embodiments, the lysine weight percentage of the protein suitable for blending with polyurethane can be in the range of about 0.5 weight % to about 20 weight %, including sub-ranges. For example, the lysine weight percentage of the protein can be in the range of about 0.5 weight % to about 20 weight %, about 1 weight % to about 19 weight %, about 2 weight % to about 18 weight %, about 3 weight % to about 17 weight %, about 4 weight % to about 16 weight %, about 5 weight % to about 15 weight %, about 6 weight % to about 14 weight %, about 7 weight % to about 13 weight %, about 8 weight % to about 12 weight %, about 9 weight % to about 11 weight % or about 9 weight % to about 10 weight %, or in the range of any two of these values ​​as endpoints, including endpoints. In some embodiments, the lysine weight percentage of the protein can be in the range of about 1 weight % to about 20 weight %. In some embodiments, the lysine weight percentage of the protein can be in the range of about 5 weight % to about 20 weight %. In some embodiments, the lysine weight percentage of the protein can be in the range of about 1 weight % to about 12 weight %. In some embodiments, the protein's lysine weight percent may be in the range of about 5 weight percent to about 12 weight percent. In some embodiments, the protein's lysine weight percent may be in the range of about 1 weight percent to about 15 weight percent. In some embodiments, the protein's lysine weight percent may be in the range of about 5 weight percent to about 15 weight percent.

[0137] In some embodiments, the protein suitable for blending with polyurethane can be heat-stable. In some embodiments, the protein can be non-heat-stable. As described herein, the protein thermal stability is determined by differential scanning calorimetry (DSC), wherein the pre-dried protein powder (wherein the moisture is less than 3%) is scanned from 0°C to 200°C. In the DSC curve of the protein, the endothermic peak greater than 10mW / mg is determined as the "denaturation peak", and the temperature corresponding to the endothermic "denaturation peak" is defined as the "denaturation temperature" of the protein. "Heat-stable" protein means that the protein has a denaturation temperature of 200°C or higher. For the purposes of this disclosure, proteins with a denaturation temperature lower than 200°C are considered to be "non-heat-stable".

[0138] Protein solubilization

[0139] In some embodiments, one or more proteins may be dissolved in an aqueous solution to form an aqueous protein mixture prior to blending with one or more polyurethanes. In some embodiments, dissolving the protein in an aqueous solution prior to blending the protein with the one or more polyurethanes may promote miscibility of the protein with the hard phase of the one or more polyurethanes. For example, dissolving the protein in an aqueous solution prior to blending the protein with the one or more polyurethanes may promote miscibility of the protein with the hard phase of the polyurethane. Not all proteins are naturally miscible with any phase of the polyurethane.

[0140] Suitable aqueous solutions include, but are not limited to, water, alkaline aqueous solutions, acid aqueous solutions, aqueous solutions including organic solvents, urea solutions, and mixtures thereof. In some embodiments, the alkaline aqueous solution may be an alkaline solution, such as sodium hydroxide, ammonia, or ammonium hydroxide solution. In some embodiments, examples of acid aqueous solutions may be acetic acid or hydrochloric acid (HCl) solutions. Suitable organic solvents include, but are not limited to, ethanol, isopropanol, acetone, ethyl acetate, isopropyl acetate, glycerol, and the like. In some embodiments, the protein concentration in the aqueous protein mixture may be in the range of about 10 g / L to about 300 g / L, including subranges.

[0141] In some embodiments, the amount of protein in the protein polyurethane alloy can be in the range of about 5% to about 50% by weight protein, including subranges. For example, in some embodiments, the amount of protein in the polyurethane alloy can be in the range of about 5% to about 50% by weight, about 10% to about 50% by weight, about 15% to about 50% by weight, about 20% to about 50% by weight, about 25% to about 50% by weight, about 30% to about 50% by weight, about 35% to about 50% by weight, about 40% to about 50% by weight, about 45% to about 50% by weight, about 5% to about 45% by weight, about 5% to about 40% by weight, about 5% to about 35% by weight, about 5% to about 30% by weight, about 5% to about 25% by weight, about 5% to about 20, about 5% to about 15% by weight, or about 5% to about 10% by weight, or in the range of any two of these values ​​as endpoints, including the endpoints. In some embodiments, the amount of protein in the protein polyurethane alloy may be in the range of about 5 wt % to about 20 wt %. In some embodiments, the amount of protein in the protein polyurethane alloy may be in the range of about 20 wt % to about 35 wt %.

[0142] In some embodiments, the amount of polyurethane in the protein polyurethane alloy may be in the range of about 50 wt % to about 95 wt %, inclusive of subranges. For example, in some embodiments, the amount of polyurethane in the protein polyurethane alloy can be in the range of about 50% to about 95% by weight, about 55% to about 95% by weight, about 60% to about 95% by weight, about 65% to about 95% by weight, about 70% to about 95% by weight, about 75% to about 95% by weight, about 80% to about 95% by weight, about 85% to about 95% by weight, about 90% to about 95% by weight, about 50% to about 90% by weight, about 50% to about 85% by weight, about 50% to about 80% by weight, about 50% to about 75% by weight, about 50% to about 70% by weight, about 50% to about 65% by weight, about 50% to about 60% by weight, or about 50% to about 55% by weight, or in the range having any two of these values ​​as endpoints, including the endpoints. In some embodiments, the amount of polyurethane in the protein polyurethane alloy can be in the range of about 80% to about 95% by weight. In some embodiments, the amount of polyurethane in the protein polyurethane alloy may range from about 65 wt % to about 80 wt %.

[0143] Any of the above-listed ranges of the weight percentages of protein and polyurethane in the protein polyurethane alloy can be combined. For example, in some embodiments, the weight percentages of protein and polyurethane in the protein polyurethane alloy can be any of the following weight percentages. The amount of protein in the polyurethane alloy can be in the range of about 5 weight % to about 50 weight %, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 50 weight % to about 95 weight %. The amount of protein in the polyurethane alloy can be in the range of about 15 weight % to about 50 weight %, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 50 weight % to about 85 weight %. The amount of protein in the polyurethane alloy can be in the range of about 20 weight % to about 50 weight %, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 50 weight % to about 80 weight %. The amount of protein in the polyurethane alloy can be in the range of about 25 weight % to about 50 weight %, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 50 weight % to about 75 weight %. The amount of protein in the polyurethane alloy can be in the range of about 30% by weight to about 50% by weight, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 50% by weight to about 70% by weight. The amount of protein in the polyurethane alloy can be in the range of about 10% by weight to about 40% by weight, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 60% by weight to about 90% by weight. The amount of protein in the polyurethane alloy can be in the range of about 15% by weight to about 40% by weight, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 60% by weight to about 85% by weight. The amount of protein in the polyurethane alloy can be in the range of about 20% by weight to about 40% by weight, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 60% by weight to about 80% by weight. The amount of protein in the polyurethane alloy can be in the range of about 20% by weight to about 35% by weight, and the amount of polyurethane in the protein polyurethane alloy can be in the range of about 65% by weight to about 80% by weight. In some embodiments, the weight percentage values ​​and ranges listed above can be based on the gross weight of the protein polyurethane alloy. In some embodiments, the weight percentage values ​​and ranges listed above may be based on the total weight of only protein and polyurethane in the protein polyurethane alloy. Unless otherwise specified, the weight percentage values ​​or ranges of polyurethane and protein are based on the total weight of only protein and polyurethane in the protein polyurethane alloy.

[0144] In some embodiments, the sum of the amount of protein plus the amount of polyurethane in the protein polyurethane alloy may be about 80 wt % or more. For example, in some embodiments, the sum of the amount of protein plus the amount of polyurethane in the protein polyurethane alloy may be in the range of about 80 wt % to 100 wt %, about 82 wt % to 100 wt %, about 84 wt % to 100 wt %, about 86 wt % to 100 wt %, about 88 wt % to 100 wt %, about 90 wt % to 100 wt %, about 92 wt % to 100 wt %, about 94 wt % to 100 wt %, about 96 wt % to 100 wt %, or about 98 wt % to 100 wt %.

[0145] In some embodiments, the protein polyurethane alloy may be a protein polyurethane alloy as described in U.S. Publication No. 2021 / 0355326 (which is hereby incorporated by reference in its entirety).

[0146] The protein polyurethane alloys described herein may be free or substantially free of protein in particulate form dispersed in the polyurethane. For example, in some embodiments, the protein polyurethane alloys may be free or substantially free of protein particles having an average diameter greater than 1 micrometer (μm).

[0147] In some embodiments, the protein polyurethane alloy may be free of or substantially free of soybean protein particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of collagen particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of gelatin particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of bovine serum albumin particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of pea protein particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of egg white albumin particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of casein particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of peanut protein particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of edema globulin particles with an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of whey protein particles having an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of karanja protein particles having an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of cellulase particles having an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of recombinant collagen fragment particles having an average diameter greater than 1 micron (μm). In some embodiments, the protein polyurethane alloy may be free of or substantially free of hemp protein particles having an average diameter greater than 1 micron (μm).

[0148] In some embodiments, the protein used in the fiber comprising the protein polyurethane alloy can be a succinylated protein. Succinylated protein is a protein modified by adding a succinyl group to the side chain of the amino acid in the protein. Most commonly, a succinyl group is added to a lysine side chain. The method of adding a succinyl group to the side chain of the amino acid in the protein is commonly referred to as protein succinylation. Adding a succinyl group to a protein can change the functional and structural properties of the protein. In some cases, adding a relatively large modification (such as a succinyl moiety) is expected to change the tertiary structure of the protein. In addition, by adding a succinyl moiety, the lysine side chain can be changed from a primary amine to an acid, making it more hydrophilic, and its charge can be changed from a positive charge to a negative charge at physiological pH. Succinylation can be accomplished using techniques well known in the art and chemical methods.

[0149] The succinylated protein used in the polyurethane alloy disclosed herein can be a lysine-containing protein. In some embodiments, the succinylated protein can be a succinylated soy protein. In some embodiments, the succinylated protein can be a succinylated soy protein isolate. In some embodiments, the succinylated protein can be a succinylated collagen. In some embodiments, the succinylated protein can be a succinylated gelatin. In some embodiments, the succinylated protein can be a succinylated bovine serum albumin. In some embodiments, the succinylated protein can be a succinylated pea protein. In some embodiments, the succinylated protein can be a succinylated egg white albumin. In some embodiments, the succinylated protein can be a succinylated casein. In some embodiments, the succinylated protein can be a succinylated peanut protein. In some embodiments, the succinylated protein can be a succinylated edema protein. In some embodiments, the succinylated protein can be a succinylated whey protein. In some embodiments, the succinylated protein can be a succinylated karanja protein. In some embodiments, the succinylated protein may be a succinylated cellulase. In some embodiments, the succinylated protein may be a succinylated hemp protein.

[0150] In some embodiments, the succinylated protein can have a solubility in water of about 50% to about 100%, including subranges, as measured as described below. For example, in some embodiments, the solubility of the succinylated protein in water can be about 50% to about 100%, about 51% to about 100%, about 52% to about 100%, about 53% to about 100%, about 54% to about 100%, about 55% to about 100%, about 56% to about 100%, about 57% to about 100%, about 58% to about 100%, about 59% to about 100%, about 60% to about 100%, about 61% to about 100%, about 62% to about 100%, about 64% to about 100%, about 66% to about 100%, about 67% to about 100%, about 68% to about 100%, about 69% to about 100%, about 70% to about 100%, about 71% to about 100%, about 72% to about 100%, about 73% to about 100%, about 74% to about 100%, about 75% to about 100%, about 76% to about 100%, about 77% to about 100%, about 78% to about 100%, about 79% to about 100%, about 80% to about 100%, about 81% to about 100%, about 82% to about 100%, about 83% to about 100%, about 84% to about 100%, about 85% to about 100%, about 86% to about 100%, about 87% to about 100%, about 88% to about 100%, about % to about 100%, about 61% to about 100%, about 62% to about 100%, about 63% to about 100%, about 64% to about 100%, about 65% to about 100%, about 66% to about 100%, about 67% to about 100%, about 68% to about 100%, about 69% to about 100%, about 70% to about 100%, about 71% to about 100%, about 72% to about 100%, From about 73% to about 100%, from about 74% to about 100%, from about 75% to about 100%, from about 76% to about 100%, from about 77% to about 100%, from about 78% to about 100%, from about 79% to about 100%, from about 80% to about 100%, from about 81% to about 100%, from about 82% to about 100%, from about 83% to about 100%, from about 84% to about 100%, from about 85% to about 10 0%, about 86% to about 100%, about 87% to about 100%, about 88% to about 100%, about 89% to about 100%, about 90% to about 100%, about 91% to about 100%, about 92% to about 100%, about 93% to about 100%, about 94% to about 100% or about 95% to about 100%, or in a range having any two of these values ​​as endpoints, inclusive.

[0151] In some embodiments, the solubility of the succinylated protein in water can be from about 60% to about 90%, from about 61% to about 90%, from about 62% to about 90%, from about 63% to about 90%, from about 64% to about 90%, from about 65% to about 90%, from about 66% to about 90%, from about 67% to about 90%, from about 68% to about 90%, from about 69% to about 90%, from about 70% to about 90%, from about 71% to about 90%. %, about 72% to about 90%, about 73% to about 90%, about 74% to about 90%, about 75% to about 90%, about 76% to about 90%, about 77% to about 90%, about 78% to about 90%, about 79% to about 90%, about 80% to about 90%, about 81% to about 90%, about 82% to about 90%, about 83% to about 90%, about 84% to about 90%, or about 85% to about 90%. In further embodiments, the solubility of the succinylated protein in water may be about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 117%, about 118%, about 119%, about 120%, about 121%, about 122%, about 123%, about 124%, about 125%, about 126%, about 127%, about 128%, about 129%, about 130%, about 131%, about 132%, about 133%, about 134%, about 135 , about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99% or about 100%.

[0152] Unless otherwise indicated, the solubility of the protein in water is measured according to the following method. The succinylated protein is suspended in a 5% (w / v) aqueous solution containing DI water, and the total solids are measured using a moisture analyzer. Then 35 mL of the 5% solution is placed in a 50 mL tube and centrifuged at 15,000×g (multiplied by gravity) for 10 minutes. After centrifugation, the supernatant is decanted and the volume and total solids of the supernatant (soluble fraction) are measured. The solubility is then calculated as follows: Solubility=(Total solids of supernatant*Volume of supernatant) / (Total solids of 5% starting solution*Volume of 5% starting solution).

[0153] In some embodiments, a succinylated protein can have an average lysine modification of about 20% to about 100%, including subranges, measured as specified below. For example, in some embodiments, the average lysine modification of the succinylated protein can be about 20% to about 100%, about 22% to about 100%, about 24% to about 100%, about 25% to about 100%, about 26% to about 100%, about 28% to about 100%, about 30% to about 100%, about 32% to about 100%, about 34% to about 100%, about 35% to about 100%, about 36% to about 100%, about 38% to about 100%, about 40% to about 100%, about 42% to about 100%, about 44% to about 100%, about 45% to about 100%, about 46% to about 100%, about 48% to about 100%, about 50% to about 100%, about 52% to about 100%, about 54% to about 100%, about 55% to about 100%, about 56% to about 100%, , about 58% to about 100%, about 60% to about 100%, about 62% to about 100%, about 64% to about 100%, about 65% to about 100%, about 66% to about 100%, about 68% to about 100%, about 70% to about 100%, about 72% to about 100%, about 74% to about 100%, about 75% to about 100%, about 76% to about 100%, about 78% to about 10 0%, about 80% to about 100%, about 82% to about 100%, about 84% to about 100%, about 85% to about 100%, about 86% to about 100%, about 88% to about 100%, about 90% to about 100%, about 92% to about 100%, about 94% to about 100%, or about 95% to about 100%, or in a range having any two of these values ​​as endpoints, inclusive.

[0154] In some embodiments, the average lysine modification of the succinylated protein may be about 60% to about 90%, about 62% to about 90%, about 64% to about 90%, about 65% to about 90%, about 66% to about 90%, about 68% to about 90%, about 70% to about 90%, about 72% to about 90%, about 74% to about 90%, about 75% to about 90%, about 76% to about 90%, about 78% to about 90%, about 80% to about 90%, about 82% to about 90%, about 84% to about 90%, or about 85% to about 90%.

[0155] In some embodiments, the average lysine modification of the succinylated protein may be about 60% to about 80%, about 62% to about 80%, about 64% to about 80%, about 65% to about 80%, about 66% to about 80%, about 68% to about 80%, about 70% to about 80%, about 72% to about 80%, about 74% to about 80%, or about 75% to about 80%.

[0156] In still further embodiments, the average lysine modification of the succinylated protein can be about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about %, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, or about 100%.

[0157] Unless otherwise indicated, the average lysine modification of the succinylated proteins disclosed herein is measured using the following lysine modification assay. The protein sample is digested using trypsin and loaded onto a liquid chromatography-mass spectrometer (LC / MS). After running the sample on the LC / MS, the sample is mapped by matching the digested peptides to the reference protein sequence of the α' subunit of β-conglycinin (gene CG-1; organism: Glycine max (soybean) (Glycine hispida), which contains the possibility of modified and unmodified lysine residues. After peptide mapping, the peak area of ​​the matching peptides is used to calculate the ratio of modified lysine to unmodified lysine at each lysine residue in the protein sequence, and then the average lysine modification% is calculated based on all detected lysines. The average lysine modification% is calculated using the following calculation. For each detected lysine, the % Lysine Modification was calculated as equal to (SUM Succinylated Lysines / (SUM Succinylated Lysines + SUM Non-Succinylated Lysines). An overall average % Lysine Modification was then calculated by averaging the individual % Lysine Modifications of all detected lysines.

[0158] The protein polyurethane alloy mixtures described herein can be formed by blending one or more proteins with one or more aqueous polyurethane dispersions in a liquid state. In some embodiments, the protein polyurethane alloy mixtures described herein can be formed by blending one or more proteins dissolved or dispersed in an aqueous solution with one or more aqueous polyurethane dispersions in a liquid state. In some embodiments, the aqueous polyurethane dispersion can be ionic, anionic or cationic. In some embodiments, the aqueous polyurethane dispersion can be non-ionic.

[0159] In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may have a modulus greater than or equal to about 0.1 cN / tex (centiNewtons / tex). In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may have a modulus ranging from about 0.1 cN / tex to about 10 cN / tex (including subranges). For example, in some embodiments, the modulus may be in the range of about 0.1 cN / tex to about 5 cN / tex, about 0.1 cN / tex to about 2 cN / tex, about 2 cN / tex to about 10 cN / tex, or about 5 cN / tex to about 10 cN / tex.

[0160] In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may have a Young's modulus greater than or equal to about 0.1 cN / tex (centiNewtons / tex). In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may have a Young's modulus ranging from about 0.1 cN / tex to about 10 cN / tex (including subranges). For example, in some embodiments, the Young's modulus may be in the range of about 0.1 cN / tex to about 5 cN / tex, about 0.1 cN / tex to about 2 cN / tex, about 2 cN / tex to about 10 cN / tex, or about 5 cN / tex to about 10 cN / tex.

[0161] In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may have a maximum elongation at break ("maximum elongation") greater than or equal to about 100%. In some embodiments, the maximum elongation may be in the range of about 100% to about 1000%, including subranges. For example, in some embodiments, the maximum elongation may be in the range of about 100% to about 750%, about 100% to about 500%, about 250% to about 1000%, or about 500% to about 1000%.

[0162] In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may have a tenacity greater than or equal to about 1 cN / tex. In some embodiments, the tenacity may be in the range of about 1 cN / tex to about 20 cN / tex, including subranges. For example, in some embodiments, the tenacity may be in the range of about 1 cN / tex to about 10 cN / tex, about 1 cN / tex to about 5 cN / tex, about 2 cN / tex to about 20 cN / tex, or about 5 cN / tex to about 20 cN / tex.

[0163] Unless otherwise stated, the modulus, Young's modulus, maximum elongation and tenacity of the fiber are the modulus, Young's modulus, maximum elongation and tenacity of the monofilament measured according to the following test. First, the fiber is conditioned overnight in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity). After conditioning, the fiber is cut into 40 mm lengths and a wire tape is attached to each end of the fiber. Then a tensile property tester ( 5965 testing machine or similar machine) test fiber. Stretch the fiber to break at 100mm / min (millimeter / minute), and record the toughness and maximum elongation. The modulus, Young's modulus, maximum elongation and toughness of the fiber are recorded as the average of at least three 40mm length sections of the fiber prepared using the same polyurethane mixture and wet spinning method. The "modulus" of the fiber is the toughness of the fiber measured at 100% elongation during the test. The Young's modulus of the fiber is calculated using the least squares fit to the test data on the initial linear portion of the tensile curve obtained using the tensile properties tester. The Young's modulus is the steepest slope of the least squares fit.

[0164] In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may include one or more colorants. In some embodiments, the colorant may be a colored dye, such as a fiber reactive dye, a direct dye, an acid dye, or a natural dye. Exemplary dyes include, but are not limited to, azo structured acid dyes, metal complex structured acid dyes, anthraquinone structured acid dyes, and azo / diazo direct dyes. In some embodiments, the colorant may be a pigment, such as a lake pigment.

[0165] In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may comprise a colored dye and a dye penetration 120 of greater than or equal to about 5% of the effective radius of the fiber 100. In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may comprise a colored dye and a dye penetration 120 of greater than or equal to about 25% of the effective radius of the fiber 100. In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may comprise a colored dye and a dye penetration 120 of greater than or equal to about 50% of the effective radius of the fiber 100. In some embodiments, the fiber 100 comprising a protein polyurethane alloy defining the core 106 of the fiber 100 may comprise a colored dye and a dye penetration 120 of greater than or equal to about 90% of the effective radius of the fiber 100.

[0166] The fiber 100 containing the protein polyurethane alloy defining the core 106 of the fiber 100 can be prepared by extruding the blended mixture into the fiber 100. In some embodiments, the blended mixture may include protein dissolved in the polyurethane and an organic solvent. In alternative embodiments, the blended mixture may include protein dissolved in the polyurethane and an aqueous solution of polyethylene oxide. In some embodiments, the blended mixture may include protein dissolved in the polyurethane, an organic solvent, and an aqueous solution of polyethylene oxide. In some embodiments, extruding the blended mixture into the fiber 100 may include wet spinning the blended mixture. After wet spinning in the coagulation bath, the fiber 100 may be removed from the coagulation bath and dried. For example, in some embodiments, the fiber 100 may be dried in an oven at a temperature of about 70° C. for 12 to 24 hours. In some embodiments, the coagulation bath for wet spinning the fiber 100 may include acetic acid and water.

[0167] In some embodiments, the protein can be blended with the water-dispersible polyurethane in an aqueous solution to form a blended mixture containing the protein dissolved in the polyurethane. Before or after the protein is blended with the water-dispersible polyurethane, an organic solvent or a polyethylene oxide aqueous solution can be added to the blended mixture. In some embodiments, the organic solvent can be an ether-containing solvent, such as tetrahydrofuran (THF) or dimethoxymethane. In some embodiments, the ether-containing solvent can include polyether. Examples of suitable ether-containing solvents include, but are not limited to, tert-amyl ethyl ether, cyclopentyl methyl ether, di-tert-butyl ether, di(propylene glycol) methyl ether, dibutyl ether, ethyl ether, diisopropyl ether, dimethoxyethane, dimethoxymethane, 1,4-dioxane, ethyl tert-butyl ether, methoxyethane, 2-(2-methoxyethoxy)ethanol, methyl tert-butyl ether, 2-methyltetrahydrofuran, morpholine, propylene glycol methyl ether, tetrahydrofurfuryl alcohol, tetrahydropyran, 2,2,5,5-tetramethyltetrahydrofuran and polyethylene glycol.

[0168] In some embodiments, the organic solvent may be an ester-containing solvent, such as butyl acetate. Other suitable examples of ester-containing solvents include, but are not limited to, ethyl acetate, propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, and ethyl acetate, hexyl acetate.

[0169] In some embodiments, the organic solvent may include an ether-containing solvent and an ester-containing solvent.

[0170] In some embodiments, the concentration of the organic solvent in the blended mixture can be defined by the volume ratio of the aqueous polyurethane dispersion to the organic solvent in the blended mixture. In some embodiments, the volume ratio of the aqueous polyurethane dispersion to the organic solvent can be in the range of about 1:2 to about 10:1, including sub-ranges. For example, in some embodiments, the volume ratio of the aqueous polyurethane dispersion to the organic solvent can be in the range of about 1:2 to about 5:1, about 1:2 to about 2:1, about 1:2 to about 1:1, about 1:1 to about 10:1, about 2:1 to about 10:1, or about 5:1 to about 10:1. As a non-limiting example, a blended mixture comprising 50 mL of an aqueous polyurethane dispersion and 50 mL of an organic solvent has a volume ratio of an aqueous polyurethane dispersion to an organic solvent of 1:1.

[0171] In some embodiments, the concentration of polyethylene oxide in the blended mixture can be in the range of about 0.5 weight % to about 10 weight %, including sub-ranges. For example, in some embodiments, the concentration of polyethylene oxide in the blended mixture can be in the range of about 0.5 weight % to about 7.5 weight %, about 0.5 weight % to about 5 weight %, about 0.5 weight % to about 2.5 weight %, about 1 weight % to about 10 weight %, about 2.5 weight % to about 10 weight % or about 5 weight % to about 10 weight %. In some embodiments, the concentration of polyethylene oxide in the blended mixture can be about 2.5 weight %. Unless otherwise stated, the concentration of polyethylene oxide in the blended mixture is the mass of polyethylene oxide relative to the mass of polyethylene oxide in the aqueous polyurethane dispersion plus the mass of polyurethane solids. As a non-limiting example, a blended mixture comprising 2.5 grams of polyethylene oxide and 97.5 grams of polyurethane solids has a polyethylene oxide concentration of 2.5 weight %.

[0172] In some embodiments, the method of preparing a fiber 100 comprising a protein polyurethane alloy defining a core 106 of the fiber 100 may include coloring the fiber 100. In some embodiments, the fiber 100 may be colored by adding a colorant to the blended mixture. For example, in some embodiments, the fiber 100 may be colored by adding a coloring dye to the blended mixture. In some embodiments, the fiber 100 may be colored with a colorant after the blended mixture is extruded into the fiber 100. For example, in some embodiments, the fiber 100 may be colored after the blended mixture is extruded into the fiber 100.

[0173] In some embodiments, the fiber 100 may include a polyurethane that is not alloyed with a protein (i.e., a "non-alloyed polyurethane") that defines the core 106 of the fiber 100. In such embodiments, the fiber 100 is substantially free of protein. In some embodiments, the fiber 100 may include greater than or equal to 80% by weight of a non-alloyed polyurethane. In some embodiments, the fiber 100 may include greater than or equal to 85% by weight of a non-alloyed polyurethane. In some embodiments, the fiber 100 may include greater than or equal to 90% by weight of a non-alloyed polyurethane. In some embodiments, the fiber 100 may include greater than or equal to 95% by weight of a non-alloyed polyurethane. In some embodiments, the fiber 100 may consist essentially of a non-alloyed polyurethane.

[0174] Suitable non-alloyed water-dispersible polyurethanes according to the embodiments described herein include, but are not limited to, aliphatic polyurethanes, aromatic polyurethanes, bio-based polyurethanes, or acrylic modified polyurethanes. Suitable polyurethanes are commercially available from manufacturers including Lubrizol, Hauthaway, Stahl, etc. In some embodiments, the polyurethane may be a bio-polyurethane. In some embodiments, the polyurethane may be a polyester polyurethane. In some embodiments, the polyurethane may be a polyether polyurethane. In some embodiments, the polyurethane may be a polycarbonate-based polyurethane. In some embodiments, the polyurethane may be an aliphatic polyester polyurethane. In some embodiments, the polyurethane may be an aliphatic polyether polyurethane. In some embodiments, the polyurethane may be an aliphatic polycarbonate polyurethane. In some embodiments, the polyurethane may be an aromatic polyester polyurethane. In some embodiments, the polyurethane may be an aromatic polyether polyurethane. In some embodiments, the polyurethane may be an aromatic polycarbonate polyurethane.

[0175] Exemplary commercial polyurethanes include, but are not limited to, L3360 and Hauthane HD-2001 from CL Hauthaway & Sons Corporation, SANCURE TMPolyurethane, BONDTHANE from Bond Polymers International TM Polyurethanes, such as UD-108, UD-250 and UD-303, are available from BASF ECO 3702 and P100ECO, and Permutex Evo EX-RC-2214 (RC-2214) available from Stahl.

[0176] In some embodiments, the fiber 100 comprising a non-alloyed polyurethane defining the core 106 of the fiber 100 may have a modulus greater than or equal to about 0.1 cN / tex. In some embodiments, the fiber 100 comprising a non-alloyed polyurethane defining the core 106 of the fiber 100 may have a modulus ranging from about 0.1 cN / tex to about 10 cN / tex (including sub-ranges). For example, in some embodiments, the modulus may be in the range of about 0.1 cN / tex to about 5 cN / tex, about 0.1 cN / tex to about 2 cN / tex, about 2 cN / tex to about 10 cN / tex, or about 5 cN / tex to about 10 cN / tex.

[0177] In some embodiments, the fiber 100 comprising a non-alloyed polyurethane defining the core 106 of the fiber 100 may have a maximum elongation greater than or equal to about 100%. In some embodiments, the maximum elongation may be in the range of about 100% to about 1000%, including sub-ranges. For example, in some embodiments, the maximum elongation may be in the range of about 100% to about 750%, about 100% to about 500%, about 250% to about 1000%, or about 500% to about 1000%.

[0178] In some embodiments, the fiber 100 comprising a non-alloyed polyurethane defining the core 106 of the fiber 100 may have a tenacity greater than or equal to about 1 cN / tex. In some embodiments, the tenacity may be in the range of about 1 cN / tex to about 20 cN / tex, including subranges. For example, in some embodiments, the tenacity may be in the range of about 1 cN / tex to about 10 cN / tex, about 1 cN / tex to about 5 cN / tex, about 2 cN / tex to about 20 cN / tex, or about 5 cN / tex to about 20 cN / tex.

[0179] In some embodiments, the fiber 100 comprising a non-alloyed polyurethane defining the core 106 of the fiber 100 may include one or more colorants. In some embodiments, the colorant may be a colored dye, such as a fiber reactive dye, a direct dye, an acid dye, or a natural dye. Exemplary dyes include, but are not limited to, azo structured acid dyes, metal complex structured acid dyes, anthraquinone structured acid dyes, and azo / diazo direct dyes. In some embodiments, the colorant may be a pigment, such as a lake pigment.

[0180] In some embodiments, the fiber 100 containing non-alloyed polyurethane defining the core 106 of the fiber 100 can be prepared by blending a water-dispersible polyurethane with an organic solvent to form a blended mixture, and wet spinning the blended mixture to form a fiber. In an alternative embodiment, the fiber 100 containing non-alloyed polyurethane defining the core 106 of the fiber 100 can be prepared by blending a water-dispersible polyurethane with an aqueous solution of polyethylene oxide to form a blended mixture, and wet spinning the blended mixture to form a fiber. After wet spinning in a coagulation bath, the fiber 100 can be removed from the coagulation bath and dried. For example, in some embodiments, the fiber 100 can be dried in an oven at a temperature of about 70° C. for 12 to 24 hours. In some embodiments, the coagulation bath for wet-spun fiber 100 can include acetic acid and water.

[0181] In some embodiments, the organic solvent can be an ether-containing solvent, such as tetrahydrofuran (THF) or dimethoxymethane. In some embodiments, the ether-containing solvent can be a polyether. The example of suitable ether-containing solvents includes but is not limited to tert-amyl ethyl ether, cyclopentyl methyl ether, di-tert-butyl ether, di(propylene glycol) methyl ether, dibutyl ether, ether, diisopropyl ether, dimethoxyethane, dimethoxymethane, 1,4-dioxane, ethyl tert-butyl ether, methoxyethane, 2-(2-methoxyethoxy) ethanol, methyl tert-butyl ether, 2-methyltetrahydrofuran, morpholine, propylene glycol methyl ether, tetrahydrofurfuryl alcohol, tetrahydropyran, 2,2,5,5-tetramethyltetrahydrofuran and polyethylene glycol.

[0182] In some embodiments, the organic solvent may be an ester-containing solvent, such as butyl acetate. Other suitable examples of ester-containing solvents include, but are not limited to, ethyl acetate, propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, and ethyl acetate, hexyl acetate.

[0183] In some embodiments, the organic solvent may include an ether-containing solvent and an ester-containing solvent.

[0184] In some embodiments, the concentration of the organic solvent in the blended mixture can be defined by the volume ratio of the aqueous polyurethane dispersion to the organic solvent in the blended mixture. In some embodiments, the volume ratio of the aqueous polyurethane dispersion to the organic solvent can be in the range of about 1:2 to about 10:1, including sub-ranges. For example, in some embodiments, the volume ratio of the aqueous polyurethane dispersion to the organic solvent can be in the range of about 1:2 to about 5:1, about 1:2 to about 2:1, about 1:2 to about 1:1, about 1:1 to about 10:1, about 2:1 to about 10:1, or about 5:1 to about 10:1. As a non-limiting example, a blended mixture comprising 50 mL of an aqueous polyurethane dispersion and 50 mL of an organic solvent has a volume ratio of an aqueous polyurethane dispersion to an organic solvent of 1:1.

[0185] In some embodiments, the concentration of polyethylene oxide in the blended mixture can be in the range of about 0.5 weight % to about 10 weight %, including sub-ranges. For example, in some embodiments, the concentration of polyethylene oxide in the blended mixture can be in the range of about 0.5 weight % to about 7.5 weight %, about 0.5 weight % to about 5 weight %, about 0.5 weight % to about 2.5 weight %, about 1 weight % to about 10 weight %, about 2.5 weight % to about 10 weight % or about 5 weight % to about 10 weight %. In some embodiments, the concentration of polyethylene oxide in the blended mixture can be about 2.5 weight %. Unless otherwise stated, the concentration of polyethylene oxide in the blended mixture is the mass of polyethylene oxide relative to the mass of polyethylene oxide in the aqueous polyurethane dispersion plus the mass of polyurethane solids. As a non-limiting example, a blended mixture comprising 2.5 grams of polyethylene oxide and 97.5 grams of polyurethane solids has a polyethylene oxide concentration of 2.5 weight %.

[0186] In some embodiments, the method of preparing a fiber 100 comprising a non-alloyed polyurethane defining a core 106 of the fiber 100 may include coloring the fiber 100. In some embodiments, the fiber 100 may be colored by adding a colorant to the blended mixture. For example, in some embodiments, the fiber 100 may be colored by adding a coloring dye to the blended mixture. In some embodiments, the fiber 100 may be colored after the blended mixture is wet spun into the fiber 100. For example, in some embodiments, the fiber 100 may be colored after the blended mixture is wet spun into the fiber 100.

[0187] In some embodiments, the fibers 100 may be formed into a fabric or textile material using techniques such as weaving, knitting, spreading, felting, stitching, and / or crocheting. In some embodiments, a plurality of fibers 100 may be bundled into a fiber bundle comprising a plurality of individual fibers 100. A fiber bundle may comprise two or more individual fibers 100. In some embodiments, a fiber bundle may comprise three or more individual fibers 100. In some embodiments, a fiber bundle may comprise ten or more individual fibers 100. In some embodiments, a fiber bundle may comprise 20 or more individual fibers 100.

[0188] The fibers 100 may be bundled using techniques such as twisting or braiding. In some embodiments, the plurality of fibers 100 may be wet spun into a fiber bundle using a multi-hole spinneret. Figure 3 A fiber bundle 300 is shown including a plurality of fibers 100 according to some embodiments.

[0189] The embodiments discussed herein will be further illustrated in the following examples.It should be understood that these examples are not limited to the embodiments described above.

[0190] Example 1: Wet spinning raw material PUD L3360 without modification

[0191] 10 grams of polyurethane dispersion (PUD) L3360 (L3360) from Hauthaway was loaded into a 20 mL syringe with a 22-gauge glutaraldehyde crosslinked (GAX) needle and injected into a 30% weight / weight (w / w) acetic acid / water coagulation bath. The extruded L3360 liquid jet solidified and formed discontinuous beads when ejected into the coagulation bath. The extruded L3360 did not form continuous fibers within the coagulation bath.

[0192] Example 2: Wet spinning of PUDL3360 / soy protein without modification

[0193] A soy protein isolate (SPI) solution was prepared by mixing 3.75 g of SPI ( XT221D-IP; DuPont; purchased from Solae LLC) was dissolved in 21.25 mL of 0.05 molar (M) sodium hydroxide (NaOH) aqueous solution in a 50 mL glass beaker. The solution was heated to 50° C. and stirred at 600 revolutions per minute (rpm) for 30 minutes to dissolve the SPI.

[0194] Then 2.6 g of SPI solution was added to 10 g of L3360 in a 25 mL beaker and mixed with an overhead stirrer for 5 minutes. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of soy protein in the resulting mixture was 90:10.

[0195] The resulting L3360 / SPI mixture was then loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 30% (w / w) acetic acid / water coagulation bath. The extruded L3360 / SPI liquid jet solidified and formed discontinuous beads when ejected into the coagulation bath. The extruded L3360 / SPI mixture did not form continuous fibers in the coagulation bath.

[0196] Example 3: Wet spinning of PUD L3360 with THF (tetrahydrofuran)

[0197] The wet spinning formulation is prepared by adding 10mL tetrahydrofuran (THF) to 10g L3360 in a 25mL beaker. The formulation is mixed for 5 minutes with an overhead stirrer. The viscosity of the formulation is measured using a Discovery HR2 rheometer and a Peltier concentric cylinder from TA Instruments with a frequency sweep test of 0.1rad / s to 100rad / s. After mixing, the formulation visually appears uniform, and the viscosity increases by about 5 times. The mixture is then loaded into a 20mL syringe with a 22-gax needle and injected into a 30% (w / w) acetic acid / water coagulation bath.

[0198] The extruded formulation solidifies and forms continuous fibers when sprayed into a coagulation bath. Then, with the continuous fibers still in the coagulation bath, a portion of the solidified fibers are stretched by hand to about 20 times their original length to confirm that the solidified fibers have suitable strength and elongation properties. In addition, stretching the fibers in the coagulation bath can help improve the mechanical strength of the fibers.

[0199] The cured fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0200] The dried fibers were then conditioned overnight in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity). After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. The fibers were then conditioned using a 500 N load cell and 1 kN clamp. 5965 testing machine to test five samples. The samples were stretched to break at 100 mm / min, and the maximum tenacity (strength) and maximum elongation were recorded. The samples had an average tenacity of about 4 cN / tex, an average elongation of about 525%, and an average modulus of 0.9 cN / tex measured at 100% elongation.

[0201] Example 4A: Wet spinning of PUD L3360 / soy protein (ratio 90:10) with THF

[0202] The SPI solution was prepared as described in Example 2.

[0203] The wet spinning formulation was prepared by adding 2.6 g SPI solution, 10 g L3360 and 10 mL THF to a 25 mL beaker. The formulation was then stirred for about 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform and the viscosity increased by about 5 times. The viscosity was measured as described in Example 3 above. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of soy protein in the resulting mixture was 90:10.

[0204] The resulting mixture is loaded into a 20 mL syringe with a 22-gax needle and injected into a 30% (w / w) acetic acid / water coagulation bath. The extruded mixture solidifies and forms a continuous protein polyurethane alloy fiber when sprayed into the coagulation bath. Then, while the continuous fiber is still placed in the coagulation bath, a portion of the fiber is stretched to approximately 14 times of its initial length by hand to confirm that the cured fiber has suitable strength and elongation properties. In addition, stretching the fiber in the coagulation bath can help improve the mechanical strength of the fiber.

[0205] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0206] Example 4B: Wet spinning of PUD L3360 / soy protein (ratio 95:5) with THF

[0207] The SPI solution was prepared as described in Example 2.

[0208] The wet spinning formulation was prepared by adding 1.24 g SPI solution, 10 g L3360 and 10 mL THF to a 25 mL beaker. The formulation was then stirred for about 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform and the viscosity increased by about 5 times. The viscosity was measured as described in Example 3 above. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of soy protein in the resulting mixture was 95:5.

[0209] The resulting mixture is loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 30% (w / w) acetic acid / water coagulation bath. The extruded mixture solidifies and forms continuous protein polyurethane alloy fibers when sprayed into the coagulation bath. Then, while the continuous fibers are still placed in the coagulation bath, a portion of the fibers is stretched by hand to approximately 14 times of its initial length to confirm that the cured fibers have suitable strength and elongation properties.

[0210] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0211] The dried fibers were then conditioned overnight in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity). After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Five samples of the fiber that was manually stretched in the coagulation bath were tested using a 5965 machine and the same method as described in Example 3. In addition, five samples of the fiber that was not manually stretched in the coagulation bath were tested using the same method. The non-manually stretched samples had an average tenacity of about 2 cN / tex, an average elongation of about 370%, and an average modulus of about 0.7 cN / tex. The manually stretched samples had an average tenacity of about 3 cN / tex and an average elongation of about 330%.

[0212] Example 5: Wet spinning of PUD RC2214 / soy protein with THF

[0213] The SPI solution was prepared as described in Example 2.

[0214] The wet spinning formulation was prepared by adding 4.37 g of SPI solution, 10 g of Permutex Evo EX-RC-2214 (RC-2214) from Stahl and 5 mL of THF into a 25 mL beaker. The formulation was then stirred for 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform and the viscosity increased by about 5 times. The viscosity was measured as described in Example 3 above. The weight ratio (w / w) of the dry mass of RC-2214 to the dry mass of the soy protein solution in the resulting mixture was 90:10 (w / w).

[0215] The resulting mixture is loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 30% (w / w) acetic acid / water coagulation bath. The extruded mixture solidifies and forms continuous protein polyurethane alloy fibers when sprayed into the coagulation bath. Then, while the continuous fibers are still placed in the coagulation bath, a portion of the fibers is stretched by hand to approximately 10 times of its initial length to confirm that the cured fibers have suitable strength and elongation properties.

[0216] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0217] Example 6: Wet spinning PUDL3360 / soybean with polyethylene oxide (PEO)

[0218] A polyethylene oxide (PEO) solution was prepared by dissolving 2.5 g of polyethylene oxide having a molecular weight of 5 million in 97.5 mL of deionized (DI) water in a 100 mL glass beaker. The mixture was then stirred at 100 rpm with a stirring bar at room temperature for three days.

[0219] The SPI solution was prepared as described in Example 2.

[0220] The wet spinning formulation was prepared by adding 2.6 g SPI solution, 10 g L3360 and 3.5 g PEO solution to a 25 mL beaker. The formulation was then stirred for 5 minutes with an overhead stirrer. After mixing, the formulation looked uniform and the viscosity increased by about 5 times. The viscosity was measured as described in Example 3 above. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of the soy protein solution in the resulting mixture was 90:10.

[0221] The resulting mixture is then loaded into a 20mL syringe with a 22-gauge GAX needle and injected into a 30% (w / w) acetic acid / water coagulation bath. The extruded mixture solidifies and forms continuous protein polyurethane alloy fibers when sprayed into the coagulation bath. It is believed that PEO is completely or partially dissolved in the coagulation bath during this process. The solidified protein polyurethane alloy fibers are then taken out from the coagulation bath by hand and transferred to a Teflon tray. The Teflon tray and fiber are placed in an oven and dried overnight at 70°C. After drying, the fiber looks uniform and continuous. The fiber feels elastic after drying and does not stick to the Teflon tray or adhere to each other.

[0222] Example 7: Pre-dyeing of protein polyurethane alloy fibers

[0223] The first dyed SPI solution was prepared by mixing 3.75 g of SPI ( XT 221D-IP; DuPont; purchased from Solae LLC) was dissolved in 21.25 mL of deionized (DI) water in a 50 mL glass beaker. Then, 100 mg of blue dye (reactive blue-21 purchased from Khushi Dyechem) was added to the SPI solution. After adding the dye, 10 N NaOH was added until a final NaOH concentration of 0.05 N was reached, and the pH of the solution was about 9. Then, the solution was heated to 50 ° C and stirred at 600 rpm for 30 minutes. The second dyeing SPI solution was prepared using the same procedure as the first dyeing solution, except that 100 mg of violet dye (reactive violet-46, purchased from Khushi Dyechem) was used.

[0224] Two wet-spun formulations were then prepared as described in Example 4A. A first wet-spun formulation was prepared using the first dyed SPI solution. A second wet-spun formulation was prepared using the second dyed SPI solution. Both formulations were wet-spun as described in Example 4A.

[0225] After drying, the sample fiber is cut along its cross section, and the uniformity of the dye in the fiber is analyzed. Based on visual observation under an optical microscope, the protein polyurethane alloy fiber prepared with both the first and second dyeing SPI solutions shows a uniform dye distribution throughout the fiber cross section. It can be seen that blue dye and purple dye have penetrated the entire fiber cross section. These results show that, for the protein polyurethane alloy fiber with the SPI of 5% by weight protein loading, uniform active pre-staining can be achieved. It is believed that the protein polyurethane alloy fiber prepared from other proteins can also be uniformly dyed using other reactive dyes soluble under alkaline conditions using this dyeing method.

[0226] After visual inspection under an optical microscope, the sample fibers were immersed in a vial with 20 mL of 1X phosphate buffered saline (PBS) (pH 7.48) to evaluate color bleeding. After immersion for 1 week at room temperature, the samples showed minimal color bleeding into the solution, indicating that the dye was fully integrated with the protein polyurethane alloy defining the fiber.

[0227] Example 8: Post-dyeing of protein polyurethane alloy fibers

[0228] Wet-spun and dried fiber samples of Example 3 (wet-spun L3360 fibers without SPI) and Example 4A (wet-spun protein polyurethane alloy fibers containing L3360 and SPI) were dyed according to the following method.

[0229] Fiber is placed in beaker and immersed in 30mL DI water.Then, 150mg blue acid dye (acid blue 158 natural blue, purchased from Panchmahal Dye Stuff Industries) is added in beaker.After adding dyestuff, measure pH and dropwise add HCl until reaching about 3.5 pH.Then the dyeing mixture of fiber immersion is left standstill overnight.On the second day, fiber is taken out from beaker and rinsed with warm water to remove unbonded dyestuff.

[0230] Based on visual observation, the fibers of Example 3 did not absorb a significant amount of the blue acid dye. The color of these fibers remained significantly unchanged after dyeing. In contrast, the fibers of Example 4A showed a significant color change.

[0231] The dyeing sample fiber of embodiment 4A is cut along its cross section, and the uniformity of dye is analyzed. Based on the visual observation under optical microscope, the protein polyurethane alloy fiber of embodiment 4A demonstrates the uniform dye distribution throughout the fiber cross section. As can be seen, the blue acid dye has penetrated the whole fiber cross section. These results show, for the protein polyurethane alloy fiber with the SPI of 5 % by weight protein loading, uniform acidic post-dyeing can be achieved. It is believed that the protein polyurethane alloy fiber prepared using other proteins can also use this post-dyeing method to dye uniformly.

[0232] Example 9: Wet spinning of PUD L3360 / succinylated SPI with THF

[0233] Succinylated soy protein isolate (S-SPI) was prepared using the following method. A 10% weight / volume (w / v) soy protein isolate (SPI) solution was prepared by adding 20 grams of SPI (Solae XT 221D-IP; DuPont) in 180 milliliters (mL) of water to prepare 200 mL of solution. Then, 54 microliters (μL) of 10N sodium hydroxide (NaOH) were added and the solution was mixed until the SPI was completely dissolved. Once the SPI was completely dissolved, 200 milligrams (mg) of solid succinic anhydride and 10N sodium hydroxide (NaOH) were added to the SPI solution simultaneously while maintaining a pH of about 9 to 9.5. After the addition of succinic anhydride and sodium hydroxide, the solution was incubated at room temperature for 1 hour while stirring using an overhead stirrer. After incubation, SnakeSkin from ThermoScientific was used. TM The solution was dialyzed against DI water for 24 hours using a dialysis tube. After dialysis, the product was lyophilized to a solid protein powder.

[0234] S-SPI solution was prepared by dissolving 3.75 g S-SPI in 21.25 mL deionized water in a 50 mL glass beaker. The solution was heated to 50°C and stirred at 600 rpm for 30 minutes to dissolve the S-SPI.

[0235] The wet spinning formulation was prepared by adding 1.24 g of S-SPI solution, 10 g of L3360 and 10 mL of THF to a 25 mL beaker. The formulation was then stirred for about 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform and the viscosity increased by about 5 times. The viscosity was measured as described in Example 3 above. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of S-SPI in the resulting mixture was 95:5.

[0236] The obtained mixture is loaded into a 20 mL syringe with a 22-gax needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidifies and forms continuous protein polyurethane alloy fibers when sprayed into the coagulation bath. The protein polyurethane alloy fibers that are solidified are then taken out from the bath by hand and transferred to a Teflon dish.

[0237] The Teflon disk and fibers were placed in an oven and dried at 75°C for 30 minutes. After drying, the fibers appeared uniform and continuous. The fibers felt springy after drying and did not stick to the Teflon disk or to each other.

[0238] Example 10: Wet spinning of PUD L3360 / cellulase with THF

[0239] 4.18 g of cellulase (purchased from Suntaq International Limited) was added 20 cellulase) was dissolved in 21.25 mL of deionized water in a 50 mL glass beaker to prepare a cellulase solution. The solution was stirred at 600 rpm for 30 minutes at room temperature to dissolve the cellulase.

[0240] The wet spinning formulation was prepared by adding 1.11 g of cellulase solution, 10 g of L3360 and 10 mL of THF into a 25 mL beaker. The formulation was then stirred for about 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform, and the viscosity increased by about 5 times. Viscosity was measured as described in Example 3 above. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of cellulase in the resulting mixture was 95:5.

[0241] The obtained mixture is loaded into a 20mL syringe with a 22-gax needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidifies and forms continuous protein polyurethane alloy fibers when sprayed into the coagulation bath. The solidified protein polyurethane alloy fibers are then taken out from the bath by hand and transferred to a Teflon (Teflon) tray. The Teflon tray and the fiber are placed in an oven and dried at 75°C for 30 minutes. After drying, the fiber looks uniform and continuous. The fiber feels elastic after drying and does not stick to the Teflon tray or adhere to each other.

[0242] The dried fibers were then conditioned overnight in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity). After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Five samples were tested using a 5965 machine and the same method as described in Example 3. The samples had an average tenacity of about 2 cN / tex and an average elongation of about 360%.

[0243] Example 11: Wet spinning of PUD L3360 / 50 KDa r-collagen fragments (ratio 80:20) with THF

[0244] The wet spinning preparation was prepared by adding 0.35g of a 50KDa r-collagen fragment containing an amino acid sequence as listed in SEQ ID NO: 1 to 5g L3360 in a 50mL beaker. The preparation was then stirred for about 10 minutes at 250rpm with an overhead stirrer. After mixing, the preparation visually appeared uniform and the collagen solids appeared to be completely dissolved. Then, 5mL THF was added to the preparation and stirred for about 15 minutes at 150rpm with an overhead stirrer. After mixing, the preparation visually appeared uniform. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of collagen in the resulting mixture was 80:20.

[0245] The resulting mixture was loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidified and formed continuous protein polyurethane alloy fibers when sprayed into the coagulation bath.

[0246] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0247] The dried fibers were then conditioned in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity) for more than 24 hours. After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Three samples were tested using a 5965 testing machine and the same method as described in Example 3. The samples had an average tenacity of about 1.5 cN / tex, an average elongation of about 262%, and an average Young's modulus of 3.4 cN / tex. The Young's modulus was calculated using a least squares fit to the test data on the initial linear portion of the tensile curve obtained by the 5965 testing machine. The steepest slope of the least squares fit was reported as the Young's modulus for each sample.

[0248] Example 12: Wet spinning of PUD L3360 with butyl acetate

[0249] The wet spinning formulation was prepared by adding 5 mL of butyl acetate to 10 g of L3360 in a 25 mL beaker. The formulation was mixed for 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform. The mixture was then loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded formulation solidified and formed continuous fibers when sprayed into the coagulation bath.

[0250] The cured fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0251] The dried fibers were then conditioned in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity) for more than 24 hours. After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Three samples were tested using a 5965 testing machine and the same method as described in Example 3. The samples had an average tenacity of about 1.5 cN / tex, an average elongation of about 353%, and an average Young's modulus of 2.0 cN / tex. The Young's modulus was calculated as described in Example 11.

[0252] Example 13: Wet spinning of PUD L3360 / soy protein (ratio 95:5) with butyl acetate

[0253] The SPI solution was prepared as described in Example 2.

[0254] The wet spinning formulation was prepared by adding 1.24 g of SPI solution, 10 g of L3360 and 5 mL of butyl acetate to a 25 mL beaker. The formulation was then stirred for about 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of soy protein in the resulting mixture was 95:5.

[0255] The resulting mixture was loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidified and formed continuous protein polyurethane alloy fibers when sprayed into the coagulation bath.

[0256] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0257] The dried fibers were then conditioned in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity) for more than 24 hours. After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Three samples were tested using a 5965 testing machine and the same method as described in Example 3. The samples had an average tenacity of about 1.0 cN / tex, an average elongation of about 169%, and an average Young's modulus of 2.7 cN / tex. The Young's modulus was calculated as described in Example 11.

[0258] Example 14: Wet spinning of PUD L3360 / soy protein (ratio 95:5) with ether

[0259] The SPI solution was prepared as described in Example 2.

[0260] The wet spinning formulation was prepared by adding 1.49 g of SPI solution, 12 g of L3360 and 10 mL of ether to a 25 mL beaker. The formulation was then stirred for about 5 minutes with an overhead stirrer. After mixing, the formulation visually appeared uniform. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of soy protein in the resulting mixture was 95:5.

[0261] The resulting mixture was loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidified and formed continuous protein polyurethane alloy fibers when sprayed into the coagulation bath.

[0262] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0263] The dried fibers were then conditioned in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity) for more than 24 hours. After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Three samples were tested using a 5965 testing machine and the same method as described in Example 3. The samples had an average tenacity of about 1.3 cN / tex, an average elongation of about 326%, and an average Young's modulus of 2.5 cN / tex. The Young's modulus was calculated as described in Example 11.

[0264] Example 15: Wet spinning of PUD using THF WLF-286BP

[0265] By adding 8mL of THF to 10mL in a 25mL beaker WLF-286BP was used to prepare the wet spinning formulation. The formulation was mixed with an overhead stirrer at 200 rpm for 2 minutes. After mixing, the formulation visually appeared uniform.

[0266] The resulting mixture was loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidified and formed continuous polyurethane fibers when sprayed into the coagulation bath.

[0267] The cured polyurethane fibers were then removed from the bath by hand and transferred to a Teflon tray. The Teflon tray and fibers were placed in an oven and dried overnight at 70°C. After drying, the fibers appeared uniform and continuous. The fibers felt springy after drying and did not stick to the Teflon tray or to each other.

[0268] Example 16: Wet spinning PUDL3360 / bovine serum albumin (ratio 95:5) with THF

[0269] Bovine serum albumin (BSA) solution was prepared by adding 1 g of BSA lyophilized powder from Sigma Aldrich to 9 g of water in a 20 mL vial. The vial was placed in a 50°C water bath and mixed with a stir bar at 600 rpm for 30 minutes.

[0270] The wet spinning formulation was prepared by adding 1.84 g of the BSA solution described above, 10 g of L3360 and 10 mL of THF to a 20 mL beaker. The formulation was then stirred for 5 minutes at 250 rpm with an overhead stirrer. After mixing, the formulation visually appeared uniform. The weight ratio (w / w) of the dry mass of L3360 to the dry mass of BSA in the resulting mixture was 95:5.

[0271] The resulting mixture was loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidified and formed continuous protein polyurethane alloy fibers when sprayed into the coagulation bath.

[0272] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried at 70°C for 1 hour. After drying, the fibers looked uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0273] The dried fibers were then conditioned in a conditioning room (23°C ± 1°C, 50% ± 5% relative humidity) for more than 24 hours. After conditioning, the fibers were cut into 40 mm lengths and a wire tape was attached to each end of a single fiber sample. Three samples were tested using a 5965 testing machine and the same method as described in Example 3. The samples had an average tenacity of about 2.4 cN / tex, an average elongation of about 368%, and an average Young's modulus of 1.4 cN / tex. The Young's modulus was calculated as described in Example 11.

[0274] Example 17: Wet spinning of PUD using THF WLF-286BP / SPI (ratio 95:5)

[0275] The SPI solution was prepared as described in Example 2.

[0276] By mixing 1.1g SPI solution and 8.9g WLF-286BP was added to a 25 mL beaker to prepare a wet spinning formulation. The formulation was then stirred for approximately 5 minutes using an overhead stirrer. After mixing, the formulation visually appeared homogeneous. The weight ratio (w / w) of the dry mass of WLF-286BP to the dry mass of soy protein was 95: 5. Then, 8 mL of THF was added to the formulation in the beaker and stirred at 150 rpm with an overhead stirrer for about 15 minutes.

[0277] The resulting mixture was loaded into a 20 mL syringe with a 22-gauge GAX needle and injected into a 60% (w / w) acetic acid / water coagulation bath. The extruded mixture solidified and formed continuous protein polyurethane alloy fibers when sprayed into the coagulation bath.

[0278] The cured protein polyurethane alloy fibers were then removed from the bath by hand and transferred to a Teflon dish. The Teflon dish and fibers were placed in an oven and dried at 70°C for 1 hour. After drying, the fibers looked uniform and continuous. The fibers felt elastic after drying and did not stick to the Teflon dish or to each other.

[0279] Although various embodiments have been described herein, they are presented by way of example only and not by way of limitation. It is apparent that, based on the teachings and guidance given herein, adjustments and modifications are intended to fall within the meaning and scope of equivalents of the disclosed embodiments. Therefore, it will be apparent to those skilled in the art that, without departing from the essence and scope of the present disclosure, various forms and details of changes may be made to the embodiments disclosed herein. The elements of the embodiments presented herein are not necessarily mutually exclusive, but are interchangeable to satisfy various situations as will be understood by those skilled in the art.

[0280] Embodiments of the present disclosure are described in detail herein with reference to the embodiments shown in the accompanying drawings, wherein similar figure numbers are used to indicate identical or functionally similar elements. References to "one embodiment," "embodiment," "some embodiments," "in certain embodiments," etc. indicate that the embodiments described may include specific features, structures, or characteristics, but each embodiment may not necessarily include specific features, structures, or characteristics. Moreover, such phrases do not necessarily refer to the same embodiment. In addition, when describing specific features, structures, or characteristics in conjunction with an embodiment, whether or not explicitly described, it is believed that a person skilled in the art will be able to implement such features, structures, or characteristics in conjunction with other embodiments.

[0281] The examples are intended to illustrate rather than limit the present disclosure. Other suitable modifications and adaptations of the various conditions and parameters normally encountered in the art and which will be apparent to those skilled in the art are within the spirit and scope of the present disclosure.

[0282] It should be understood that the phraseology or terminology employed herein is for the purpose of description and not limitation.The breadth and scope of the present disclosure should not be limited by any of the above-described exemplary embodiments, but should be defined in accordance with the following claims and their equivalents.

[0283] sequence

[0284] SEQ ID NO: 1: Collagen fragment

[0285] DVKSGVAVGGLAGYPGPAGPPGPPGPPGTSGHPGSPGSPGYQGPPGEPGQAGPSGPPGPPGAIGPSGPAGKDGESGRPGRPGERGLPGPPGIKGPAGIPGFPGMKGHRGFDGRNGEKGETGAPGLKGENGLPGENGAPGPMGPRGAPGERGRPGLPGAAGARGNDGARGSDGQPGPPGPPGTAGFPGSPGAKGEVGPAGSPGSNGAPGQRGEPGPQGHAGAQGPGPPGINGSPGGKGEMGPAGIPGAPGLMGARGPPPGAGANGAPGLRGGA GEPGKNGAKGEPGPRGERGEAGIPGVPGAKGEDGKDGSPGEPGANGLPGAAGERGAPGFRGPAGPNGIPGEKGPAGERGAPGPAGPRGAAGEPGRDGVPGGPGMRGMPGSPGGPGSDGKPGPPGSQGESGRPGPPG PSGPRGQPGVMGFPGPKGNDGAPGKNGERGGPGGPGPQGPPGKNGETGPQGPPGPTGPGDKGDTGPPGPQGLQGLPGTGGPPGENGKPGEPGPKGDAGAPGAPGGKGDAGAPGERGPPAIAGIGGEKAGGFAPYYG

Claims

1. A protein polyurethane alloy construct comprising a protein dissolved in a polyurethane, wherein the construct is in the form of a fiber, and wherein the core of the fiber is defined by the protein polyurethane alloy.

2. The protein polyurethane alloy construct of claim 1, wherein the fibers are wet-spun fibers.

3. The protein polyurethane alloy construct of claim 1 or claim 2, wherein the protein is selected from the group consisting of soy protein, collagen, gelatin, bovine serum albumin, pea protein, egg white albumin, casein, peanut protein, edema globulin, whey protein, karanja protein, hemp protein, enzymes and cellulases.

4. The protein polyurethane alloy construct of claim 1 or claim 2, wherein the protein is soy protein.

5. The protein polyurethane alloy construct according to claim 4, wherein the soy protein is soy protein isolate.

6. The protein polyurethane alloy construct according to any one of claims 1 to 5, further comprising a dye.

7. The protein polyurethane alloy construct of any one of claims 1 to 6, wherein the length of the fibers is greater than or equal to about 5 mm.

8. The protein polyurethane alloy construct of any one of claims 1 to 7, wherein the effective diameter of the fibers is in the range of about 1 micron to about 1 centimeter.

9. The protein polyurethane alloy construct of any one of claims 1 to 8, wherein the fiber has an aspect ratio of greater than or equal to about 10, the aspect ratio being defined as the ratio of the length of the fiber to the effective diameter of the fiber.

10. The protein polyurethane alloy construct of claim 9, wherein the aspect ratio is in the range of about 10 to about 1000.

11. The protein polyurethane alloy construct of any one of claims 1 to 10, wherein the fiber has a modulus greater than or equal to about 0.1 cN / tex.

12. The protein polyurethane alloy construct of any one of claims 1 to 10, wherein the modulus of the fiber is in the range of about 0.1 cN / tex to about 10 cN / tex.

13. The protein polyurethane alloy construct of any one of claims 1 to 12, wherein the maximum elongation of the fibers is greater than or equal to about 100%.

14. The protein polyurethane alloy construct of any one of claims 1 to 12, wherein the maximum elongation of the fibers is in the range of about 100% to about 1000%.

15. The protein polyurethane alloy construct of any one of claims 1 to 14, wherein the fiber has a tenacity greater than or equal to about 1 cN / tex.

16. The protein polyurethane alloy construct of any one of claims 1 to 14, wherein the fiber has a tenacity in the range of about 1 cN / tex to about 20 cN / tex.

17. The protein polyurethane alloy construct according to any one of claims 1 to 16, comprising: dyes; and Dye penetration is greater than or equal to about 5% of the effective radius of the fiber.

18. The protein polyurethane alloy construct of claim 17, wherein the dye penetration is greater than or equal to about 50% of the effective radius of the fiber.

19. The protein polyurethane alloy construct of claim 17, wherein the dye penetration is greater than or equal to about 90% of the effective radius of the fiber.

20. The protein polyurethane alloy construct of any one of claims 1 to 19, wherein the polyurethane comprises a polyol component selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, and combinations thereof.

21. A fiber bundle, comprising: a plurality of protein polyurethane alloy constructs according to any one of claims 1 to 20.

22. A method for preparing protein polyurethane alloy fiber, the method comprising: The blended mixture is extruded into protein polyurethane alloy fibers, the blended mixture comprising: Protein dissolved in polyurethane; as well as Organic solvents.

23. The method according to claim 22, comprising: blending the protein with polyurethane in an aqueous solution to form a blended mixture comprising the protein dissolved in the polyurethane; as well as The organic solvent is added to the blended mixture.

24. The method of claim 22 or claim 23, wherein extruding the blended mixture into the protein polyurethane alloy fibers comprises wet spinning the blended mixture.

25. The method according to any one of claims 22 to 24, wherein the organic solvent is an ether-containing solvent or an ester-containing solvent.

26. The method of claim 25, wherein the organic solvent is an ethereal solvent, and the ethereal solvent is tetrahydrofuran.

27. The method of claim 25, wherein the organic solvent is an ethereal solvent, and the ethereal solvent is diethyl ether.

28. The method of claim 25, wherein the organic solvent is an ethereal solvent, and the ethereal solvent is a polyether.

29. The method of claim 25, wherein the organic solvent is an ester-containing solvent, and the ester-containing solvent is butyl acetate.

30. The method of any one of claims 22 to 29, wherein the blended mixture further comprises a dye.

31. A method according to any one of claims 22 to 29 or claims 22 to 30, further comprising dyeing the protein polyurethane alloy fiber.

32. The method of any one of claims 22 to 31, wherein the polyurethane is a water dispersible polyurethane.

33. The method of any one of claims 22 to 32, wherein the polyurethane comprises a polyol component selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, and combinations thereof.

34. A method for wet spinning polyurethane fibers, the method comprising: blending a water-dispersible polyurethane and an organic solvent to form a blended mixture; as well as The blended mixture is wet spun to form polyurethane fibers.

35. The method of claim 34, wherein the polyurethane fibers are substantially free of protein.

36. The method of claim 34 or claim 35, wherein the organic solvent is an ether-containing solvent or an ester-containing solvent.

37. The method of claim 36, wherein the organic solvent is an ethereal solvent, and the ethereal solvent is tetrahydrofuran.

38. The method of claim 36, wherein the organic solvent is an ethereal solvent, and the ethereal solvent is diethyl ether.

39. The method of claim 36, wherein the organic solvent is an ethereal solvent, and the ethereal solvent is a polyether.

40. The method of claim 36, wherein the organic solvent is an ester-containing solvent, and the ester-containing solvent is butyl acetate.

41. The method of any one of claims 34 to 40, wherein the blended mixture further comprises a dye.

42. A method according to any one of claims 34 to 40 or claims 34 to 41 further comprising dyeing the polyurethane fibres.

43. The method of any one of claims 34 to 42, wherein the polyurethane fibers have a length greater than or equal to about 5 mm.

44. The method of any one of claims 34 to 43, wherein the polyurethane fiber has a modulus greater than or equal to about 0.1 cN / tex.

45. The method of any one of claims 34 to 44, wherein the polyurethane fiber has a maximum elongation greater than or equal to about 100%.

46. ​​The method of any one of claims 34 to 45, wherein the polyurethane fiber has a tenacity greater than or equal to about 1 cN / tex.

47. A method for preparing a protein polyurethane alloy fiber, the method comprising: The blended mixture is extruded into protein polyurethane alloy fibers, the blended mixture comprising: Protein dissolved in polyurethane; as well as Polyethylene oxide aqueous solution.

48. The method of claim 47, comprising: blending the protein with polyurethane in an aqueous solution to form a blended mixture comprising the protein dissolved in the polyurethane; as well as The aqueous polyethylene oxide solution is added to the blended mixture.

49. The method of claim 47 or claim 48, wherein extruding the blended mixture into the protein polyurethane alloy fibers comprises wet spinning the blended mixture.

50. The method of any one of claims 47 to 49, wherein the blended mixture further comprises a dye.

51. A method according to any one of claims 47 to 49 or claims 47 to 50 further comprising dyeing the protein polyurethane alloy fiber.

52. The method of any one of claims 47 to 51, wherein the polyurethane is a water dispersible polyurethane.

53. A method for wet spinning polyurethane fibers, the method comprising: blending a water-dispersible polyurethane and an aqueous solution of polyethylene oxide to form a blended mixture; as well as The blended mixture is wet spun to form polyurethane fibers.

54. The method of claim 53, wherein the polyurethane fibers are substantially free of protein.

55. The method of claim 53 or claim 54, wherein the blended mixture further comprises a dye.

56. The method of any one of claims 53, 54, or 53 to 55, further comprising dyeing the polyurethane fiber.

57. The method of any one of claims 53 to 56, wherein the polyurethane fibers have a length greater than or equal to about 5 mm.

58. The method of any one of claims 53 to 57, wherein the polyurethane fiber has a modulus greater than or equal to about 0.1 cN / tex.

59. The method of any one of claims 53 to 58, wherein the polyurethane fiber has a maximum elongation greater than or equal to about 100%.

60. The method of any one of claims 53 to 59, wherein the polyurethane fiber has a tenacity greater than or equal to about 1 cN / tex.