Nonaqueous electrolyte electricity storage element and electricity storage device
By using the positive electrode active material particles and negative pressure states of lithium transition metal composite oxide in the non-aqueous electrolyte power storage element, the resistance increase caused by cracks of the positive electrode active material particles after deep discharge is solved, and the output performance is significantly improved stability.
Patent Information
- Application Number
- CN202380034291.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-22
AI Technical Summary
After deep discharge of existing nonaqueous electrolyte power storage components, the positive electrode active material particles are prone to cracks, resulting in higher resistance and lowered output performance.
The positive electrode active material particles are used for lithium transition metal composite oxide, and the content of lithium element relative to the transition metal element exceeds 1.0, and gas soluble in the non-aqueous electrolyte is stored in the container to maintain a negative pressure state to suppress the positive electrode activity. The expansion and cracks of the material particles ensure that the electrode body is pressed in the lamination direction.
It effectively suppresses the reduction in output performance after charging and discharging cycles, and improves the circulation performance of nonaqueous electrolyte power storage components.
Smart Images

Figure CN119013811A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a nonaqueous electrolyte electricity storage element and an electricity storage device. Background Art
[0002] Non-aqueous electrolyte secondary batteries represented by lithium-ion secondary batteries are widely used in electronic devices such as personal computers, communication terminals, and automobiles due to their high energy density. The above-mentioned non-aqueous electrolyte secondary batteries generally have: an electrode body having a pair of electrodes electrically isolated by an isolator and a non-aqueous electrolyte between the electrodes, and are configured to charge and discharge by transferring charge ions between the two electrodes. In addition, as non-aqueous electrolyte storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and double-layer capacitors have also been widely popularized.
[0003] As positive electrode active material particles for such non-aqueous electrolyte storage elements, lithium transition metal composite oxides having an α-NaFeO2 type crystal structure are known. For example, various active materials (hereinafter also referred to as "LiMeO2 type" active materials) have been proposed, in which the molar ratio of Mn in the transition metal element (Me) (Mn / Me) is less than 0.5, the molar ratio of Li to the transition metal element (Me) is 1, and the composition formula can be typically represented by LiMeO2 (see Patent Document 1). As the above-mentioned "LiMeO2 type" active materials, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 or the like is a composite oxide containing Ni, Co and Mn (hereinafter also referred to as "NCM type" active material).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2011-216485 Summary of the invention
[0007] In the positive electrode active material particles having the above-mentioned α-NaFeO2 type crystal structure and containing a lithium transition metal composite oxide containing Ni, Co and Mn, cracks are generated in the positive electrode active material particles when deep discharge is performed, which becomes one of the reasons for reducing the charge and discharge cycle performance of the non-aqueous electrolyte storage element. Here, deep discharge refers to a state in which deep discharge is performed until the positive electrode active material particles fully absorb Li. In addition, in a non-aqueous electrolyte storage element having such positive electrode active material particles, there is a tendency for the resistance to increase by performing a charge and discharge cycle accompanied by deep discharge. If the resistance becomes high, problems such as reduced output performance are likely to occur.
[0008] An object of the present invention is to provide a non-aqueous electrolyte electricity storage element and an electricity storage device capable of suppressing a decrease in output performance after a charge and discharge cycle.
[0009] A nonaqueous electrolyte storage element according to one aspect of the present invention comprises an electrode body formed by stacking a positive electrode and a negative electrode containing positive electrode active material particles, a nonaqueous electrolyte, and a sealable container for containing the electrode body and the nonaqueous electrolyte, wherein the positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure, the content of lithium element in the lithium transition metal composite oxide relative to the transition metal element being greater than 1.0 in terms of molar ratio, the positive electrode active material particles contain a heterogeneous element, and the heterogeneous element is aluminum element, tungsten element, boron element, zinc element, titanium element or a combination thereof, a gas soluble in the nonaqueous electrolyte is contained inside the container, the interior of the container is in a negative pressure state, and the electrode body is in a state of being pressed in the stacking direction of the positive electrode and the negative electrode.
[0010] A power storage device according to another aspect of the present invention includes two or more nonaqueous electrolyte power storage elements and includes one or more nonaqueous electrolyte power storage elements according to the one aspect of the present invention.
[0011] According to one aspect of the present invention, a nonaqueous electrolyte energy storage element capable of suppressing a decrease in output performance after charge and discharge cycles can be provided.
[0012] According to another aspect of the present invention, it is possible to provide a power storage device capable of suppressing a decrease in output performance after a charge and discharge cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a schematic exploded perspective view showing a nonaqueous electrolyte energy storage device according to one embodiment of the present invention.
[0014] Figure 2 This is a schematic diagram showing one embodiment of an electricity storage device constituted by assembling a plurality of nonaqueous electrolyte electricity storage elements. DETAILED DESCRIPTION
[0015] First, the outline of the nonaqueous electrolyte electricity storage element and electricity storage device disclosed in this specification will be described.
[0016] [1] A non-aqueous electrolyte storage element according to one aspect of the present invention comprises an electrode body formed by stacking a positive electrode and a negative electrode containing positive electrode active material particles, a non-aqueous electrolyte, and a sealable container for storing the electrode body and the non-aqueous electrolyte, wherein the positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure, the content of lithium element in the lithium transition metal composite oxide relative to the transition metal element being greater than 1.0 in terms of molar ratio, the positive electrode active material particles contain a heterogeneous element, the heterogeneous element is aluminum element, tungsten element, boron element, zinc element, titanium element or a combination thereof, a gas soluble in the non-aqueous electrolyte is stored inside the container, the inside of the container is in a negative pressure state, and the electrode body is in a state of being pressed in the stacking direction of the positive electrode and the negative electrode.
[0017] The non-aqueous electrolyte storage element described in [1] above can suppress the reduction of output performance after charge and discharge cycles. The reason for this effect is not clear, but it is speculated as follows. By making the content of lithium element in the lithium transition metal composite oxide relative to the transition metal element exceed 1.0 in molar ratio, cracks are not easily generated in the positive electrode active material particles even in the case of deep discharge, which can reduce the expansion of the positive electrode. On the other hand, lithium transition metal composite oxides in which the content of lithium element relative to the transition metal element exceeds 1.0 in molar ratio have the following problems due to the high content of lithium element: as a lithium source, the lithium compound used excessively during the synthesis of the lithium transition metal composite oxide remains more than the "LiMeO2 type" active material, and gas is generated due to the decomposition of the lithium compound during charging, causing the non-aqueous electrolyte storage element to expand. In contrast, by making the positive electrode active material particles containing the lithium transition metal composite oxide contain heterogeneous elements, the decomposition of the lithium compound can be suppressed, and the expansion of the non-aqueous electrolyte storage element caused by the generation of gas can be suppressed. In addition, the nonaqueous electrolyte storage element described in [1] above generates a force that pulls the container inward because the interior of the container is in a negative pressure state, so that the electrode body is pressed in the stacking direction of the positive electrode and the negative electrode. As a result, the expansion of the positive electrode caused by the cracks in the positive electrode active material particles is further suppressed, so the reduction in output performance after the charge and discharge cycle can be further suppressed. Furthermore, the nonaqueous electrolyte storage element described in [1] above is a gas soluble in a nonaqueous electrolyte solution contained in the sealed container, and the gas is dissolved in the nonaqueous electrolyte solution. As a result, the pressure inside the container decreases, so that the interior of the container can be more reliably in a negative pressure state, and the electrode body can be more reliably in the stacking direction of the positive electrode and the negative electrode. The nonaqueous electrolyte storage element described in [1] can suppress the reduction in output performance after the charge and discharge cycle. "The stacking direction of the positive electrode and the negative electrode" refers to the direction in which the positive electrode and the negative electrode are stacked, and "the state of being pressed in the stacking direction" refers to the state in which pressure is applied in the direction in which the distance between the stacked layers of the electrode body becomes smaller. "Gases soluble in non-aqueous electrolytes" refers to gases soluble in 1 cm2 of non-aqueous electrolytes at 1 atmosphere and 25°C. 3 The solubility in 1cm 3 "The interior of the container is in a negative pressure state" means that the pressure of the remaining space inside the container is lower than the pressure outside the container.
[0018] It should be noted that, in the case where the lithium transition metal composite oxide can be prepared before the positive electrode is made, the composition ratio of the lithium transition metal composite oxide in this specification refers to the composition ratio of the lithium transition metal composite oxide before the positive electrode is made. In the case of preparing from the assembled non-aqueous electrolyte storage element, it refers to the composition ratio when the full discharge state is reached by the following method. First, the non-aqueous electrolyte storage element is charged with a constant current at a current of 0.05C until the charge termination voltage during normal use is reached, and it becomes a fully charged state. After pausing for 30 minutes, discharge at a constant current of 0.05C to the lower limit voltage during normal use. Disassemble and remove the positive electrode, use a metal lithium electrode as the counter electrode to assemble a test battery, and discharge at a constant current value of 10mA per 1g of positive electrode mixture until the positive electrode potential reaches 2.0V vs.Li / Li + , adjust the positive electrode to a fully discharged state. Disassemble and remove the positive electrode again. Use dimethyl carbonate to thoroughly clean the non-aqueous electrolyte attached to the removed positive electrode, and after drying at room temperature for a day and a night, recover the lithium transition metal composite oxide of the positive electrode active material particles. The recovered lithium transition metal composite oxide is provided for measurement. The operations from disassembling the non-aqueous electrolyte storage element to recovering the lithium transition metal composite oxide are carried out in an argon atmosphere with a dew point below -60°C. Here, normal use refers to the case where the non-aqueous electrolyte storage element is used under the recommended or specified charging and discharging conditions for the non-aqueous electrolyte storage element. When a charger for the non-aqueous electrolyte storage element is prepared, it refers to the case where the non-aqueous electrolyte storage element is used using the charger.
[0019] [2] In the non-aqueous electrolyte storage element described in [1] above, the gas soluble in the non-aqueous electrolyte solution may be carbon dioxide. The non-aqueous electrolyte storage element described in [2] above can improve the solubility of the gas in the non-aqueous electrolyte solution by using carbon dioxide as the gas soluble in the non-aqueous electrolyte solution.
[0020] [3] In the non-aqueous electrolyte storage element described in [1] or [2] above, the transition metal element may include at least one of nickel, cobalt and manganese, and the ratio of the number of moles of the foreign element to the sum of the number of moles of the nickel, cobalt, manganese and the foreign element may be higher near the surface of the positive electrode active material particle than near the center. The non-aqueous electrolyte storage element described in [3] above can further suppress the reduction of output performance after charge and discharge cycles because the transition metal element includes at least one of nickel, cobalt and manganese, and the ratio of the number of moles of the foreign element to the sum of the number of moles of the nickel, cobalt, manganese and the foreign element is higher near the surface of the positive electrode active material particle than near the center. Here, in the present invention, for "near the center and near the surface of the positive electrode active material particle", the distance from the center of the positive electrode active material particle to the surface of the particle is divided into 8 equal parts, and each of the obtained regions is used as a measurement point. When the center of the positive electrode active material particle is set as Point 0 and the outermost surface of the positive electrode active material particle is set as Point 8, "near the center" refers to the region of the above-mentioned Point 0, and "near the surface" refers to the region of the above-mentioned Point 8. "The ratio of the number of moles of the foreign element to the sum of the number of moles of the nickel element, the cobalt element, the manganese element and the foreign element near the surface of the above-mentioned positive electrode active material particle is higher than that near the center" means that the ratio of the number of moles of the region of the above-mentioned Point 8 of the above-mentioned positive electrode active material particle is greater than the ratio of the number of moles of the region of the above-mentioned Point 0 of the above-mentioned positive electrode active material particle. The ratio of the number of moles of the foreign element near the center of the above-mentioned positive electrode active material particle and near the surface of the above-mentioned positive electrode active material particle is calculated according to the following steps. First, according to the same steps as the method for calculating the composition ratio of the above-mentioned lithium transition metal composite oxide, a positive electrode adjusted to a fully discharged state is prepared. For the cross-section of the positive electrode processed by the cross-section polisher, the distance from the center of the positive electrode active material particle to the surface of the particle is divided into 8 equal parts by a scanning electron microscope-energy dispersive X-ray analyzer (SEM-EDX), and the center of the positive electrode active material particle at this time is set as Point 0 and the outermost surface of the positive electrode active material particle is set as Point 8, and the molar concentration of the foreign element, nickel element, manganese element and cobalt element at each point is measured. Next, the molar concentration of the foreign element is divided by the total molar concentration of nickel element, manganese element, cobalt element and the foreign element to calculate the ratio of the number of moles of the foreign element. The ratio of the number of moles of the foreign element in the whole positive electrode active material particle is calculated by high-frequency inductively coupled plasma (ICP) emission spectrometry, except that the molar concentration of the foreign element, nickel element, manganese element and cobalt element is measured by high-frequency inductively coupled plasma (ICP) emission spectrometry, and the ratio of the number of moles of the foreign element near the center of the positive electrode active material particle and near the surface of the positive electrode active material particle is calculated in the same steps as the method of calculating the ratio of the number of moles of the foreign element near the center of the positive electrode active material particle and near the surface of the positive electrode active material particle.
[0021] [4] In the non-aqueous electrolyte storage element described in any one of [1] to [3] above, the transition metal element preferably contains manganese, and the content of manganese relative to the transition metal element is 0.35 to 0.65 in terms of molar ratio. The non-aqueous electrolyte storage element described in [4] above can suppress the dissolution of manganese from the positive electrode active material particles, and can further suppress the reduction in output performance of the non-aqueous electrolyte storage element after charge and discharge cycles, because the content of manganese relative to the transition metal element is greater than the lower limit and less than the upper limit.
[0022] [5] A power storage device according to another aspect of the present invention includes two or more nonaqueous electrolyte power storage elements and includes one or more nonaqueous electrolyte power storage elements according to any one of [1] to [4] above.
[0023] According to the power storage device described in [5] above, it is possible to suppress a decrease in output performance after charge and discharge cycles.
[0024] The following describes in detail the structure of a non-aqueous electrolyte storage element, the structure of a storage device, the manufacturing method of a non-aqueous electrolyte storage element, and other embodiments of the present invention. It should be noted that the names of the components (components) used in each embodiment are sometimes different from the names of the components (components) used in the background art.
[0025] <Structure of non-aqueous electrolyte energy storage device>
[0026] A non-aqueous electrolyte storage element (hereinafter also referred to as "storage element") according to one embodiment of the present invention comprises an electrode body formed by stacking a positive electrode, a negative electrode and a separator, a non-aqueous electrolyte and a sealable container for containing the electrode body and the non-aqueous electrolyte. The electrode body is in a state of being pressed in the stacking direction of the positive electrode and the negative electrode. A gas soluble in the non-aqueous electrolyte is contained inside the container, and the inside of the container is in a negative pressure state. The electrode body is generally a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked via a separator, or a winding type in which a positive electrode and a negative electrode are stacked via a separator. The non-aqueous electrolyte exists in a state contained in the positive electrode, the negative electrode and the separator. As an example of a non-aqueous electrolyte storage element, a non-aqueous electrolyte secondary battery (hereinafter also referred to as "secondary battery") is described.
[0027] Figure 1A non-aqueous electrolyte storage element 1 is shown as an example of a square battery. The non-aqueous electrolyte storage element 1 comprises a wound electrode body 2 formed by winding a positive electrode and a negative electrode stacked via a separator, a positive electrode collector 14 and a negative electrode collector 15 respectively connected to both ends of the electrode body 2, a container 3 for storing them, and a positive terminal 4 and a negative terminal 5 provided in the container 3. As the container 3, a known metal container, a resin container, etc. commonly used as a container for a non-aqueous electrolyte secondary battery can be used. As the above-mentioned metal, for example, aluminum, stainless steel, nickel-plated steel, etc. can be exemplified. As the above-mentioned metal, among them, from the viewpoint of being easily deformed by negative pressure (and thus making the inside of the container negative pressure so that the electrode body is more effectively pressed in the stacking direction of the above-mentioned positive electrode and the above-mentioned negative electrode), it is preferred to use a container 3 made of aluminum or an aluminum alloy.
[0028] The container 3 includes a flat bottomed square tube-shaped container body 3a and an elongated rectangular plate-shaped cover 3b capable of closing the elongated rectangular opening of the container body 3a. The electrode body 2 is in direct or indirect contact with the inner surface of the container body 3a.
[0029] The lid 3b is provided with a positive terminal 4 and a negative terminal 5 for external electrical connection. The positive electrode is electrically connected to the positive terminal 4 via a positive current collector 14 connected to the positive electrode substrate, and the negative electrode is electrically connected to the negative terminal 5 via a negative current collector 15 connected to the negative electrode substrate.
[0030] In the non-aqueous electrolyte storage element 1, the electrode body 2 is pressed in the stacking direction of the positive electrode and the negative electrode by the negative pressure state inside the container 3. The electrode body 2 directly or indirectly in contact with the inner surface of the container body 3a is pressed in the stacking direction by the negative pressure state inside the container 3, that is, by generating a force to pull the container 3 inward. As a result, the expansion of the positive electrode caused by cracks in the positive electrode active material particles is suppressed, thereby improving the effect of suppressing the reduction in output performance after charge and discharge cycles.
[0031] In the state before the container 3 is sealed, the minimum width ( Figure 1 The minimum width of the inner space of the container 3 in the Y direction) relative to the thickness of the electrode body 2 in the stacking direction ( Figure 1 The upper limit of the ratio of the thickness of the electrode body 2 in the Y direction in the container 3 is preferably 1.20, and more preferably 1.10. When the above ratio is below the above upper limit, the container 3 is easily deformed and presses the electrode body 2 in the stacking direction. It should be noted that the lower limit of the above ratio is not particularly limited, and may be 1.05, for example.
[0032] The pressure (absolute pressure) inside the container 3 is not particularly limited as long as it is smaller than the pressure outside the container 3 (typically atmospheric pressure = 1 atmosphere = 0.1013 MPa). From the viewpoint of better exerting the effect of reducing the expansion of the positive electrode, the pressure inside the container 3 is preferably 0.09 MPa or less, more preferably 0.085 MPa or less, and further preferably 0.075 MPa or less. In some embodiments, the pressure may be 0.07 MPa or less, or 0.065 MPa or less. The lower limit of the pressure inside the container 3 is not particularly limited, and may be 0.02 MPa, for example. From the viewpoint of the negative pressure resistance of the container, the pressure inside the container 3 may be 0.03 MPa or more, or 0.04 MPa or more.
[0033] A gas soluble in a non-aqueous electrolyte is contained in the container 3. By containing a gas soluble in a non-aqueous electrolyte in the sealed container 3, the gas is dissolved in the non-aqueous electrolyte, and the pressure inside the container 3 can be effectively reduced, so that the inside of the container can be more reliably in a negative pressure state.
[0034] Examples of the gas soluble in the non-aqueous electrolyte include carbon dioxide and nitrous oxide. As the gas, carbon dioxide is preferred because it has high solubility in the non-aqueous electrolyte and is easy to handle and obtain.
[0035] In the case of using carbon dioxide as a gas soluble in the above-mentioned non-aqueous electrolyte, the content (concentration) of carbon dioxide in the remaining space inside the container at 1 atmosphere and 25°C is not particularly limited, but from the perspective of making the inside of the container an appropriate negative pressure state, it is preferably 2% by volume or more, more preferably 2.5% by volume or more, and further preferably 3% by volume or more. In some embodiments, the content of the above-mentioned carbon dioxide can be 4% by volume or more, or 5% by volume or more. The upper limit of the content of the above-mentioned carbon dioxide is not particularly limited, and it can be roughly 100% by volume (for example, 80% by volume). The content of the above-mentioned carbon dioxide can be, for example, 50% by volume or less, or 30% by volume or less (for example, 20% by volume or less, typically 15% by volume or less). In the case of using carbon dioxide as a gas soluble in the above-mentioned non-aqueous electrolyte, the content (concentration) of carbon dioxide in the non-aqueous electrolyte inside the container is not particularly limited, but from the perspective of making the inside of the container an appropriate negative pressure state, it is preferably 0.001% by volume or more, and more preferably 0.003% by volume or more. In some embodiments, the content (concentration) of carbon dioxide in the non-aqueous electrolyte solution in the container may be 0.0035% by volume or more, or 0.005% by volume or more.
[0036] As the lower limit of the pressure applied to the electrode body in the state of pressing the electrode body in the stacking direction of the positive and negative electrodes, it is preferably 0.1MPa, and more preferably 0.2MPa. By pressing the electrode body in the stacking direction with a pressure above the above lower limit, the expansion of the positive electrode caused by the cracks of the positive electrode active material particles is suppressed, so that the inhibitory effect of the reduction of the output performance after the charge and discharge cycle can be further improved. As the upper limit of the pressure applied to the above-mentioned electrode body, for example, it can be 5MPa, or it can be 2MPa, 1MPa, 0.5MPa or 0.3MPa. By pressing the electrode body in the stacking direction with a pressure below the above upper limit, the charge and discharge performance can be improved. The above pressure can be above any of the above lower limits and below any of the above upper limits.
[0037] As a method for making the electrode body be pressed (load applied), it is preferred to make the inside of the container be in a negative pressure state. By making the inside of the container in a negative pressure state, the container is deformed in a concave manner in the stacking direction of the positive and negative electrodes, and the electrode body is pressed in the stacking direction of the positive and negative electrodes. In addition to the method of making the inside of the container in a negative pressure state, the method of making the electrode body be pressed can also be carried out using a pressurizing component that pressurizes the container from the outside, for example. The pressurizing component can be a constraining component that constrains the shape of the container. The pressurizing component (constraining component) is, for example, configured to clamp the electrode body from both sides in the thickness direction of the container and pressurize it. The pressurized surface of the electrode body is in contact with the inner surface of the container directly or via other components. Therefore, by pressurizing the container, the electrode body is pressurized. As a pressurizing component, for example, a restraining belt, a metal frame, etc. can be cited. For example, in a metal frame, it can be configured to be able to adjust the load using bolts, etc. Alternatively, a plurality of nonaqueous electrolyte storage elements may be arranged in the thickness direction of the electrode body and fixed using a frame or the like while being pressurized from both ends in the thickness direction. Here, the pressure applied to the electrode body is a value measured by the following method.
[0038] (i) When a load is applied to the non-aqueous electrolyte storage element by a pressurizing member or the like
[0039] First, in a state where a load is applied by a pressure member, the non-aqueous electrolyte storage element is discharged at a constant current to the lower limit voltage during normal use, and then set in an X-ray computed tomography (CT) device. Scan in a direction parallel to the thickness direction of the electrode body to confirm whether the electrode body is in direct or indirect contact with the inner surface of the container. When the electrode body is not in direct or indirect contact with the inner surface of the container, the pressure applied to the electrode body is 0MPa. When the electrode body is in direct or indirect contact with the inner surface of the container, the load applied to the electrode body is measured using an automatic recorder according to the following steps. The non-aqueous electrolyte storage element in a state where a load is applied by a pressure member is set in an automatic recorder. A load sufficiently smaller than the load generated by a pressure member is applied to the non-aqueous electrolyte storage element by an automatic recorder. In this state, that is, in a state where the thickness of the non-aqueous electrolyte storage element is maintained, the load generated by the pressure member is released, and the change in load measured by the automatic recorder is used as the load applied to the electrode body. The value obtained by dividing the load applied to the electrode body by the area of the contact surface between the automatic recorder and the non-aqueous electrolyte storage element is used as the pressure applied to the electrode body. In addition, although a load is usually applied to a pair of opposing surfaces of a nonaqueous electrolyte storage element by a pressurizing member or the like, the area of only one surface of the pair of surfaces is defined as the area of the surface to which the load is applied.
[0040] (ii) When no load is applied to the nonaqueous electrolyte storage element by a pressurizing member or the like
[0041] When the non-aqueous electrolyte storage element is constrained by a constraining member but no load is applied through the constraining member, the pressure applied to the electrode body is measured according to the following steps. First, the non-aqueous electrolyte storage element is discharged at a constant current to the lower limit voltage during normal use, and then placed in an X-ray CT device. Scan in a direction parallel to the thickness direction of the electrode body to confirm whether the electrode body is in direct or indirect contact with the inner surface of the container. When the electrode body is not in direct or indirect contact with the inner surface of the container, the pressure applied to the electrode body is 0MPa. When the electrode body is in direct or indirect contact with the inner surface of the container, an X-ray transmission image of the electrode body is taken to measure the maximum thickness in the stacking direction of the electrode body. Disassemble the non-aqueous electrolyte storage element, take out the electrode body, and place it in an automatic recorder. Using the automatic recorder, gradually apply a load to the electrode body to compress the electrode body to the maximum thickness in the thickness direction of the electrode body measured from the X-ray transmission image. The load measured by the automatic recorder at this time is used as the load applied to the electrode body. The value obtained by dividing the above load by the area of the contact surface between the automatic recorder and the electrode body is used as the pressure applied to the electrode body. In addition, although the load is usually applied to a pair of opposing surfaces of the electrode assembly through the container, the area of only one surface of the pair of surfaces is set as the area of the surface to which the load is applied.
[0042] (positive electrode)
[0043] The positive electrode includes a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0044] The positive electrode substrate has electrical conductivity. Whether it has "electrical conductivity" is determined by measuring the volume resistivity of 10 7 Ω·cm is used as the threshold value for judgment. As the material of the positive electrode substrate, metals such as aluminum, titanium, tantalum, stainless steel, or their alloys can be used. Among them, from the viewpoints of potential resistance, high conductivity and cost, aluminum or aluminum alloys are preferred. As the positive electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be cited. From the viewpoint of cost, foil is preferred. Therefore, aluminum foil or aluminum alloy foil is preferably used as the positive electrode substrate. As aluminum or aluminum alloy, A1085, A3003, A1N30, etc. specified in JIS-H-4000 (2014) or JIS-H-4160 (2006) can be exemplified.
[0045] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, further preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By making the average thickness of the positive electrode substrate within the above range, the strength of the positive electrode substrate can be increased, and the energy density per unit volume of the secondary battery can be increased.
[0046] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer reduces the contact resistance between the positive electrode substrate and the positive electrode active material layer by including a conductive agent such as carbon particles. The composition of the intermediate layer is not particularly limited, and for example, includes a binder and a conductive agent.
[0047] The positive electrode active material layer contains positive electrode active material particles and optionally contains a conductive agent, a binder, a thickener, a filler, and other optional components.
[0048] (Positive electrode active material particles)
[0049] The positive electrode active material particles include a lithium transition metal composite oxide having an α-NaFeO2 structure. The molar ratio (Li / Me) of the lithium element (Li) to the transition metal element (Me) in the above-mentioned lithium transition metal composite oxide exceeds 1.0. In addition, the above-mentioned positive electrode active material particles include a heterogeneous element. The above-mentioned heterogeneous element is an aluminum element, a tungsten element, a boron element, an zinc element, an titanium element or a combination thereof. The above-mentioned heterogeneous element inhibits the decomposition of the lithium compound remaining in the above-mentioned lithium transition metal composite oxide as a synthetic raw material for the above-mentioned lithium transition metal composite oxide, and further inhibits the expansion of the non-aqueous electrolyte storage element caused by the generation of gas. In the positive electrode active material particles of the non-aqueous electrolyte storage element, the content of the lithium element in the lithium transition metal composite oxide relative to the transition metal element exceeds 1.0 in terms of molar ratio, and contains the above-mentioned heterogeneous element, so that even in the case of deep discharge, cracks are not easily generated in the positive electrode active material particles, the expansion of the positive electrode can be reduced, and the expansion of the non-aqueous electrolyte storage element can be inhibited. The heterogeneous element may be contained in the positive electrode active material particles as a component constituting the lithium transition metal composite oxide, or may be contained in the positive electrode active material particles as a component different from the lithium transition metal composite oxide. 1+α (Ni β Co γ Mn δ Y ε ) 1-α O2 (0<α<1, 0≤β<1, 0≤γ<1, 0<δ<1, 0<ε<0.2, β+γ+δ+ε=1, β+γ≠0).
[0050] The lower limit of the content of lithium element (Li) relative to transition metal element (Me) in the above-mentioned lithium transition metal composite oxide, i.e., (1+α) / (1-α), is preferably 1.05, more preferably 1.08, further preferably 1.10, and further preferably 1.15. On the other hand, the upper limit of (1+α) / (1-α) is preferably 1.50, more preferably 1.45, further preferably 1.40, and further preferably 1.35. (1+α) / (1-α) can be above any of the above lower limits and below any of the above upper limits. By making (1+α) / (1-α) above the above lower limit and below the above upper limit, the discharge capacity per unit mass of the lithium transition metal composite oxide is large, and the effect of suppressing the reduction of output performance after charge and discharge cycles is high. It should be noted that the content (ratio of content) of each element in the lithium transition metal composite oxide is an atomic ratio, which is equal to the molar ratio.
[0051] The above transition metal element preferably includes at least one of nickel, cobalt and manganese. The lithium transition metal composite oxide can be composed of Li1+α (Ni β Co γ Mn δ ) 1-α O2 (0<α<1, 0≤β≤1, 0≤γ≤1, 0≤δ≤1, β+γ+δ=1) represents.
[0052] The molar ratio (Mn / Me) of Mn to the transition metal element (Me) in the above-mentioned lithium transition metal composite oxide, i.e., δ, can be, for example, 0.10 to 0.80, preferably 0.35 to 0.65, and more preferably 0.40 to 0.60. By making Mn / Me greater than 0.10, the output performance of the non-aqueous electrolyte storage element can be improved. By making Mn / Me less than 0.80, the dissolution of Mn from the positive electrode active material particles can be suppressed, and the reduction in the output performance of the non-aqueous electrolyte storage element after the charge and discharge cycle can be further suppressed, and the output performance, etc. are also improved. In particular, when Mn / Me is 0.40 to 0.60, a high discharge capacity can be obtained even without the high potential formation described later, so it is more preferred.
[0053] When the lithium transition metal composite oxide is 1.3≤(1+α) / (1-α) and 0.5<Mn / Me, in order to activate the lithium transition metal composite oxide, it is preferred to perform the positive electrode potential to 4.5V vs. Li / Li + In this way, when the high potential formation is performed, the symmetry of the crystal changes with the release of lithium in the crystal, and thus the diffraction peak with a diffraction angle 2θ in the range of 20° to 22° in the X-ray diffraction pattern of the lithium transition metal composite oxide using CuKα rays disappears.
[0054] On the other hand, when the lithium transition metal composite oxide is 1.0<(1+α) / (1-α)<1.3 and 0.4≤Mn / Me≤0.6, the high potential formation causes a change in the crystal structure in the direction of reducing the diffusion rate of lithium ions in the solid phase, so there is a risk of increasing the internal resistance with the charge and discharge cycle, so it is preferably not performed at high potential. In this case, in the X-ray diffraction pattern of the lithium transition metal composite oxide using CuKα rays, there is a diffraction peak in the range of diffraction angle 2θ of 20° to 22°.
[0055] The content of Ni in the lithium transition metal composite oxide relative to the transition metal element (Me) (Ni / Me), i.e., β, can be, for example, 0.10 to 0.80, preferably 0.20 to 0.70, and more preferably 0.30 to 0.60. By making Ni / Me greater than 0.10, the output performance, energy density, etc. of the non-aqueous electrolyte storage element can be improved. By making Ni / Me less than 0.80, the output performance, etc. of the non-aqueous electrolyte storage element can be improved.
[0056] The content (Co / Me) of Co in the above-mentioned lithium transition metal composite oxide relative to the transition metal element (Me), i.e., γ, can be, for example, 0 to 0.60, or 0.10 to 0.30. By making Co / Me greater than 0.10, the output performance, energy density, etc. of the non-aqueous electrolyte storage element can be improved. On the other hand, by making Co / Me less than 0.60, the output performance of the non-aqueous electrolyte storage element can be improved while suppressing the cost of raw materials, etc. Co / Me can also be 0.
[0057] The non-aqueous electrolyte storage element can suppress the reduction of output performance after charge and discharge cycles by dispersing and existing the above-mentioned heterogeneous elements near the center and near the surface of the positive electrode active material particles containing the above-mentioned lithium transition metal composite oxide. By including the above-mentioned heterogeneous elements near the center of the above-mentioned positive electrode active material particles, there is a tendency to suppress the fine crystal structure changes during the charge and discharge cycle and suppress the reduction of output performance after the charge and discharge cycle. In addition, it is preferred that the above-mentioned transition metal element contains at least one of nickel, cobalt and manganese, and the ratio of the molar number of the heterogeneous element to the sum of the molar numbers of nickel, cobalt, manganese and heterogeneous elements is higher near the surface of the above-mentioned positive electrode active material particles than near the center. The ratio of the molar number of the above-mentioned heterogeneous elements near the surface of the above-mentioned positive electrode active material particles to the sum of the molar numbers of nickel, cobalt, manganese and heterogeneous elements is high in the molar number of the above-mentioned heterogeneous elements near the center of the above-mentioned positive electrode active material particles, which can further improve the suppression effect of the reduction of output performance after the charge and discharge cycle of the non-aqueous electrolyte storage element.
[0058] The lower limit of the ratio of the number of moles of the heterogeneous elements in the positive electrode active material particles to the sum of the number of moles of the nickel element, the cobalt element, the manganese element and the heterogeneous elements is preferably 0.2 mol%, more preferably 0.3 mol%, and further preferably 0.5 mol%. On the other hand, the upper limit of the ratio of the number of moles of the above heterogeneous elements is preferably 6.0 mol%, more preferably 4.0 mol%, and further preferably 3.0 mol%. By making the ratio of the number of moles of the heterogeneous elements in the positive electrode active material particles to the sum of the number of moles of the nickel element, the cobalt element, the manganese element and the heterogeneous elements greater than the lower limit and less than the upper limit, the reduction in the output performance of the nonaqueous electrolyte storage element after the charge and discharge cycle can be further suppressed.
[0059] The lithium transition metal composite oxide may contain other transition metal elements and the like within a range that exhibits the effects of the present invention, and may contain other foreign elements and the like other than the above-mentioned foreign elements as impurities.
[0060] The positive electrode active material layer may contain other positive electrode active material particles in addition to the above-mentioned lithium transition metal composite oxide. As other positive electrode active material particles, they can be appropriately selected from known positive electrode active material particles commonly used in lithium ion secondary batteries, etc. As the above-mentioned other positive electrode active material particles, materials that can occlude and release lithium ions are generally used. For example, lithium transition metal oxides, polyanionic compounds, chalcogen compounds, sulfur, etc. having the above-mentioned LiMeO2 type active material, spinel-type crystal structures can be cited. Among them, the content of the above-mentioned lithium transition metal composite oxide in all the positive electrode active material particles contained in the positive electrode active material layer is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 99% by mass or more, and particularly preferably 100% by mass.
[0061] The average particle size of the positive electrode active material particles is, for example, preferably 0.1 μm to 20 μm. By making the average particle size of the positive electrode active material particles greater than the above lower limit, the manufacture or handling of the positive electrode active material particles becomes easy. By making the average particle size of the positive electrode active material particles less than the above upper limit, the electronic conductivity of the positive electrode active material layer is improved. It should be noted that when a composite of positive electrode active material particles and other materials is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material particles. "Average particle size" refers to the particle size distribution measured by the laser diffraction / scattering method of the diluted solution obtained by diluting the particles with a solvent in accordance with JIS-Z-8825 (2013), based on the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) as 50%.
[0062] In order to obtain particles such as positive electrode active material particles with a predetermined particle size, a pulverizer, a classifier, etc. can be used. As a pulverization method, for example, a method using a mortar, a ball mill, a sand mill, a vibrating ball mill, a planetary ball mill, a jet mill, a reverse jet mill, a rotating airflow jet mill or a sieve can be cited. During pulverization, wet pulverization in which a non-aqueous solvent such as water or hexane coexists can also be used. As a classification method, a dry, wet sieve, a wind classifier, etc. can be used as needed.
[0063] The content of the positive electrode active material particles in the positive electrode active material layer is preferably 50% to 99% by mass, more preferably 70% to 98% by mass, and further preferably 80% to 95% by mass. By making the content of the positive electrode active material particles within the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.
[0064] The conductive agent is not particularly limited as long as it is a material with conductivity. As such a conductive agent, for example, carbonaceous materials, metals, conductive ceramics, etc. can be mentioned. As carbonaceous materials, graphite, non-graphite carbon, graphene-based carbon, etc. can be mentioned. As non-graphite carbon, carbon nanofibers, pitch-based carbon fibers, carbon black, etc. can be mentioned. As carbon black, furnace black, acetylene black, Ketjen black, etc. can be mentioned. As graphene-based carbon, graphene, carbon nanotubes (CNT), fullerene, etc. can be mentioned. As the shape of the conductive agent, powder, fiber, etc. can be mentioned. As the conductive agent, one of these materials can be used alone, or two or more can be mixed and used. In addition, these materials can also be used in a composite. For example, a material after carbon black and CNT composite can be used. Among them, from the viewpoint of electronic conductivity and coating properties, carbon black is preferred, and acetylene black is preferred.
[0065] The content of the conductive agent in the positive electrode active material layer is preferably 1% to 10% by mass, and more preferably 3% to 9% by mass. When the content of the conductive agent is within the above range, the energy density of the secondary battery can be increased.
[0066] Examples of adhesives include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic acid, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.
[0067] The content of the binder in the positive electrode active material layer is preferably 1% by mass to 10% by mass, and more preferably 3% by mass to 9% by mass. When the content of the binder is within the above range, the active material can be stably retained.
[0068] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the thickener has a functional group that reacts with lithium or the like, the functional group may be inactivated in advance by methylation or the like.
[0069] The filler is not particularly limited. As the filler, there can be mentioned polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, aluminum oxide, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, and other materials derived from mineral resources or their artificial products, etc.
[0070] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metals such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than positive electrode active material particles, conductive agents, binders, thickeners, and fillers.
[0071] (Method for producing positive electrode active material particles)
[0072] As a method for producing positive electrode active material particles, there are exemplified (1) a method of drying after immersing a particulate positive electrode active material in a liquid in which a heterogeneous element compound (compound containing a heterogeneous element) is dissolved or suspended; (2) a method of reacting after immersing a particulate positive electrode active material in a liquid in which a heterogeneous element compound is dissolved or suspended by heating or the like; (3) a method of firing a mixture containing a positive electrode active material precursor, a lithium compound and a heterogeneous element compound; (4) a method of firing a mixture containing a heterogeneous element compound and a particulate positive electrode active material; (5) a method of firing a mixture containing a heterogeneous element positive electrode active material precursor and a lithium compound, etc. In particular, in (5), by making the state in which the heterogeneous element is contained on the particle surface at the stage of preparing the positive electrode active material precursor, it is easy to adjust so that more heterogeneous elements are contained near the surface of the above-mentioned positive electrode active material particles than near the center. Specifically, the positive electrode active material particles are prepared by dripping an aqueous solution containing nickel, cobalt, manganese, etc. and an aqueous solution containing heterogeneous elements and mixing them, and then firing the mixture containing the positive electrode active material precursor and the lithium compound, thereby easily and appropriately adjusting the ratio of the molar number of heterogeneous elements near the center and near the surface of the positive electrode active material particles to the sum of the molar numbers of nickel, cobalt, manganese and heterogeneous elements. The method for producing positive electrode active material particles according to the method (5) above is described in detail below.
[0073] The positive electrode active material precursor is preferably a coprecipitated precursor in which nickel element, cobalt element, manganese element, a different element, or the like exists in one particle.
[0074] The above-mentioned coprecipitation precursor is made using a reaction crystallization method. Here, as the above-mentioned coprecipitation precursor, a hydroxide precursor and a carbonate precursor can usually be cited. Here, in the method for manufacturing a carbonate precursor, the crystallization speed is fast, and the content of heterogeneous elements near the center and the surface of the positive electrode active material particles is difficult to control. On the other hand, in the method for manufacturing a hydroxide precursor, by applying a complexing agent, it is easy to control the crystallization speed, so it is easy to adjust the content of heterogeneous elements near the center and the surface of the positive electrode active material particles. From this viewpoint, it is preferred to manufacture a hydroxide precursor as a method for a coprecipitation precursor.
[0075] When manufacturing the above-mentioned hydroxide precursor, preferably in the aqueous solution in the reaction tank maintaining alkalinity, together with the aqueous solution containing transition metal element (Me) and heterogeneous element, an alkaline aqueous solution containing alkali metal hydroxide (neutralizing agent), complexing agent and reducing agent is added dropwise to make transition metal hydroxide and heterogeneous element hydroxide coprecipitate. As complexing agent, ammonia (NH3), ammonium sulfate, ammonium nitrate etc. can be used. As reducing agent, hydrazine, sodium borohydride etc. can be used. As alkali metal hydroxide, sodium hydroxide, lithium hydroxide, potassium hydroxide etc. can be used.
[0076] When manufacturing the above-mentioned carbonate precursor, it is preferred that an alkaline aqueous solution containing a neutralizing agent and a complexing agent such as sodium carbonate and lithium carbonate is added dropwise to an aqueous solution in a reaction tank maintained at an alkaline state, together with an aqueous solution containing a transition metal element (Me) and a heterogeneous element, so that the transition metal carbonate and the heterogeneous element carbonate are co-precipitated.
[0077] As the raw material of the coprecipitation precursor, nickel compounds, cobalt compounds and manganese compounds containing nickel, cobalt and manganese as transition metal elements (Me) can be used. As nickel compounds, nickel hydroxide, nickel carbonate, nickel sulfate, nickel nitrate, nickel acetate and the like can be mentioned. As cobalt compounds, cobalt sulfate, cobalt nitrate, cobalt acetate and the like can be mentioned. As manganese compounds, manganese oxide, manganese carbonate, manganese sulfate, manganese nitrate, manganese acetate and the like can be mentioned. In addition, aluminum compounds, tungsten compounds, boron compounds, zinc compounds and titanium compounds containing aluminum, tungsten, boron, zinc, titanium or their combinations as heterogeneous elements can be used. As aluminum compounds, aluminum hydroxide, aluminum sulfate, aluminum nitrate, aluminum acetate and the like can be mentioned. As tungsten compounds, tungsten trioxide, tungsten dioxide, lithium tungstate and the like can be mentioned. As boron compounds, boric acid (orthoboric acid), boron oxide and the like can be mentioned.
[0078] When making the coprecipitation precursor, the manganese element is easily oxidized, so for example it is not easy to make the coprecipitation precursor in which the nickel element, the cobalt element and the manganese element are uniformly distributed in a divalent state, and the uniform mixing of the nickel element, the cobalt element and the manganese element at the atomic level is easily insufficient. Therefore, in order to suppress the oxidation of the manganese element present in the coprecipitation precursor, it is preferred to remove the dissolved oxygen in each aqueous solution used. As a method for removing dissolved oxygen, a method for bubbling using an oxygen-free gas can be enumerated. As an oxygen-free gas, it is not limited, and nitrogen, argon, carbon dioxide gas etc. can be enumerated.
[0079] For the dropwise addition of the raw aqueous solution, it is preferred to drop an aqueous solution containing a transition metal element (Me) and an aqueous solution containing a foreign element separately. According to this method, the foreign element and the transition metal element (Me) are not easily dispersed uniformly. More specifically, the transition metal hydroxide and the foreign element hydroxide are not easily mixed uniformly. As a result, it is easy to adjust the content of the foreign element near the center and near the surface of the positive electrode active material particles. There are no particular restrictions on the pH of the aqueous solution when preparing the coprecipitation precursor in the aqueous solution, the dropping speed of the raw aqueous solution, etc., and conditions of the same degree as the conventionally known manufacturing conditions can be adopted. The pH of the aqueous solution may be, for example, 8 to 11, or 9.5 to 10.5. In addition, the dropping speed of the raw aqueous solution may be, for example, 0.1 cm 3 / min~10cm 3 / minute.
[0080] In the presence of a complexing agent such as NH3 in the reaction tank and under certain convection conditions, the rotation of the coprecipitation precursor particles and the revolution in the stirring tank are promoted by further continuous stirring after the addition of the raw material aqueous solution is completed. In this process, the coprecipitation precursor particles collide with each other and the coprecipitation precursor particles grow into concentric spheres in stages. That is, the coprecipitation precursor is formed by the reaction of the metal complex formation reaction when the raw material aqueous solution is added dropwise to the reaction tank and the precipitation formation reaction generated by the metal complex in the retention of the reaction tank.
[0081] The preferred stirring duration after the dropwise addition of the raw material aqueous solution, i.e., the reaction time, is also affected by the size of the reaction tank, stirring conditions, pH, reaction temperature, etc., and is, for example, preferably 0.5 to 20 hours, more preferably 1 to 15 hours.
[0082] By mixing and firing the coprecipitation precursor (positive electrode active material precursor) obtained by the above method and the lithium compound, positive electrode active material particles are obtained. As the lithium compound, lithium hydroxide, lithium carbonate, etc. can be used. In addition, together with these lithium compounds, lithium fluoride (LiF), lithium sulfate (Li2SO4) or lithium phosphate (Li3PO4) can be used as a sintering aid. The addition ratio of these sintering aids is preferably 1 mol% to 10 mol% relative to the total amount of the lithium compound. It should be noted that it is expected that a part of the lithium compound disappears during firing, and the total amount of the lithium compound is preferably over-added by about 1 mol% to 5 mol%.
[0083] The firing temperature is preferably 750°C to 1000°C. By setting the firing temperature to be above the lower limit, positive electrode active material particles with a high degree of sintering can be obtained, and the charge-discharge cycle performance can be improved. On the other hand, by setting the firing temperature to be below the upper limit, the reduction in discharge performance caused by the structural change from the layered α-NaFeO2 structure to the rock salt type cubic structure can be suppressed.
[0084] (negative electrode)
[0085] The negative electrode comprises a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The structure of the intermediate layer is not particularly limited, and can be selected from the structures exemplified in the above-mentioned positive electrode.
[0086] The negative electrode substrate has conductivity. As the material of the negative electrode substrate, metals such as copper, nickel, stainless steel, nickel-plated steel, aluminum, or their alloys, carbonaceous materials, etc. can be used. Among them, copper or copper alloys are preferred. As the negative electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be cited. From the perspective of cost, foil is preferred. Therefore, copper foil or copper alloy foil is preferably used as the negative electrode substrate. As examples of copper foil, rolled copper foil, electrolytic copper foil, etc. can be cited.
[0087] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate to the above range, the strength of the negative electrode substrate can be increased, and the energy density per unit volume of the secondary battery can be increased.
[0088] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains any component such as a conductive agent, a binder, a thickener, and a filler as needed. The conductive agent, the binder, the thickener, the filler, and any component can be selected from the materials exemplified in the positive electrode.
[0089] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, transition metals such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, W as ingredients other than the negative electrode active material, conductive agent, binder, thickener and filler.
[0090] The negative electrode active material can be appropriately selected from known negative electrode active materials. As the negative electrode active material for lithium ion secondary batteries, materials that can absorb and release lithium ions are generally used. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 , LiTiO2, TiNb2O7 and other titanium-containing oxides; polyphosphate compounds; silicon carbide; graphite, non-graphite carbon (easy graphitization carbon or difficult graphitization carbon) and other carbon materials. Among these materials, when carbon dioxide is contained in the interior of the container as a gas soluble in a non-aqueous electrolyte, carbon dioxide reacts with lithium ions in the non-aqueous electrolyte to become lithium carbonate and precipitate on the surface of the negative electrode, and the interior of the container is easily in a negative pressure state, it is preferred that the negative electrode potential when lithium ions are absorbed is 1V vs. Li / Li + Of the following materials, Si, Si oxides, and carbon materials are more preferred, carbon materials are further preferred, and graphite and non-graphite carbon are further preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0091] “Graphite” refers to the average lattice spacing (d) of the (002) plane determined by X-ray diffraction before charge or discharge or in the discharged state. 002 ) is a carbon material having a diameter of 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. From the perspective of obtaining a material with stable physical properties, artificial graphite is preferred.
[0092] “Non-graphite carbon” refers to the average lattice spacing (d ) of the (002) plane determined by X-ray diffraction before charge / discharge or during discharge. 002 ) is a carbon material having a carbon thickness of 0.34 nm to 0.42 nm. Examples of non-graphite carbon include difficult-graphitization carbon and easy-graphitization carbon. Examples of non-graphite carbon include materials derived from resins, petroleum asphalt or materials derived from petroleum asphalt, petroleum coke or materials derived from petroleum coke, materials derived from plants, materials derived from alcohols, and the like.
[0093] Here, the "discharge state" of carbon materials such as graphite refers to a state in which the carbon material as the negative electrode active material is discharged in a manner such that ions such as lithium that can be absorbed and released during charge and discharge are fully released. For example, the following state: in a half-cell using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic lithium (Li) as a counter electrode, the open circuit voltage is 0.7V or more.
[0094] "Difficult to graphitize carbon" refers to the above-mentioned 002 It is a carbon material with a diameter of 0.36nm to 0.42nm.
[0095] "Easily graphitizable carbon" refers to the above-mentioned 002 A carbon material having a diameter of 0.34 nm or more and less than 0.36 nm.
[0096] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be set to, for example, 1 nm to 100 μm. When the negative electrode active material is a carbon material, a titanium-containing oxide or a polyphosphate compound, its average particle size can be 1 μm to 100 μm. When the negative electrode active material is Si, Sn, Si oxide or Sn oxide, etc., its average particle size can be 1 nm to 1 μm. By making the average particle size of the negative electrode active material above the above lower limit, the manufacture or handling of the negative electrode active material becomes easy. By making the average particle size of the negative electrode active material below the above upper limit, the electronic conductivity of the active material layer is improved. In order to obtain a powder with a specified particle size, a pulverizer, a classifier, etc. can be used. The pulverization method and the classification method can be selected, for example, from the methods exemplified in the above-mentioned positive electrode. When the negative electrode active material is a metal such as metal Li, the negative electrode active material can be in the form of foil.
[0097] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% to 99% by mass, more preferably 90% to 98% by mass. When the content of the negative electrode active material is within the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0098] (Isolator)
[0099] The separator can be appropriately selected from known separators. As the separator, for example, a separator consisting only of a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and an adhesive is formed on one surface or both surfaces of the substrate layer, etc. can be used. As the shape of the substrate layer of the separator, for example, woven fabrics, non-woven fabrics, porous resin films, etc. can be cited. Among these shapes, porous resin films are preferred from the viewpoint of strength, and non-woven fabrics are preferred from the viewpoint of liquid retention of non-aqueous electrolytes. As the material of the substrate layer of the separator, from the viewpoint of insulation function, for example, polyolefins such as polyethylene and polypropylene are preferred, and from the viewpoint of resistance to oxidative decomposition, for example, polyimides, aromatic polyamides, etc. are preferred. As the substrate layer of the separator, a material composited with these resins can also be used.
[0100] The heat-resistant particles contained in the heat-resistant layer preferably have a mass reduction of 5% or less when the temperature is increased from room temperature to 500°C in an air atmosphere of 1 atmosphere, and more preferably have a mass reduction of 5% or less when the temperature is increased from room temperature to 800°C. As materials whose mass reduction is less than the prescribed value, inorganic compounds can be cited. As inorganic compounds, for example, oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminum silicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, and other mineral resources or their artificial products. As inorganic compounds, simple substances or composites of these substances can be used alone, or two or more can be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of safety of the nonaqueous electrolyte storage element.
[0101] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, the "porosity" is a value based on volume, and refers to a value measured using a mercury porosimeter.
[0102] As a separator, a polymer gel composed of a polymer and a non-aqueous electrolyte can be used. Examples of the polymer include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, and polyvinylidene fluoride. If a polymer gel is used, leakage can be suppressed. As a separator, a porous resin film or nonwoven fabric as described above can also be used in combination with a polymer gel.
[0103] (Non-aqueous electrolyte)
[0104] The non-aqueous electrolyte solution may be appropriately selected from known non-aqueous electrolyte solutions. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.
[0105] As nonaqueous solvent, it can be suitably selected from known nonaqueous solvents. As nonaqueous solvent, cyclic carbonate, linear carbonate, carboxylate, phosphoric acid ester, sulfonic acid ester, ether, amides, nitrile etc. can be enumerated. As nonaqueous solvent, it is also possible to use the solvent after a part of the hydrogen atom included in these compounds is replaced by halogen.
[0106] Examples of the cyclic carbonate include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among them, EC is preferred.
[0107] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among them, EMC is preferred.
[0108] As the non-aqueous solvent, preferably cyclic carbonate or linear carbonate is used, more preferably cyclic carbonate and linear carbonate are used in combination. By using cyclic carbonate, the dissociation of electrolyte salt can be promoted and the ion conductivity of non-aqueous electrolyte can be improved. By using linear carbonate, the viscosity of non-aqueous electrolyte can be suppressed to be low. In the case of using cyclic carbonate and linear carbonate in combination, as the volume ratio of cyclic carbonate and linear carbonate (cyclic carbonate: linear carbonate), for example, preferably in the range of 5:95 to 50:50.
[0109] The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, Among them, lithium salts are preferred.
[0110] As lithium salts, inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium salts having halogenated hydrocarbon groups such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3 can be cited. Among them, inorganic lithium salts are preferred, and LiPF6 is more preferred.
[0111] The content of the electrolyte salt in the non-aqueous electrolyte is preferably 0.1 mol / dm 3 ~2.5mol / dm 3 , more preferably 0.3 mol / dm 3 ~2.0mol / dm 3 , more preferably 0.5 mol / dm 3 ~1.7mol / dm 3, particularly preferably 0.7 mol / dm 3 ~1.5mol / dm 3 By setting the content of the electrolyte salt to be within the above range, the ion conductivity of the non-aqueous electrolyte can be improved.
[0112] In addition to the non-aqueous solvent and the electrolyte salt, the non-aqueous electrolyte may also contain additives. Examples of additives include oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partial hydride of terphenyl, cyclohexylbenzene, tert-butylbenzene, tert-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; and oxadiene carbonate. Vinyl ester, methyl vinylene carbonate, ethyl vinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; vinyl sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, vinyl sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiapentane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiapentane, thioanisole, diphenyl disulfide, bipyridine disulfide, 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tri(trimethylsilyl) borate, tri(trimethylsilyl) phosphate, tetra(trimethylsilyl) titanate, monofluorolithium phosphate, difluorolithium phosphate, etc. These additives may be used alone or in combination of two or more.
[0113] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% to 10% by mass, more preferably 0.1% to 7% by mass, further preferably 0.2% to 5% by mass, and particularly preferably 0.3% to 3% by mass, relative to the overall mass of the non-aqueous electrolyte. By making the content of the additive within the above range, the capacity retention performance or cycle performance after high temperature storage can be improved, or the safety can be further improved.
[0114] The shape of the non-aqueous electrolyte storage element of this embodiment is not particularly limited, and for example, a flat square battery is preferred. Since the shape of the non-aqueous electrolyte storage element is a flat square battery, when the inside of the container is in a negative pressure state, a force is generated to pull the container inward, and the electrode body is pressed in the stacking direction of the positive electrode and the negative electrode. As a result, the expansion of the positive electrode caused by the cracks in the positive electrode active material particles is suppressed, and the reduction in output performance after the charge and discharge cycle can be further reduced.
[0115] <Configuration of power storage device>
[0116] The non-aqueous electrolyte storage element of the present embodiment can be used as a storage device having a storage unit (battery module) composed of a plurality of non-aqueous electrolyte storage elements and can be mounted on a power supply for vehicles such as electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), a power supply for electronic devices such as personal computers and communication terminals, or a power supply for power storage, etc. In this case, the technology of the present invention can be applied to at least one non-aqueous electrolyte storage element included in the storage device.
[0117] A power storage device according to another embodiment of the present invention includes two or more non-aqueous electrolyte power storage elements and one or more non-aqueous electrolyte power storage elements according to one embodiment of the present invention (hereinafter referred to as the "second embodiment"). The technology of one embodiment of the present invention may be applied to at least one non-aqueous electrolyte power storage element included in the power storage device according to the second embodiment, and the power storage device may include one non-aqueous electrolyte power storage element according to one embodiment of the present invention and one or more non-aqueous electrolyte power storage elements unrelated to one embodiment of the present invention, or two or more non-aqueous electrolyte power storage elements according to one embodiment of the present invention may be included.
[0118] Figure 2 2 shows an example of a power storage device 30 of the second embodiment in which power storage units 20 formed by collecting two or more electrically connected non-aqueous electrolyte power storage elements 1 are further collected. The power storage device 30 may include a bus bar (not shown) that electrically connects the two or more non-aqueous electrolyte power storage elements 1, a bus bar (not shown) that electrically connects the two or more power storage units 20, and the like. The power storage unit 20 or the power storage device 30 may include a state monitoring device (not shown) that monitors the state of one or more non-aqueous electrolyte power storage elements 1.
[0119] <Method for producing non-aqueous electrolyte storage element>
[0120] The manufacturing method of the non-aqueous electrolyte storage element of this embodiment can be appropriately selected from known methods. The manufacturing method, for example, comprises: preparing an electrode body, preparing a non-aqueous electrolyte, storing the electrode body and the non-aqueous electrolyte in a container, storing a gas soluble in the non-aqueous electrolyte in the container, and sealing the container. In this embodiment, after storing the gas soluble in the non-aqueous electrolyte in the container and sealing the container, the inside of the container is made into a negative pressure state by dissolving the gas soluble in the non-aqueous electrolyte in the non-aqueous electrolyte. Preparing an electrode body comprises: preparing a positive electrode and a negative electrode, and stacking or winding the positive electrode and the negative electrode through an isolator to form an electrode body.
[0121] The positive electrode can be prepared by applying the positive electrode mixture paste directly or via an intermediate layer to the positive electrode substrate and drying. The positive electrode mixture paste contains various components constituting the positive electrode active material layer (positive electrode mixture) such as positive electrode active material particles and a dispersion medium. A suitable method for manufacturing positive electrode active material particles is as described above.
[0122] The negative electrode can be prepared by, for example, applying a negative electrode mixture paste directly or via an intermediate layer to a negative electrode substrate and drying the paste. The negative electrode mixture paste contains components constituting a negative electrode active material layer (negative electrode mixture) such as a negative electrode active material and a dispersion medium.
[0123] The nonaqueous electrolyte solution may be stored in the container by appropriately selecting from known methods. For example, the nonaqueous electrolyte solution may be injected from an injection port formed in the container and then the injection port may be sealed.
[0124] After the nonaqueous electrolyte is contained in the container, the gas soluble in the nonaqueous electrolyte is contained in the container. Specifically, after the nonaqueous electrolyte is contained in the above-mentioned container, the gas soluble in the nonaqueous electrolyte is injected into the container from the injection port, thereby the gas soluble in the nonaqueous electrolyte is contained in the container. The injection of the gas soluble in the nonaqueous electrolyte can be implemented under atmospheric pressure, or it can be implemented under the state where the pressure inside the container is decompressed using a vacuum pump, etc. Here, "decompression" refers to that the pressure of the remaining space inside the container is less than atmospheric pressure. It should be noted that if the above-mentioned gas is contained in the container until the inside of the container becomes a pressurized state, the above-mentioned gas is too much dissolved in the nonaqueous electrolyte before the sealing, so there is a risk that the above-mentioned gas is difficult to further dissolve in the nonaqueous electrolyte after the container is sealed, and the inside of the container will not fully become a negative pressure state, so it is not preferred. In addition, the injection port can also be separately arranged from the injection port for injecting the nonaqueous electrolyte.
[0125] In this way, by injecting a gas soluble in a nonaqueous electrolyte into a container containing a nonaqueous electrolyte, after the container is sealed, the pressure inside the container is effectively reduced by the above-mentioned gas dissolving in the nonaqueous electrolyte, and the inside of the container can be in a proper negative pressure state. On the other hand, after the gas soluble in the above-mentioned nonaqueous electrolyte is stored in the above-mentioned container, in the method of storing the above-mentioned nonaqueous electrolyte in the container, when the above-mentioned nonaqueous electrolyte is stored, the gas soluble in the above-mentioned nonaqueous electrolyte is mostly dissolved in the nonaqueous electrolyte, and before the container is sealed, the gas soluble in the above-mentioned nonaqueous electrolyte is excessively dissolved in the above-mentioned nonaqueous electrolyte (for example, saturated dissolution), so there is a risk that the above-mentioned gas is difficult to further dissolve in the nonaqueous electrolyte after the container is sealed, and the inside of the container will not fully become a negative pressure state, so it is not preferred.
[0126] As the storage capacity of the gas soluble in the above-mentioned non-aqueous electrolyte contained in the interior of the container, from the viewpoint of further reducing the pressure inside the above-mentioned container, the volume of the remaining space inside the container is preferably 40% by volume or more, more preferably 70% by volume or more, for example, 95% by volume or more. As the storage capacity of the gas soluble in the above-mentioned non-aqueous electrolyte, the volume of the remaining space inside the container can be 100% by volume. Here, "the volume of the remaining space in the container" refers to the volume obtained by subtracting the volume of the structure such as the electrode body, non-aqueous electrolyte and collector from the internal volume of the container. In addition, the volume of the electrode body refers to the apparent volume of the constituent elements (electrodes, separators, etc.) of the electrode body, and does not include the gaps between the electrodes and in the separator.
[0127] From the viewpoint of further reducing the pressure inside the above-mentioned container, the content of the gas soluble in the above-mentioned non-aqueous electrolyte contained in the container is preferably 80 volume % or more, preferably 98 volume % or more, and more preferably 100 volume % relative to the storage amount of all the gases contained in the container. From the viewpoint of the ease of handling of the above-mentioned gas, the content of the gas soluble in the above-mentioned non-aqueous electrolyte can be 80 volume % or less relative to the storage amount of all the gases contained in the container.
[0128] The container is sealed in a state where the gas soluble in the non-aqueous electrolyte is contained in the container. Specifically, the non-aqueous electrolyte storage element can be obtained by sealing the injection port after containing the gas soluble in the non-aqueous electrolyte in the container. The sealing of the injection port is performed, for example, by plugging the injection port with a sealing member and fixing the sealing member by laser welding or the like.
[0129] The period from the time when the gas soluble in the non-aqueous electrolyte is contained in the container until the injection port is sealed may include temporarily sealing the injection port. Temporarily sealing the injection port includes, for example, temporarily plugging the injection port using a rubber plug member or the like. By temporarily sealing the injection port, it is possible to suppress the gas soluble in the non-aqueous electrolyte contained in the container from being released to the outside of the container via the injection port due to diffusion. In this case, when sealing the injection port, the injection port may be plugged with a sealing member after the plug member or the like is removed, and the sealing member may be fixed by laser welding or the like. In addition, when sealing the injection port, a sealing member such as a plug member that covers the entire plugging of the injection port may be configured, and the sealing member may be fixed by laser welding or the like.
[0130] The details of the electrode body, the nonaqueous electrolyte solution, the gas soluble in the nonaqueous electrolyte solution, the container, etc. in the method for producing the nonaqueous electrolyte storage element are as described above.
[0131] <Other embodiments>
[0132] It should be noted that the nonaqueous electrolyte storage element of the present invention is not limited to the above-mentioned embodiment, and various changes can be made within the scope of the present invention. For example, the structure of other embodiments can be added to the structure of one embodiment, and in addition, a part of the structure of one embodiment can be replaced by the structure of other embodiments or known technology. Furthermore, a part of the structure of one embodiment can be deleted. In addition, known technology can be added to the structure of one embodiment.
[0133] In the above embodiment, the case where the non-aqueous electrolyte storage element is used as a non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) that can be charged and discharged is described, but the type, shape, size, capacity, etc. of the non-aqueous electrolyte storage element are arbitrary. The present invention can also be applied to various secondary batteries, double-layer capacitors, or capacitors such as lithium ion capacitors.
[0134] Example
[0135] The present invention is further described below by way of examples. The present invention is not limited to the following examples.
[0136] [Example 1]
[0137] (Preparation of Hydroxide Precursor)
[0138] When preparing positive electrode active material particles, a hydroxide precursor (positive electrode active material precursor) was prepared by a reaction crystallization method. First, 415.9 g of nickel sulfate hexahydrate, 160.6 g of cobalt sulfate heptahydrate, and 445.1 g of manganese sulfate pentahydrate were weighed and dissolved in 4 L of ion exchange water to prepare a 1.0 mol / dm 3 In addition, 20.3 g of aluminum sulfate decahydrate was weighed and dissolved in 0.08 L of ion exchange water to prepare a 0.5 mol / dm 3 of aluminum sulfate aqueous solution. Next, 2 L of ion exchange water is injected into a reaction tank with an internal volume of 5 L and an inner diameter of 200 mm, and nitrogen is bubbled for 30 minutes to remove oxygen contained in the ion exchange water. The temperature of the reaction tank is set to 50°C (±2°C), and the reaction tank is stirred at a rotation speed of 1200 rpm using a paddle equipped with a stirring motor while sufficient convection is performed in the reaction tank. Next, the above-mentioned sulfate aqueous solution is added to the reaction tank at a rate of 4 mL / min and the above-mentioned aluminum sulfate aqueous solution is added to the reaction tank at a rate of 0.08 mL / min from different nozzles spaced at a distance of 10 mm to 50 mm for 17 hours. Here, from the start to the end of the dropwise addition, a solution of 2.0 mol / dm 3 of sodium hydroxide, 0.2 mol / dm 3 of ammonia and 0.2 mol / dm 3 The mixed alkali aqueous solution composed of hydrazine is controlled so that the pH in the reaction tank is always maintained at 11.0 ± 0.1, and a part of the reaction solution is discharged by overflow, so that the convection in the tank is controlled to occur continuously. After the dropwise addition is completed, the stirring in the reaction tank is further continued for 1 hour. After the stirring stops, it is allowed to stand at room temperature for more than 3 hours. Next, the hydroxide precursor particles generated in the reaction tank are separated using a suction filtration device, and the sodium ions attached to the particles are further removed by washing with ion exchange water, and an electric furnace is used in an air atmosphere and under normal pressure, and dried at 80 ° C for 12 hours. Then, in order to make the particle size consistent, it is crushed for a few minutes with an automatic mortar made of agate.
[0139] (Preparation of Positive Electrode Active Material Particles)
[0140] Lithium hydroxide monohydrate was added to the obtained hydroxide precursor, and the mixture was thoroughly mixed using an agate automatic mortar to prepare a mixed powder having a molar ratio of Li: (Ni, Co, Mn) of 1.09: 0.91. After the mixed powder was formed into particles, it was placed on an alumina boat and heated from room temperature to 900°C in an air atmosphere and at normal pressure using a box-type electric furnace (model: AMF20) for 10 hours, and then fired at 900°C for 4 hours. After firing, the switch of the heater was turned off, and the alumina boat was placed in the furnace and cooled naturally. As a result, the temperature of the furnace dropped to about 200°C after 5 hours, but the cooling rate was slightly slow thereafter. After a day and a night, it was confirmed that the temperature of the furnace was below 100°C, and then the particles were taken out and crushed for a few minutes using an agate automatic mortar to make the particle size uniform. In this way, the positive electrode active material particles of Example 1 were prepared. The positive electrode active material particles are in particle form, and it is confirmed by the above method that a part of the aluminum element exists near the center of the positive electrode active material particles, and another part of the aluminum element exists near the surface of the positive electrode active material particles. In this way, a lithium transition metal composite oxide containing Ni, Co and Mn in a molar ratio of Ni:Co:Mn=36:13:42, a molar ratio of lithium element to transition metal element of Li / Me=1.2, and a positive electrode active material particle containing aluminum element as a heterogeneous element, and a molar ratio of aluminum element to the sum of the molar numbers of nickel element, cobalt element, manganese element and aluminum element of Al:(Ni, Co, Mn, Al)=1.0:100 (the content of aluminum element is 1.0% in terms of molar ratio) is prepared. In the positive electrode active material particles, the aluminum element concentration near the surface is higher than the aluminum element concentration near the center.
[0141] (Production of positive electrode)
[0142] A positive electrode mixture paste was prepared, which contained the obtained positive electrode active material particles, acetylene black (AB) as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder at a mass ratio of 90:5:5 (solid content conversion), and N-methylpyrrolidone (NMP) as a dispersion medium. The positive electrode mixture paste was applied to an aluminum foil (thickness 20 μm) as a positive electrode substrate, dried, and then pressed to obtain a positive electrode.
[0143] (Production of negative electrode)
[0144] A negative electrode mixture paste containing graphite as a negative electrode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener at a mass ratio of 97:2:1 (solid content conversion) and water as a dispersion medium was prepared. The negative electrode mixture paste was applied to a copper foil (thickness 10 μm) as a negative electrode substrate, dried, and then pressed to obtain a negative electrode.
[0145] (Assembly of non-aqueous electrolyte storage element)
[0146] The positive electrode and the negative electrode are housed in a flat bottomed square tube-shaped container body made of aluminum alloy to assemble a non-aqueous electrolyte storage element. It should be noted that as a non-aqueous electrolyte, a non-aqueous solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 6:7:7 is used. 3 A solution is prepared by dissolving lithium hexafluorophosphate (LiPF6) as an electrolyte salt at a concentration of , and a polyolefin microporous membrane is used as a separator.
[0147] (Storage of Gases Soluble in Non-aqueous Electrolyte)
[0148] In the assembled non-aqueous electrolyte storage element, after the pressure inside the container is reduced to 0.09 MPa using a vacuum pump, carbon dioxide gas as a gas soluble in the non-aqueous electrolyte is stored until the pressure inside the container reaches 0.1 MPa. The carbon dioxide gas is stored in the container for 5 minutes and then the injection port is sealed, thereby sealing the container.
[0149] (Initial charge and discharge)
[0150] For the non-aqueous electrolyte storage element after the carbon dioxide gas is stored, the initial charge and discharge are performed at 25°C according to the following procedures. After constant current charging to 4.35V with a charging current of 0.1C, constant voltage charging is performed at 4.35V. The charging termination condition is the moment when the current value decays to 0.02C. A 10-minute stop time is set after charging. Then, constant current discharge is performed to 2.5V with a discharge current of 0.1C. In this way, the non-aqueous electrolyte storage element of Example 1 is obtained. The pressure inside the container of the non-aqueous electrolyte storage element is 0.097MPa. It should be noted that the positive electrode potential of the initial charge and discharge is less than 4.5V vs.Li / Li + In the X-ray diffraction diagram of the positive electrode in the non-aqueous electrolyte storage element after initial charge and discharge using CuKα rays, it was confirmed that the positive electrode active material particles have an α-NaFeO2 structure, and there is a diffraction peak in the range of diffraction angle 2θ of 20° to 22°. In addition, the carbon dioxide gas contained in the container is dissolved in the non-aqueous electrolyte, so the interior of the container of the non-aqueous electrolyte storage element of Example 1 is in a negative pressure state. Furthermore, the container is made of aluminum alloy with a thin thickness, so the container is deformed by the negative pressure state inside the container. In addition, the minimum width of the internal space of the container in the stacking direction is sufficiently small relative to the thickness of the electrode body, so through the deformation of the container, the electrode body becomes pressed in the stacking direction of the positive and negative electrodes.
[0151] [Example 2 to Example 4]
[0152] The non-aqueous electrolyte storage elements of Examples 2 to 4 were obtained in the same manner as in Example 1, except that the amounts of nickel sulfate hexahydrate, cobalt sulfate heptahydrate, and manganese sulfate pentahydrate, and the amounts of hydroxide precursor and lithium hydroxide monohydrate were adjusted so that the molar ratio of lithium element to transition metal element (Li / Me) and the molar ratio of Ni, Co, and Mn (Ni:Co:Mn) in the target lithium transition metal composite oxide were the values shown in Table 1. It was confirmed that in these positive electrode active material particles, the aluminum element concentration near the surface was higher than the aluminum element concentration near the center.
[0153] [Example 5]
[0154] The nonaqueous electrolyte storage element of Example 5 was obtained by the same production method as Example 1 except that the sulfate aqueous solution during the preparation of the hydroxide precursor was a mixed aqueous solution of aluminum sulfate, nickel sulfate, cobalt sulfate, and manganese sulfate. It was confirmed that in the positive electrode active material particles of Example 5, the aluminum element was present in both the vicinity of the center and the vicinity of the surface without being biased.
[0155] [Comparative Example 1]
[0156] A lithium transition metal composite oxide was prepared by the same method as in Example 1 except that no aluminum sulfate aqueous solution was added dropwise during the preparation of the hydroxide precursor. The lithium transition metal composite oxide was used as the positive electrode active material particle of Comparative Example 1. A nonaqueous electrolyte storage element of Comparative Example 1 was obtained in the same manner as in Example 1 except that the positive electrode active material particle of Comparative Example 1 was used.
[0157] [Comparative Example 2]
[0158] A nonaqueous electrolyte storage element of Comparative Example 2 was obtained in the same manner as in Example 1 except that air was contained in the container instead of carbon dioxide gas and the pressure in the container was the same as the atmospheric pressure.
[0159] [Comparative Example 3]
[0160] A nonaqueous electrolyte storage element of Comparative Example 3 was obtained in the same manner as in Comparative Example 1 except that air was contained in the container instead of carbon dioxide gas and the pressure in the container was the same as the atmospheric pressure.
[0161] [Comparative Examples 4 and 5]
[0162] With the composition formula LiNi 0.50 Co 0.20 Mn 0.30In the method represented by O2, the amount of nickel sulfate hexahydrate, cobalt sulfate heptahydrate and manganese sulfate pentahydrate, as well as the amount of hydroxide precursor and lithium hydroxide monohydrate were adjusted during the preparation of the hydroxide precursor, and no aluminum sulfate aqueous solution was added. Except for this, a lithium transition metal composite oxide was prepared by the same preparation method as Example 1. This was used as the positive electrode active material particle of Comparative Examples 4 and 5.
[0163] A nonaqueous electrolyte storage device of Comparative Example 4 was obtained in the same manner as in Example 1 except that the positive electrode active material particles of Comparative Examples 4 and 5 were used. A nonaqueous electrolyte storage device of Comparative Example 5 was obtained in the same manner as in Comparative Example 2 except that the positive electrode active material particles of Comparative Examples 4 and 5 were used.
[0164] [Comparative Example 6]
[0165] A nonaqueous electrolyte electricity storage device of Comparative Example 6 was obtained in the same manner as in Comparative Example 2 except that the positive electrode active material particles of Example 2 were used.
[0166] (Charge and discharge cycle test)
[0167] For the non-aqueous electrolyte storage elements of Examples 1 to 5 and Comparative Examples 1 to 6 after the above-mentioned initial charge and discharge, a charge and discharge cycle test was carried out under the following conditions. First, after being kept in a constant temperature chamber at 45°C for 3 hours, the elements were charged to 4.35V at a constant current of 0.1C and charged at the same constant voltage. The end condition for charging is that the total charging time reaches 3 hours. A stop time of 10 minutes is set after charging. Then, after constant current discharge to 2.5V at a discharge current of 0.1C, a stop time of 10 minutes is set. These charging, discharging and stopping processes are regarded as one cycle, and the charge and discharge are repeated 300 times in a constant temperature chamber at 45°C.
[0168] (Output ratio after charge and discharge cycle)
[0169] For each non-aqueous electrolyte storage element before and after the above-mentioned charge and discharge cycle test, in a thermostatic chamber at 25°C, charge with a constant current of 0.1C to a voltage at which SOC50% is reached. Next, at 25°C, the lower limit voltage is set to 2.7V and the current is discharged for 30 seconds at 0.1C, 0.2C, and 0.5C by the IV method, and the output is measured from the voltage at the 10th second from the start of discharge. After each discharge is completed, charge with a constant current of 0.1C to a voltage at which SOC50% is reached. Calculate the ratio (%) of the output after the charge and discharge cycle of each non-aqueous electrolyte storage element relative to the output before the charge and discharge cycle as the output ratio after the charge and discharge cycle. The evaluation results are shown in Table 1.
[0170]
[0171] As shown in Table 1, the output ratio after the charge and discharge cycle of Examples 1 to 5 becomes higher. In Examples 1 to 5, the above-mentioned positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure, and the content of the lithium element in the above-mentioned lithium transition metal composite oxide relative to the transition metal element exceeds 1.0 in terms of molar ratio, and the above-mentioned positive electrode active material particles contain aluminum element as a heterogeneous element. Carbon dioxide gas is contained inside the container and is in a negative pressure state, and the above-mentioned electrode body is in a state of being pressed in the stacking direction of the above-mentioned positive electrode and the above-mentioned negative electrode.
[0172] On the other hand, compared with Examples 1 to 5, in Comparison Example 1 in which the positive electrode active material particles do not contain aluminum as a foreign element, Comparison Examples 2 and 6 in which the interior of the container is not in a negative pressure state and is not pressed in the stacking direction of the positive electrode and the negative electrode, Comparison Example 3 in which the positive electrode active material particles do not contain aluminum as a foreign element, the interior of the container is not in a negative pressure state and is not pressed in the stacking direction of the positive electrode and the negative electrode, Comparison Example 4 in which the content of lithium element in the lithium transition metal composite oxide is less than 1.0 in terms of molar ratio relative to the transition metal element, and Comparison Example 5 in which the content of the lithium element in the lithium transition metal composite oxide is less than 1.0 in terms of molar ratio relative to the transition metal element, the interior of the container is not in a negative pressure state and is not pressed in the stacking direction of the positive electrode and the negative electrode, the output ratio after the charge and discharge cycle is poor.
[0173] In addition, according to the comparison between Example 1 and Comparative Example 2, when the above-mentioned positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure and the content of the lithium element in the above-mentioned lithium transition metal composite oxide relative to the transition metal element is more than 1.0 in molar ratio, the effect of improving the output ratio after the charge and discharge cycle by the pressure inside the container being a negative pressure state is 11 (=92-81) percentage points, and according to the comparison between Comparative Example 4 and Comparative Example 5, when the above-mentioned positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure and the content of the lithium element in the above-mentioned lithium transition metal composite oxide relative to the transition metal element is not more than 1.0 in molar ratio, the effect of improving the output ratio after the charge and discharge cycle by the pressure inside the container being a negative pressure state is only 2 (=79-77) percentage points. That is, it can be seen that the effect of improving the output ratio after the charge and discharge cycle by bringing the pressure inside the container into a negative pressure state is particularly significant when the positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure and the content of the lithium element in the above-mentioned lithium transition metal composite oxide relative to the transition metal element exceeds 1.0 in terms of molar ratio.
[0174] From the above results, it is understood that the nonaqueous electrolyte energy storage device can suppress a decrease in output performance after charge and discharge cycles.
[0175] Industrial Applicability
[0176] The present invention can be applied to non-aqueous electrolyte storage elements used as power sources for electronic devices such as personal computers and communication terminals, automobiles, and industrial applications.
[0177] Explanation of symbols
[0178] 1 Non-aqueous electrolyte storage element
[0179] 2 Electrode body
[0180] 3 Container
[0181] 3a Container body
[0182] 3b Cover
[0183] 4 Positive terminal
[0184] 14. Positive electrode collector
[0185] 5 Negative terminal
[0186] 15 Negative electrode collector
[0187] 20 Storage unit
[0188] 30 Power storage device
Claims
1. A non-aqueous electrolyte storage element comprising: An electrode body formed by stacking a positive electrode and a negative electrode containing positive electrode active material particles, Non-aqueous electrolyte, and a sealable container for accommodating the electrode body and the non-aqueous electrolyte; The positive electrode active material particles contain a lithium transition metal composite oxide having an α-NaFeO2 structure. The content of lithium element in the lithium transition metal composite oxide relative to the transition metal element is greater than 1.0 in terms of molar ratio, The positive electrode active material particles contain a heterogeneous element, and the heterogeneous element is aluminum, tungsten, boron, zinc, titanium or a combination thereof. A gas soluble in the non-aqueous electrolyte is contained in the container. The interior of the container is in a negative pressure state, The electrode body is in a state of being pressed in a stacking direction of the positive electrode and the negative electrode.
2. The nonaqueous electrolyte storage element according to claim 1, wherein The gas soluble in the non-aqueous electrolyte is carbon dioxide.
3. The nonaqueous electrolyte storage element according to claim 1 or 2, wherein The transition metal element comprises at least one of nickel, cobalt and manganese, The ratio of the number of moles of the foreign element to the sum of the number of moles of the nickel element, the cobalt element, the manganese element, and the foreign element is higher near the surface of the positive electrode active material particle than near the center.
4. The nonaqueous electrolyte storage element according to claim 1 or 2, wherein The transition metal element includes a manganese element, and the content of the manganese element relative to the transition metal element is 0.35 to 0.65 in terms of molar ratio. 5 . A power storage device comprising two or more nonaqueous electrolyte power storage elements and comprising one or more nonaqueous electrolyte power storage elements according to claim 1 or 2.
Citation Information
Patent Citations
Positive active material, and positive electrode and lithium battery including the positive active material