ZnWO4 / g-C3N4 composite antibacterial material as well as preparation method and application thereof
Through the preparation of ZnWO4/g-C3N4 composite antibacterial materials, the metal functional groups and photoresponsive properties are used to inhibit microbial growth, which solves the problems of high cost and environmental pollution of traditional antibacterial materials, and achieves effective microbial inhibition effect, which is suitable for antibacterial applications in public environments. .
Patent Information
- Application Number
- CN202411125211.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to effectively inhibit or eliminate pathogenic microorganisms transmitted through contact, especially in public environments, where traditional antibacterial materials are costly, environmentally contaminated and limited applications.
ZnWO4/g-C3N4 composite antibacterial material is used to prepare ZnWO4 nanomaterials and g-C3N4 through high-pressure hydrothermal method to form composite materials with metal functional groups and photoresponsive properties, and use metal functional groups to inhibit microbial growth and photoresponsiveness to generate oxidative free radicals. Destroy microbial cells.
It has achieved low-cost, non-toxic and environmentally friendly antibacterial effects, significantly inhibited microbial reproduction, reduced the risk of microbial transmission in public environments, and has wide application value.
Smart Images

Figure CN119014429A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano antibacterial materials, and specifically relates to a ZnWO4 / g-C3N4 composite antibacterial material and a preparation method and application thereof. Background Art
[0002] In recent years, the spread of pathogenic microorganisms in the air has had a significant impact on human health, especially during the virus epidemic, the harm it brings is even more serious, not only affecting human health but also seriously restricting the development of the world economy. Therefore, how to inhibit or reduce the impact of pathogenic microorganisms on humans and nature is an important research direction. The spread of pathogenic microorganisms mainly relies on contact between air and objects. Among them, transmission through contact with objects is a very important means of transmission. The development of nano-antibacterial materials that can inhibit or eliminate pathogenic microorganisms is of great significance for inhibiting contact transmission and has great application value.
[0003] ZnWO4 is a tetragonal material with good stability, non-toxicity, low price and cost. It has application value in the fields of photoelectric conversion and photocatalytic degradation. g-C3N4 also has high chemical and thermal stability. The combination of the two materials as antibacterial materials has two different antibacterial mechanisms. One is to inhibit the growth of microorganisms by providing metal functional groups through ZnWO4 materials, and the other is to destroy the cell membrane and shell of microorganisms by generating oxidative free radicals through light response. At the same time, the combination of the two materials also strengthens the transfer of photogenerated electrons and holes under light conditions, promotes the generation of photogenerated oxidative species, and further improves the antibacterial ability under light illumination conditions. Summary of the invention
[0004] The purpose of the present invention is to provide a ZnWO4 / g-C3N4 antibacterial agent and a preparation method thereof, which is simple, convenient, low-cost, mild in conditions and conducive to large-scale production.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is: a ZnWO4 / g-C3N4 composite antibacterial material, the preparation method is as follows:
[0006] 1) Add zinc salt and tungsten salt to deionized water, add chelating agent, and stir magnetically for 1-2 hours to obtain a precursor solution;
[0007] 2) placing the precursor solution into a high-pressure hydrothermal reactor for reaction, cooling naturally, and washing to obtain ZnWO4 nanomaterials;
[0008] 3) The obtained ZnWO4 nanomaterial is mixed with a carbon nitrogen precursor in a certain proportion, and annealed under certain atmosphere and temperature conditions to obtain a ZnWO4 / g-C3N4 composite antibacterial material.
[0009] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 1), the zinc salt is zinc acetate, zinc nitrate, zinc sulfate or zinc chloride.
[0010] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 1), the tungsten salt is sodium tungstate or tungsten chloride.
[0011] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 1), the molar ratio of zinc salt: tungsten salt is 1:1.
[0012] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 1), the chelating agent is polyethylene glycol, citric acid or an organic surfactant.
[0013] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 2), the hydrothermal reaction temperature is 160-180°C and the reaction time is 6-48 hours.
[0014] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 3), the carbon-nitrogen precursors are melamine and urea.
[0015] In the above-mentioned ZnWO4 / g-C3N4 composite antibacterial material, in step 3), the atmosphere may be nitrogen, argon or air, and the annealing temperature is 550°C.
[0016] The above-mentioned ZnWO4 / g-C3N4 composite antibacterial material is used in the preparation of antibacterial products.
[0017] The preferred material antibacterial performance evaluation method is as follows: the culture medium is divided into two groups, 1. blank control; 2. adding the composite antibacterial material. Use a pipette to absorb 100uL of yeast culture dilution, evenly spread it on the two groups of culture medium, and place the culture medium upside down in an incubator at 37°C for 48h to observe the colony.
[0018] The beneficial effects of the present invention are as follows: the present invention uses tungsten salt, zinc salt and carbon nitrogen precursor to prepare ZnWO4 / g-C3N4 composite antibacterial material, and applies it to inhibit the growth of microorganisms and reduce the spread of microorganisms in public environments. The preparation method provided by the present invention has cheap raw materials, is non-toxic and safe, greatly reduces costs, and has no pollution to the environment, realizes green chemistry, can inhibit the reproduction of microorganisms, and has an antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is the antibacterial experimental control of the antibacterial material and the blank control group, where A is the blank control group (without adding antibacterial material) and B is the antibacterial effect of the ZnWO4@g-C3N4 composite antibacterial material prepared in Example 1. DETAILED DESCRIPTION
[0020] Example 1 ZnWO4 / g-C3N4 composite antibacterial material
[0021] The preparation method is as follows
[0022] 1) First, 0.510g of ammonium tungstate hydrate (NH4) 10 H2(W2O7)6·xH2O was added to 5 mL of water, stirred at 80°C in a water bath heating magnetic stirrer until completely dissolved, 0.439 g of zinc acetate dihydrate C4H6O4Zn·2H2O was added, 45 mL of water was added, stirring was continued for 10 min, 1.5 g of PEG2000 was added, stirring was continued until uniformly mixed, the mixed solution was transferred to a polytetrafluoroethylene-lined hydrothermal reactor with a capacity of 80 mL, the reaction was maintained at 180°C for 12 h, naturally cooled, and centrifuged and washed to obtain ZnWO4 nanomaterials.
[0023] 2) The obtained ZnWO4 nanomaterial was mixed with 1.26 g of melamine and ground, and calcined at 550°C for 4 h in an air environment with a heating rate of 5°C / min, and then naturally cooled to obtain a ZnWO4 / g-C3N4 composite antibacterial material.
[0024] Example 2 ZnWO4 / g-C3N4 composite antibacterial material
[0025] The preparation method is as follows
[0026] 1) First, 0.586 g of sodium tungstate Na2WO4 was added to 5 mL of water, and stirred at 80 ° C in a water bath heating magnetic stirrer until completely dissolved, 0.439 g of zinc acetate dihydrate C4H6O4Zn·2H2O was added, 45 mL of water was added, and stirring was continued for 10 min, 1.5 g of PEG2000 was added, and stirring was continued until the mixture was uniform, and the mixed solution was transferred to a polytetrafluoroethylene-lined hydrothermal reactor with a capacity of 80 mL, and the reaction was maintained at 180 ° C for 12 h, and the ZnWO4 nanomaterial was obtained by centrifugal washing.
[0027] 2) The obtained ZnWO4 crystals were mixed with 3 grams of urea and ground, and calcined at 550°C for 4 hours in an air environment with a heating rate of 5°C / min, and then naturally cooled to obtain a ZnWO4 / g-C3N4 composite antibacterial material.
[0028] Example 3 ZnWO4 / g-C3N4 composite antibacterial material
[0029] The preparation method is as follows
[0030] 1) First, 0.510g of ammonium tungstate hydrate (NH4) 10H2(W2O7)6·xH2O was added to 5 mL of water, stirred at 80°C in a water bath heating magnetic stirrer until completely dissolved, 0.439 g of zinc acetate dihydrate C4H6O4Zn·2H2O was added, 45 mL of water was added, stirring was continued for 10 min, 1.5 g of PEG2000 was added, and stirring was continued until uniformly mixed, and the mixed solution was transferred to a polytetrafluoroethylene-lined hydrothermal reactor with a capacity of 80 mL, and the reaction was maintained at 180°C for 12 h, and the ZnWO4 nanomaterial was obtained by centrifugal washing.
[0031] 2) 1.26 g of melamine was dissolved in 50 ml of 80°C hot water, and then the obtained ZnWO4 nanomaterial was added and evaporated in an oven at 60°C to obtain a white powder. The powder was calcined at 550°C for 4 h in an air environment at a heating rate of 5°C / min, and then naturally cooled to obtain a ZnWO4 / g-C3N4 composite antibacterial material.
[0032] Example 4 ZnWO4 / g-C3N4 composite antibacterial material
[0033] The preparation method is as follows
[0034] 1) First, 0.586g of ammonium tungstate hydrate (NH4) 10 H2(W2O7)6·xH2O was added to 5 mL of water, stirred at 80°C in a water bath heating magnetic stirrer until completely dissolved, 0.378 g of zinc nitrate Zn(NO3)2 was added, 45 mL of water was added, stirring was continued for 10 min, 1.5 g of PEG2000 was added, and stirring was continued until uniformly mixed, the mixed solution was transferred to a polytetrafluoroethylene-lined hydrothermal reactor with a capacity of 80 mL, the reaction was maintained at 160°C for 12 h, and the ZnWO4 nanomaterial was obtained by centrifugal washing.
[0035] 2) The obtained ZnWO4 nanomaterial was mixed and ground with 1.26 g of melamine, calcined at 550°C for 4 h under a nitrogen atmosphere at a heating rate of 5°C / min, and then naturally cooled to obtain a ZnWO4 / g-C3N4 composite antibacterial material.
[0036] Example 5 Application
[0037] Ordinary yeast culture medium is prepared as follows, using 5g of trypsin; 2.5g of yeast extract; 5g of glucose; 250ml of distilled water; adjust the pH value to 7.2-7.4, and sterilize with high-temperature steam at 121°C for 20min. The sterilized culture medium is poured into a culture dish to cool and solidify. The yeast is diluted in an aqueous solution to form a pre-prepared simple bacterial solution for standby use. At the same time, 0.5g of inorganic antibacterial material is diluted in 95ml of aqueous solution to form a suspension, and 5ml of the pre-prepared simple bacterial solution is added. Use a spreader to evenly spread 0.1mL of diluted bacterial solution containing the antibacterial material (prepared in Example 1) and without the antibacterial material on the surface of the solid culture medium. The culture medium is placed in a constant temperature incubator at 37°C (with fluctuations of no more than 1°C) for culture. After 48 hours, take photos to record changes in the number of yeast. Figure 1 As shown in the figure on the right, the yeast colonies on the culture medium with the addition of ZnWO4@g-C3N4 composite antibacterial material are less inhibited, which indicates that the material has antibacterial ability. The antibacterial properties of the antibacterial materials obtained in Examples 1-4 were tested. By counting the number of colonies, it was found that the colony counts in the samples of Examples 1-4 were 71, 85, 102 and 89, respectively, and the colony count of the blank control group was 141, which indicates that the composite antibacterial material has certain antibacterial properties.
Claims
1. A ZnWO4 / g-C3N4 composite antibacterial material, characterized in that: The preparation method is as follows: 1) Add zinc salt and tungsten salt to deionized water, add chelating agent, and stir magnetically for 1-2 hours to obtain a precursor solution; 2) placing the precursor solution into a high-pressure hydrothermal reactor for reaction, cooling naturally, and washing to obtain ZnWO4 nanomaterials; 3) The obtained ZnWO4 nanomaterial is mixed with a carbon nitrogen precursor in a certain proportion, and annealed under certain atmosphere and temperature conditions to obtain a ZnWO4 / g-C3N4 composite antibacterial material.
2. A ZnWO4 / g-C3N4 composite antibacterial material as claimed in claim 1, characterized in that: In step 1), the zinc salt is zinc acetate, zinc nitrate, zinc sulfate or zinc chloride.
3. The ZnWO4 / g-C3N4 composite antibacterial material according to claim 1, characterized in that: In step 1), the tungsten salt is sodium tungstate or tungsten chloride.
4. The ZnWO4 / g-C3N4 composite antibacterial material according to claim 1, characterized in that: In step 1), the molar ratio of zinc salt:tungsten salt is 1:
1.
5. The ZnWO4 / g-C3N4 composite antibacterial material according to claim 1, characterized in that: In step 1), the chelating agent is polyethylene glycol, citric acid or an organic surfactant.
6. The ZnWO4 / g-C3N4 composite antibacterial material according to claim 1, characterized in that: In step 2), the hydrothermal reaction is carried out at a temperature of 160-180° C. and a reaction time of 6-48 hours.
7. The ZnWO4 / g-C3N4 composite antibacterial material according to claim 1, characterized in that: In step 3), the carbon-nitrogen precursors are melamine and urea.
8. The ZnWO4 / g-C3N4 composite antibacterial material according to claim 1, characterized in that: In step 3), the atmosphere may be nitrogen, argon or air, and the annealing temperature is 550°C.
9. Use of a ZnWO4 / g-C3N4 composite antibacterial material according to any one of claims 1 to 8 in the preparation of antibacterial products.