Polymer splint and preparation method thereof

By adopting reversible hydrogel complexes and metal shrapnel triggering mechanisms in polymer splints, the problems of comfort and fixation steps of existing polymer splints are solved, and a convenient, flexible and reusable polymer is achieved. Splint reduces the weight load on the affected area and promotes healing.

CN119015467APending Publication Date: 2024-11-26HANGZHOU YINSHENG MEDICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410932937.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing polymer splints have poor comfort and cumbersome fixing steps during use, requiring water or wet water triggering and professional tools to remove, which is inconvenient to operate.

Method used

The hydrogel composite is used as the core material of the plywood to achieve reversible transformation of soft and rigid states through temperature changes. Combined with metal shrapnel and non-woven fabric cladding, it provides a triggering method and fixing mechanism, simplifying the operation and disassembly process.

Benefits of technology

It realizes the polymer splint that is easy to operate, flexible and has good plasticity. It does not require water conditions to trigger before fixing. It only needs to be heated during removal to soften and remove. It has strong reusability, which reduces the load on the affected area and promotes healing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004940368590000011
    Figure HDA0004940368590000011
Patent Text Reader

Abstract

The invention discloses a polymer splint, which comprises a coating layer and a hydrogel complex arranged in the coating layer, the hydrogel complex has a soft state and a rigid hardened state, and the hydrogel complex can be converted into the rigid hardened state after being triggered in the soft state. The macromolecular splint is convenient and flexible to operate and good in plasticity, does not need to be triggered under a water condition before being fixed, and does not need a special tool when being disassembled. And the device can be repeatedly used. The device is low in material consumption, light in weight, capable of enabling the load of an affected part to be small, capable of reducing the load of functional exercise after fixation, beneficial to blood circulation and capable of promoting healing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of medical technology, and particularly relates to a medical polymer splint and a preparation method thereof. Background Art

[0002] Plaster bandages have strong shaping ability and good stability. They are used for fixation in orthopedics or orthopedics. Since plaster bandages are inconvenient to use, more and more doctors are starting to use medical polymer splints to replace plaster bandages and plaster supports. The polymer splints on the market are made of glass fiber or polyester fiber coated with polyurethane compounds. They have the characteristics of fast hardening and high strength, but they need to be triggered in water or wet water spray and then fixed by professionals. Special tools are needed for removal, which is inconvenient to operate.

[0003] The patent document with the publication number CN 219000793 U discloses a polymer splint that is easy to clamp, including: polymer splint 1 and polymer splint 2, both of which are arc-shaped, and the outer side walls of polymer splint 1 and polymer splint 2 are provided with a protective layer, and the two protective layers are rotatably connected by a hinge; a fixing belt, which is provided with a plurality of fixing belts, one end of which is fixedly connected to the outer wall of the protective layer at one end of polymer splint 1, and the other end is fixedly connected to polymer splint 1 through a connecting buckle; and a threaded rod, which drives two threaded sleeves to move inward at the same time by rotating the threaded rod, thereby moving the push plate inward, clamping polymer splint 1 and polymer splint 2, and playing the role of adjusting the tightness between polymer splint 1 and polymer splint 2. This document solves the problem of easy clamping to a certain extent, but because polymer splint 1 and polymer splint 2 are structurally fixed polymer materials, the hardness is relatively large, the comfort is relatively poor during use, and the fixing steps are relatively cumbersome.

[0004] The patent document with publication number CN 208808792 U discloses a polymer splint, including a packaging box, a soaking tank is provided on the top of the packaging box, an electric heating wire is provided under the soaking tank, and the electric heating wire is installed in the inner cavity of the packaging box, a splint slot is provided on one side of the soaking tank, and the splint slot and the side wall of the soaking tank are both movably connected with a cover plate through a hinge. This document solves the symptoms of itching or wrinkling of the patient's skin due to long-term moisture in the prior art. However, this technical solution also has the above-mentioned problems of poor comfort and cumbersome fixation. Summary of the invention

[0005] The invention provides a polymer splint which is convenient to operate and use, flexible and has good plasticity.

[0006] A polymer splint comprises a coating layer and a hydrogel complex arranged in the coating layer. The hydrogel complex has a soft state and a rigid hardened state. When the hydrogel complex is in the soft state, it can be converted into the rigid hardened state after being triggered.

[0007] Preferably, the hydrogel composite is reversibly transformable between a soft state and a rigid hardened state.

[0008] The product of the present invention is in a soft state before use, and is then triggered to be shaped, hardened and fixed using a specific triggering method, and the state change is reversible. The hydrogel can be softened from hard (i.e., converted from a rigid hardened state to a soft state) by heating and the softening temperature is 50-100°C.

[0009] Preferably, the hydrogel complex is an acrylamide-sodium acetate hydrogel complex; further, the hydrogel complex is an acrylamide-sodium acetate hydrogel containing an initiator. The acrylamide is obtained by cross-linking acrylamide monomer with a cross-linking agent and a photoinitiator under light.

[0010] The initiator is a water-soluble photoinitiator, including but not limited to phenyl (2,4,6-trimethylbenzoyl) lithium phosphate LAP, initiator 2959 and the like.

[0011] Preferably, in the soft state, the hydrogel complex is composed of an integrally arranged hydrogel skeleton and a supersaturated sodium acetate solution, the concentration of the supersaturated sodium acetate solution is 1000-2000 g / L; wherein sodium acetate accounts for 40-60% of the total weight of the hydrogel complex; and water accounts for 20-50% of the weight of the hydrogel.

[0012] The triggering method mentioned in the present invention includes but is not limited to bending the metal spring pre-embedded in the hydrogel, using a sharp object to pierce the sealed bag, etc.

[0013] Preferably, a trigger is further provided in the coating layer. The trigger is further preferably a metal spring. Further preferably, the metal spring can be folded.

[0014] The hydrogel composite can be used alone or in combination with other materials to further enhance the strength and toughness after hardening. Preferably, the coating layer is also provided with a reinforcing material for enhancing the strength and toughness after hardening. These reinforcing materials include but are not limited to non-woven fabrics such as glass fiber, carbon fiber, needle-punched fabric and spunlace fabric. The reinforcing material is 1-300% of the weight of the substrate, where the substrate is the weight of the hydrogel composite before the reinforcing material is added.

[0015] Preferably, the covering layer comprises a sealing bag, and optionally comprises a non-woven fabric arranged on the outside of the sealing bag.

[0016] As a specific preference, the polymer splint is composed of an interlayer and a protective layer, the interlayer is a hydrogel complex wrapped in a sealing bag, and the protective layer is a non-woven fabric. In this case, the sealing bag and the non-woven fabric constitute the coating layer.

[0017] A method for preparing a polymer splint comprises the following steps:

[0018] Step 1: Dissolve the hydrogel monomer, crosslinking agent and photoinitiator in water to obtain solution A; prepare sodium acetate solution I to obtain solution B.

[0019] Step 2: Mix solution A and solution B, keep the mixed solution in a liquid state, pour it into a mold, irradiate it with light corresponding to the initiator, and obtain the hydrogel composite after photocuring and cross-linking;

[0020] Step 3: Load the obtained hydrogel complex into a coating layer, soften it, and cool it to obtain the polymer splint.

[0021] Preferably, the hydrogel monomer is acrylamide, and the cross-linking agent is N,N'-methylenebisacrylamide.

[0022] Preferably, the monomer accounts for 5-10% of the weight of the hydrogel, the cross-linking agent accounts for 0.1-0.5% of the weight of the hydrogel, the initiator accounts for 0.1-1% of the weight of the hydrogel, the sodium acetate accounts for 40-60% of the weight of the hydrogel, and water accounts for 20-50% of the weight of the hydrogel; the weight of the hydrogel is the total weight of the hydrogel complex.

[0023] Solution B needs to be kept in liquid state during the preparation of solution B in step 1 and the light mixing and light curing process in step 2. For example, in step 1, solution B needs to be maintained at a specific temperature, which needs to be determined according to the concentration of solution B, and it can be above the saturation temperature corresponding to the current concentration; in step 2, solution A and solution B need to be mixed at the specific temperature. After pouring into the mold, it is not necessary to heat it separately, and the material can be preheated. If the temperature of the mixed liquid is lower than the saturation temperature, it can be properly heated before pouring into the mold.

[0024] Furthermore, a polymer splint, the preparation process includes the following steps:

[0025] Step 1, solution A (hydrogel solution): dissolve an appropriate amount of acrylamide monomer, an appropriate amount of N,N'-methylenebisacrylamide and an appropriate amount of photoinitiator in an appropriate amount of water.

[0026] Step 2, solution B (sodium acetate solution): dissolve an appropriate amount of anhydrous sodium acetate in an appropriate amount of water at an appropriate temperature. In steps 2 to 4, the sodium acetate solution is kept at a liquid temperature.

[0027] Step 3, mixing solution A and solution B to obtain a mixed solution C at an appropriate temperature.

[0028] Step 4: Pour the mixed solution C into a mold, pre-place a certain amount of reinforcing fiber (i.e. reinforcing material) and metal shrapnel (e.g., a 0.2mm bendable metal shrapnel) in the mold, and immediately irradiate it with ultraviolet light for a period of time to photocuring and cross-linking. Wait for it to cool naturally to room temperature and demold it.

[0029] Step 5, putting the demolded sample into a sealed bag, heating it to a softening temperature after sealing it to melt the crystallized salt therein, and then cooling it to room temperature.

[0030] Step 6, wrap the sealed bag in non-woven fabric and sew it.

[0031] The design principle of the present invention is to utilize the phase change principle of hydrated salt, with polymer as the matrix and hydrated salt as the reinforcing phase that can be phase-changed. The huge difference in the solubility of sodium acetate at different temperatures, the stability of supersaturated sodium acetate solution, and the property of hydrogel swelling and binding water are utilized. The sodium acetate-acrylamide hydrogel complex can be switched between soft and hard states. When softening, sodium acetate is in the liquid phase, and the mechanical properties of the sodium acetate-acrylamide hydrogel complex are determined by the acrylamide hydrogel. When hardening, sodium acetate is in the solid phase, and the mechanical properties of the sodium acetate-acrylamide hydrogel complex are determined by the acrylamide hydrogel and sodium acetate.

[0032] A polymer splint, the preparation process includes the following steps:

[0033] A polymer splint, the use process is: the polymer splint is covered on the place that needs to be wrapped, and then the metal spring is bent to trigger it to shape, harden and fix. The triggering mechanism is that the bending causes the metal spring to vibrate, causing the supersaturated sodium acetate solution to precipitate and crystallize, becoming rigid.

[0034] A polymer splint, the disassembly process is: heating the splint, for example, covering it with a hot towel for a few minutes, so that it becomes soft and can be directly removed. Alternatively, the sealed bag can be cut open, soaked in water, and then directly removed after it melts and softens.

[0035] The present invention utilizes the characteristics of supersaturated salt solution to compound hydrogel and supersaturated salt solution to prepare a new type of polymer splint. This polymer splint can be transformed into soft and hard states. When the salt solution is in a supersaturated liquid state, the hydrogel shows flexibility. When external factors, such as vibration or crystallization point, are introduced, the supersaturated solution begins to precipitate crystals, and the whole shows rigidity. Heating in a rigid state can restore its flexibility. Utilizing its characteristics, the prepared polymer splint is easy to operate, flexible, and has good plasticity. It does not require water conditions to trigger before fixation. It only needs to be heated to soften and remove during disassembly. It can also destroy the sealing bag and soak it in water to dissolve and remove it. It can be reused many times without destroying the sealing bag. It uses less materials and is light in weight, which can reduce the load on the affected area, reduce the load on functional exercises after fixation, is beneficial to blood circulation, and promotes healing. It has great clinical significance and social value.

[0036] The present invention provides a polymer splint, which is easy to operate, flexible, and has good plasticity. It does not require water conditions to trigger before fixation, and does not require special tools when removed. It can be reused for multiple cycles. It uses less material and is light in weight, which can reduce the load on the affected part, reduce the load on functional exercises after fixation, is beneficial to blood circulation, and promotes healing. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is the appearance picture of the polymer splint. DETAILED DESCRIPTION

[0038] The embodiments of the present invention are described in detail below. The described embodiments are exemplary and are intended to be used to explain the present invention, but should not be understood as limiting the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] This embodiment provides a method for preparing a polymer splint, the method comprising the following steps:

[0041] 1. Solution A (hydrogel solution): 6 g acrylamide monomer, 0.2 g N,N'-methylenebisacrylamide and 0.075 g photoinitiator LAP were dissolved in 6 mL water.

[0042] 2. Solution B (sodium acetate solution): Dissolve 30 g of anhydrous sodium acetate in 20 ml of water. This process needs to be heated to 85°C.

[0043] 3. Mix solution A and solution B at 85°C to obtain mixed solution C.

[0044] 4. Casting: Pour the mixed solution C into the mold and immediately irradiate it with blue light (405nm) for 15 seconds to make it photocured and cross-linked. Wait for it to cool naturally to room temperature and demold it.

[0045] 5. Softening: After demoulding, put it into a sealed bag and seal it. Heat it in a water bath to 85°C, keep it for 1 hour, then turn off the water bath and wait for it to cool naturally to room temperature. After taking it out, wrap it in non-woven fabric and sew it. The product of the present invention is shown in the figure Figure 1 As shown, the interlayer is a softened hydrogel complex sealed in a sealed bag, and the protective layer is a non-woven fabric.

[0046] Example 2

[0047] This embodiment provides a method for preparing a polymer splint, the method comprising the following steps:

[0048] 1. Solution A (hydrogel solution): Dissolve 6 g acrylamide monomer, 0.1 g N,N'-methylenebisacrylamide and 0.33 g photoinitiator 2959 in 6 mL water.

[0049] 2. Solution B (sodium acetate solution): Dissolve 38g of anhydrous sodium acetate in 20ml of water. This process needs to be heated to 95℃.

[0050] 3. Mix solution A and solution B at 95°C to obtain mixed solution C.

[0051] 4. Casting: Pour the mixed solution C into the mold, which has glass fiber mat and metal sheet placed in advance, and immediately irradiate with ultraviolet light (365nm) for 70 seconds to photocuring and crosslinking. Wait for it to cool naturally to room temperature and demould it.

[0052] 5. Softening: After demoulding, put it into a sealed bag and seal it. Heat it in a water bath to 95°C, keep it for 1 hour, then turn off the water bath and wait for it to cool naturally to room temperature. After taking it out, wrap it in non-woven fabric and sew it.

[0053] Example 3

[0054] This embodiment provides a method for preparing a polymer splint, the method comprising the following steps:

[0055] 1. Solution A (hydrogel solution): Dissolve 6 g acrylamide monomer, 0.1 g N,N'-methylenebisacrylamide and 0.33 g photoinitiator 2959 in 6 mL water.

[0056] 2. Solution B (sodium acetate solution): Dissolve 38g of anhydrous sodium acetate in 20ml of water. This process needs to be heated to 95℃.

[0057] 3. Mix solution A and solution B at 95°C to obtain mixed solution C.

[0058] 4. Casting: Pour the mixed solution C into the mold, put the needle-punched cloth and metal sheet in the mold in advance, and immediately irradiate it with ultraviolet light (365nm) for 70 seconds to make it photocured and cross-linked. Wait for it to cool naturally to room temperature and demould it.

[0059] 5. Softening: After demoulding, put it into a sealed bag and seal it. Heat it in a water bath to 95°C, keep it for 1 hour, then turn off the water bath and wait for it to cool naturally to room temperature. After taking it out, wrap it in non-woven fabric and sew it.

[0060] Performance Testing:

[0061] (a) Curing pressure bearing: The polymer plywood prepared in the above Examples 1, 2, and 3 was subjected to a curing pressure bearing test. The test results are shown in Table 1.

[0062] The solidification pressure testing method is:

[0063] 1. Take a pair of plywood and make a sample with a length of 30 cm and a width of 15 cm (thickness of about 4 mm).

[0064] 2. Place a 15kg weight in the middle and measure the difference between the concave distance and the horizontal distance of the splint with a universal measuring tool for 1 hour.

[0065] (b) Impact strength: The impact strength of the polymer plywood prepared in Examples 1 to 3 was tested in accordance with the national standard GB / T 1043.1-2008. The test results are shown in Table 1.

[0066] Table 1

[0067] Example Example 1 Example 2 Example 3 Curing pressure (sinking distance / mm) / 16 20 <![CDATA[Impact strength (kJ / m 2 )]]> 15.5 23.0 19.9

[0068] Example 1 broke when cured and subjected to pressure. Comparison between Example 2 and Example 3 shows that the addition of reinforcing materials greatly increases the overall strength and toughness.

Claims

1. A polymer splint, It is characterized in that The invention comprises a coating layer and a hydrogel complex arranged in the coating layer. The hydrogel complex has a soft state and a rigid hardened state. When the hydrogel complex is in the soft state, it can be converted into the rigid hardened state after being triggered.

2. The polymer splint according to claim 1, It is characterized in that The hydrogel composite is reversibly transformable between a soft state and a rigid hardened state.

3. The polymer splint according to claim 1, It is characterized in that The hydrogel complex is an acrylamide-sodium acetate hydrogel complex.

4. The polymer splint according to claim 1, It is characterized in that In the soft state, the hydrogel complex is composed of an integrally arranged hydrogel skeleton and a supersaturated sodium acetate solution, the concentration of the supersaturated sodium acetate solution is 1000-2000 g / L; the sodium acetate accounts for 40-60% of the total weight of the hydrogel complex; and water accounts for 20-50% of the weight of the hydrogel.

5. The polymer splint according to claim 1, It is characterized in that A triggering member is also arranged in the coating layer.

6. The polymer splint according to claim 1, It is characterized in that The coating layer is also provided with a reinforcing material for enhancing the strength and toughness after hardening.

7. The polymer splint according to claim 1, It is characterized in that The covering layer includes a sealing bag and optionally includes a non-woven fabric arranged outside the sealing bag.

8. A method for preparing the polymer splint according to any one of claims 1 to 7, It is characterized in that The steps include: Step 1: Dissolve the hydrogel monomer, crosslinking agent and photoinitiator in water to obtain solution A; prepare sodium acetate solution I to obtain solution B. Step 2: Mix solution A and solution B, keep the mixed solution in a liquid state, pour it into a mold, irradiate it with light corresponding to the initiator, and obtain the hydrogel composite after photocuring and cross-linking; Step 3: Load the obtained hydrogel complex into a coating layer, soften it, and cool it to obtain the polymer splint.

9. The method for preparing the polymer splint according to claim 8, It is characterized in that The hydrogel monomer is acrylamide, and the cross-linking agent is N,N'-methylenebisacrylamide.

10. The method for preparing the polymer splint according to claim 8, It is characterized in that The monomer accounts for 5-10% of the weight of the hydrogel, the crosslinker accounts for 0.1-0.5% of the weight of the hydrogel, the initiator accounts for 0.1-1% of the weight of the hydrogel, the sodium acetate accounts for 40-60% of the weight of the hydrogel, and the water accounts for 20-50% of the weight of the hydrogel; the weight of the hydrogel is the total weight of the hydrogel complex.