Sorting method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore
By using a combination of highly active quicklime and EMD-506 separation inhibitors in the Panxi mining area and combining the flotation process, the problem of the ineffective recycling of associated elements is solved, and the efficient separation of sulfur concentrate and cobalt concentrate is achieved, improving the improvement of Resource utilization value.
Patent Information
- Application Number
- CN202411255862.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-26
AI Technical Summary
There is little research on the comprehensive recycling of associated elements in Panxi mining area, which leads to serious waste of resources. Except for some sulfur being recycled, other associated minerals have not been effectively recycled.
Using highly active quicklime and EMD-506 separation inhibitors as special agent combinations of sulfhydryl ore, the sulfur concentrate and cobalt concentrate are realized through the process of one crude selection and three selections, combined with the use of a stirring barrel and flotation machine. efficient separation and recycling.
It has achieved efficient separation and recovery of sulfur ore and cobalt-rich minerals in sulfur ore, enhanced the comprehensive utilization value of ore, stabilized acquisition of cobalt-rich concentrate, and simplified the ore process.
Smart Images

Figure CN119016185A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flotation, and in particular relates to a separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore. Background Art
[0002] Cobalt is an important strategic metal with excellent high temperature resistance, corrosion resistance and magnetic properties. It is an important raw material and strategic resource for the manufacture of high temperature alloys, cemented carbides, ceramic pigments, etc. The prospective reserves of vanadium-titanium magnetite in Panzhihua area are as high as 10 billion tons. It is not only an important supplement to iron ore, but also the main carrier of chromium, vanadium and titanium resources. It is an important raw material for many metals such as steel, vanadium and titanium; and it also has considerable associated resources of sulfur, cobalt, nickel, copper, platinum group elements, rare earth elements and scattered elements. Among the associated resources in the four major mining areas of Panxi, the cobalt metal resources are 900,000 tons, nickel is 700,000 tons, rare earths are 1.5 million tons, scandium is 250,000 tons, gallium is 180,000 tons, and a large amount of copper, sulfur and other resources have extremely high comprehensive utilization value.
[0003] At present, there is little research on the comprehensive recovery of associated elements in the Panzhihua mining area and the level is low. Except for some sulfur that has been recovered, other associated minerals have basically not been recycled, resulting in serious waste of resources. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a separation method for separating sulfur concentrate and cobalt concentrate from sulfide-cobalt ore, which can efficiently separate and recover sulfur ore and cobalt-rich minerals in the sulfide-cobalt ore, thereby improving the comprehensive utilization value of the ore.
[0005] The present invention provides a separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore, which is characterized by comprising the following steps:
[0006] a) mixing sulphur-cobalt ore pulp, sodium xanthate, quicklime and EMD-506 type separation inhibitor to obtain slurry to be floated;
[0007] b) the ore pulp to be floated is sent to a roughing flotation machine for roughing, and sulfur concentrate foam and roughing tailings pulp are obtained respectively;
[0008] c) the roughing tailings slurry is sent to a refiner flotation machine for first refinement to obtain refiner concentrate foam and refiner tailings slurry;
[0009] The first concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the roughing flotation machine in step b) for cyclic treatment;
[0010] d) the first concentrate tailings slurry is sent to a second concentrate flotation machine for a second concentration to obtain second concentrate foam and second concentrate tailings slurry;
[0011] The froth of the secondary concentrate is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the primary concentrate flotation machine in step c) for cyclic treatment;
[0012] e) the refined secondary tailings slurry is sent to a refined tertiary flotation machine for a third concentration to obtain refined tertiary concentrate foam and cobalt-rich concentrate slurry;
[0013] The refined third concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the refined first flotation machine in step c) for cyclic treatment.
[0014] Preferably, in step a), the amount of sodium xanthate used is 40-60 g / t ore.
[0015] Preferably, in step a), the amount of quicklime used is 600-1500 g / t ore.
[0016] Preferably, in step a), the amount of the EMD-506 separation inhibitor used is 500-1000 g / t ore.
[0017] Preferably, in step c), the amount of quicklime used is 60-90 g / t ore.
[0018] Preferably, in step c), the amount of the EMD-506 separation inhibitor used is 70-100 g / t ore.
[0019] Preferably, in step d), the amount of quicklime used is 30-70 g / t ore.
[0020] Preferably, in step d), the amount of the EMD-506 separation inhibitor used is 20 to 60 g / t ore.
[0021] Preferably, in step e), the amount of quicklime used is 5-40 g / t ore.
[0022] Preferably, in step e), the amount of the EMD-506 separation inhibitor used is 10 to 60 g / t ore.
[0023] Compared with the prior art, the present invention provides a separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore, comprising the following steps: a) mixing sulphur-cobalt ore pulp, sodium xanthate, quicklime and EMD-506 type separation inhibitor to obtain slurry to be floated; b) sending the slurry to be floated into a roughing flotation machine for roughing, respectively obtaining sulfur concentrate foam and roughing tailings pulp; c) sending the roughing tailings pulp into a first refinement flotation machine for first refinement, respectively obtaining first refinement concentrate foam and first refinement tailings pulp; and the first refinement concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the first refinement flotation machine for first refinement. Return to the roughing flotation machine of step b) for cyclic treatment; d) the first concentrate tailings pulp is sent to the second concentrate flotation machine for the second selection, and the second concentrate concentrate foam and the second concentrate tailings pulp are obtained respectively; the second concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the first concentrate flotation machine of step c) for cyclic treatment; e) the second concentrate tailings pulp is sent to the third concentrate flotation machine for the third selection, and the third concentrate foam and the cobalt-rich concentrate pulp are obtained respectively; the third concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the first concentrate flotation machine of step c) for cyclic treatment. The present invention adopts "high-activity quicklime + EMD-506 type separation inhibitor" as a special agent combination for sulfur-cobalt separation of sulfide-cobalt ore, and adopts the separation process of "one roughing selection + three selections, and the intermediate ore is returned in sequence", so as to realize the efficient separation and recovery of sulfur ore and cobalt-rich minerals in sulfide-cobalt ore, and improve the comprehensive utilization value of ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0025] Figure 1 It is a selection flow chart provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The present invention provides a separation method for separating sulfur concentrate and cobalt concentrate from sulfide-cobalt ore, comprising the following steps:
[0028] a) mixing the slurry of the cobalt sulfide ore, sodium xanthate (xanthate), quicklime and EMD-506 type separation inhibitor to obtain the slurry to be floated;
[0029] b) the ore pulp to be floated is sent to a roughing flotation machine for roughing, and sulfur concentrate foam and roughing tailings pulp are obtained respectively;
[0030] c) the roughing tailings slurry is sent to a refiner flotation machine for first refinement to obtain refiner concentrate foam and refiner tailings slurry;
[0031] The first concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the roughing flotation machine in step b) for cyclic treatment;
[0032] d) the first concentrate tailings slurry is sent to a second concentrate flotation machine for a second concentration to obtain second concentrate foam and second concentrate tailings slurry;
[0033] The froth of the secondary concentrate is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the primary concentrate flotation machine in step c) for cyclic treatment;
[0034] e) the refined secondary tailings slurry is sent to a refined tertiary flotation machine for a third concentration to obtain refined tertiary concentrate foam and cobalt-rich concentrate slurry;
[0035] The refined third concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the refined first flotation machine in step c) for cyclic treatment.
[0036] In the present invention, the EMD-506 separation inhibitor is a commercially available product produced by the Institute of Comprehensive Utilization of Mineral Resources, Chinese Academy of Geological Sciences.
[0037] In the present invention, in step a), the amount of sodium xanthate is preferably 40-60 g / t, specifically 40 g / t, 45 g / t, 50 g / t, 55 g / t or 60 g / t; the amount of quicklime is preferably 600-1500 g / t, specifically 600 g / t, 650 g / t, 700 g / t, 750 g / t, 800 g / t, 850 g / t, 900 g / t, 1000 g / t, 1100 g / t, 1200 g / t, 1500 g / t, 1600 g / t, 1700 g / t, 1800 g / t, 1900 g / t, 2000 g / t, 2100 g / t, 2200 g / t, 2300 g / t, 2400 g / t, 2500 g / t, 2600 g / t, 2700 g / t, 2800 g / t, 2900 g / t, 3000 g / t, 3100 g / t, 3200 g / t, 3300 g / t, 3400 g / t, 3500 g / t, 3600 g / t, 3700 g / t, 3800 g / t, 3900 g / t, 4000 g / t, 4100 g / t, 4200 g / t, 4300 g / t, 4400 g / t, 4500 g / t, 4600 g / t, 4700 g / t, 4800 g / t, 4900 g / t, 5000 g / t, 5100 g / t, 5200 g / t 0g / t ore, 1200g / t ore, 1300g / t ore, 1400g / t ore or 1500g / t ore; the dosage of the EMD-506 separation inhibitor is preferably 500-1000g / t ore, specifically 500g / t ore, 550g / t ore, 600g / t ore, 650g / t ore, 700g / t ore, 750g / t ore, 800g / t ore, 850g / t ore, 900g / t ore, 950g / t ore or 1000g / t ore.
[0038] In the present invention, in step c), the amount of quicklime is preferably 60-90 g / t, specifically 60 g / t, 65 g / t, 70 g / t, 75 g / t, 80 g / t, 85 g / t or 90 g / t; the amount of EMD-506 separation inhibitor is preferably 70-100 g / t, specifically 70 g / t, 75 g / t, 80 g / t, 85 g / t, 90 g / t, 95 g / t or 100 g / t.
[0039] In the present invention, in step d), the amount of quicklime is preferably 30-70 g / t, specifically 30 g / t, 35 g / t, 40 g / t, 45 g / t, 50 g / t, 55 g / t, 60 g / t, 65 g / t or 70 g / t; the amount of EMD-506 separation inhibitor is preferably 20-60 g / t, specifically 20 g / t, 25 g / t, 30 g / t, 35 g / t, 40 g / t, 45 g / t, 50 g / t, 55 g / t or 60 g / t.
[0040] In the present invention, in step e), the amount of quicklime is preferably 5-40 g / t, specifically 5 g / t, 10 g / t, 15 g / t, 20 g / t, 25 g / t, 30 g / t, 35 g / t or 40 g / t; the amount of EMD-506 separation inhibitor is preferably 10-60 g / t, specifically 10 g / t, 15 g / t, 20 g / t, 25 g / t, 30 g / t, 35 g / t, 40 g / t, 45 g / t, 50 g / t, 55 g / t or 60 g / t.
[0041] The separation method provided by the present invention adopts "high-activity quicklime + EMD-506 separation inhibitor" as a special agent combination for sulfur-cobalt separation of sulfide-cobalt ore, and adopts a separation process of "one roughing + three fine cleanings, and sequential return of intermediate ore", thereby achieving efficient separation and recovery of sulfur ore and cobalt-rich minerals in sulfide-cobalt ore and improving the comprehensive utilization value of the ore.
[0042] The present invention solves the problem of directly separating the sulfur (cobalt) concentrate obtained by on-site production without grinding and de-doping, and can stably obtain cobalt-rich concentrate (Co≥1.0%). The sulfur content of the flotation separation tailings (sulfur concentrate) is the same as that of the feed ore, and does not affect the price of the original sulfur concentrate product. The mineral processing process is simple, which provides a reference for the comprehensive utilization of low-grade ores.
[0043] For the purpose of greater clarity, the invention is described in detail through the following examples.
[0044] Example 1
[0045] A separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore, such as Figure 1 As shown in the figure, the separation process of "mixing barrel + one roughing + three cleaning, and the intermediate ore is returned in sequence" is adopted, as follows:
[0046] (1) Start the slurry lifting mixing barrel (1 unit), add xanthate into the sulfide cobalt ore slurry (the S content of the sulfide cobalt ore is greater than 30wt%, the Co content is greater than 0.30wt%, the slurry concentration is 20wt%, and the -200 mesh content in the slurry is 60-75wt%) according to conventional operation, and the amount of xanthate added is 50g / t ore; add quicklime and EMD-506 in the mixing barrel according to a certain proportion, the quicklime addition ratio is 750g / t ore, and the EMD-506 addition ratio is 600g / t ore, so that the reagent and the sulfide cobalt ore are fully contacted, fused and reacted;
[0047] (2) Start the roughing flotation machine (3 units), adjust the valve at the roughing tailings end, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the roughing, specifically, the quicklime addition ratio is 80g / t ore, and the EMD-506 addition ratio is 90g / t ore; the roughing concentrate foam is sulfur concentrate, and the sulfur content is 31-33wt%.
[0048] (3) Start the first-stage flotation machine (2 units), adjust the valve at the tailings end of the first stage, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the second stage to the first stage, specifically, the addition ratio of quicklime is 50g / t ore, and the addition ratio of EMD-506 is 40g / t ore;
[0049] (4) Start the second-stage flotation machine (2 units), adjust the valve at the tailings end of the second-stage flotation machine, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the third stage of the second stage of the flotation machine, specifically, the addition ratio of quicklime is 20g / t ore, and the addition ratio of EMD-506 is 20g / t ore;
[0050] (5) Start the refined three flotation machine (1 unit) to produce qualified cobalt concentrate, which is transported to the cobalt concentrate storage pool through a slurry pump to meet the grade requirement of cobalt concentrate ≥1.0%.
[0051] Example 2
[0052] A separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore, such as Figure 1 As shown in the figure, the separation process of "mixing barrel + one roughing + three cleaning, and the intermediate ore is returned in sequence" is adopted, as follows:
[0053] (1) Start the slurry lifting mixing barrel (1 unit), add xanthate into the sulfide cobalt ore slurry (the S content of the sulfide cobalt ore is greater than 30wt%, the Co content is greater than 0.30wt%, the slurry concentration is 20wt%, and the -200 mesh content in the slurry is 60-75wt%) according to conventional operation, and the amount of xanthate added is 50g / t ore; add quicklime and EMD-506 in the mixing barrel according to a certain proportion, the quicklime addition ratio is 1200g / t ore, and the EMD-506 addition ratio is 900g / t ore, so that the reagent and the sulfide cobalt ore are fully contacted, fused and reacted;
[0054] (2) Start the roughing flotation machine (3 units), adjust the valve at the roughing tailings end, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the roughing, specifically, the quicklime addition ratio is 70g / t ore, and the EMD-506 addition ratio is 80g / t ore; the roughing concentrate foam is sulfur concentrate, and the sulfur content is 31-33wt%.
[0055] (3) Start the first-stage flotation machine (2 units), adjust the valve at the tailings end of the first stage, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the second stage to the first stage, specifically, the addition ratio of quicklime is 40g / t ore, and the addition ratio of EMD-506 is 30g / t ore;
[0056] (4) Start the second-stage flotation machine (2 units), adjust the valve at the tailings end of the second-stage flotation machine, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the third stage of the second stage of the flotation machine, specifically, the addition ratio of quicklime is 10g / t ore, and the addition ratio of EMD-506 is 30g / t ore;
[0057] (5) Start the refined three flotation machine (1 unit) to produce qualified cobalt concentrate, which is transported to the cobalt concentrate storage pool through a slurry pump to meet the grade requirement of cobalt concentrate ≥ 0.8%.
[0058] Example 3
[0059] A separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore, such as Figure 1 As shown in the figure, the separation process of "mixing barrel + one roughing + three cleaning, and the intermediate ore is returned in sequence" is adopted, as follows:
[0060] (1) Start the slurry lifting mixing barrel (1 unit), add xanthate into the sulfide cobalt ore slurry (the S content of the sulfide cobalt ore is greater than 30wt%, the Co content is greater than 0.30wt%, the slurry concentration is 20wt%, and the -200 mesh content in the slurry is 60-75wt%) according to conventional operation, and the amount of xanthate added is 50g / t ore; add quicklime and EMD-506 in the mixing barrel according to a certain proportion, the quicklime addition ratio is 1400g / t ore, and the EMD-506 addition ratio is 900g / t ore, so that the reagent and the sulfide cobalt ore are fully contacted, fused and reacted;
[0061] (2) Start the roughing flotation machine (3 units), adjust the valve at the roughing tailings end, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the roughing, specifically, the quicklime addition ratio is 70g / t ore, and the EMD-506 addition ratio is 80g / t ore; the roughing concentrate foam is sulfur concentrate, and the sulfur content is 31-33wt%.
[0062] (3) Start the first-stage flotation machine (2 units), adjust the valve at the tailings end of the first stage, control the amount of flotation concentrate foam, and add some reagents to the pulp foam returned from the second stage to the first stage, specifically, the quicklime addition ratio is 65g / t ore, and the EMD-506 addition ratio is 50g / t ore;
[0063] (4) Start the second-stage flotation machine (2 units), adjust the valve at the tailings end of the second-stage flotation machine, control the amount of flotation concentrate foam hanging out, and add some reagents to the pulp foam returned from the third stage of the second stage of the flotation machine, specifically, the addition ratio of quicklime is 30g / t ore, and the addition ratio of EMD-506 is 55g / t ore;
[0064] (5) Start the refined three flotation machine (1 unit) to produce qualified cobalt concentrate, which is transported to the cobalt concentrate storage pool through a slurry pump to meet the grade requirement of cobalt concentrate ≥1.2%.
[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A separation method for separating sulfur concentrate and cobalt concentrate from sulfur-cobalt ore, characterized in that: The following steps are involved: a) mixing sulphur-cobalt ore pulp, sodium xanthate, quicklime and EMD-506 type separation inhibitor to obtain slurry to be floated; b) the ore pulp to be floated is sent to a roughing flotation machine for roughing, and sulfur concentrate foam and roughing tailings pulp are obtained respectively; c) the roughing tailings slurry is sent to a refiner flotation machine for first refinement to obtain refiner concentrate foam and refiner tailings slurry; The first concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the roughing flotation machine in step b) for cyclic treatment; d) the first concentrate tailings slurry is sent to a second concentrate flotation machine for a second concentration to obtain second concentrate foam and second concentrate tailings slurry; The froth of the secondary concentrate is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the primary concentrate flotation machine in step c) for cyclic treatment; e) the refined secondary tailings slurry is sent to a refined tertiary flotation machine for a third concentration to obtain refined tertiary concentrate foam and cobalt-rich concentrate slurry; The refined third concentrate foam is supplemented with quicklime and EMD-506 type separation inhibitor and then returned to the refined first flotation machine in step c) for cyclic treatment.
2. The selection method according to claim 1, characterized in that: In step a), the amount of sodium xanthate used is 40-60 g / t ore.
3. The selection method according to claim 1, characterized in that: In step a), the amount of quicklime used is 600-1500 g / t ore.
4. The selection method according to claim 1, characterized in that: In step a), the dosage of the EMD-506 separation inhibitor is 500-1000 g / t ore.
5. The selection method according to claim 1, characterized in that: In step c), the amount of quicklime used is 60-90 g / t ore.
6. The selection method according to claim 1, characterized in that: In step c), the dosage of the EMD-506 separation inhibitor is 70-100 g / t ore.
7. The selection method according to claim 1, characterized in that: In step d), the amount of quicklime used is 30-70 g / t ore.
8. The selection method according to claim 1, characterized in that: In step d), the amount of the EMD-506 separation inhibitor used is 20 to 60 g / t ore.
9. The selection method according to claim 1, characterized in that: In step e), the amount of quicklime used is 5-40 g / t ore.
10. The sorting method according to claim 1, characterized in that: In step e), the dosage of the EMD-506 separation inhibitor is 10 to 60 g / t ore.