Decorative sheet and decorative sheet

By using a multi-layer structure, microcrystalline resin layer and inorganic particles in the decorative sheet, the high load-load abrasion resistance and bending processability of the decorative sheet are improved, and the insufficient abrasion resistance and bending process in the prior art are solved. Poor sex problem.

CN119017806APending Publication Date: 2024-11-26DAI NIPPON PRINTING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411304305.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-02-28
Filing Date
2018-02-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing decorative sheets are insufficiently resistant to abrasion under high load conditions, and are prone to cracks or breaks of surface protective layer during bending processing, making it difficult to take into account both abrasion resistance and bending processing.

Method used

A structure consisting of a first olefin resin layer, a second olefin resin layer and a surface protective layer is adopted, wherein the indentation hardness of the second olefin resin layer is HIT2≥100MPa, the indentation hardness of the surface protective layer is HIT1>HIT2, and HIT1≥450MPa , the hardness and abrasion resistance are improved by the use of microcrystalline olefin resin layer and inorganic fine particles.

Benefits of technology

It achieves scratch resistance and excellent bending processability under high load conditions, avoids cracks and breaks of the surface protective layer during bending process, and improves the overall performance of the decorative sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017806A_ABST
    Figure CN119017806A_ABST
Patent Text Reader

Abstract

Provided are: a decorative sheet having excellent scratch resistance under high load conditions and excellent bending workability; and a decorative plate using the decorative sheet. Specifically, the present invention provides a decorative sheet and a decorative sheet using the same, the decorative sheet being characterized by having a first olefin resin layer, a second olefin resin layer, and a surface protective layer in this order, the indentation hardness HIT2 of the second olefin resin layer and the indentation hardness HIT1 of the surface protective layer satisfying the following formulae (1) and (2): HIT2 > = 100 MPa (1) and HIT1 > HIT2 (2).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is filed on February 28, 2018 、Application number is 201880014480.3 (PCT / JP2018 / 007437) , divisional application with the invention name of decorative sheet and decorative panel. Technical Field

[0002] The invention relates to a decorative sheet and a decorative board. Background Art

[0003] In order to improve the scratch resistance of decorative sheets used as surface materials of building materials, etc., a method of forming a surface protective layer of the sheet from a cured coating of an ionizing radiation curing resin is known. However, even if such decorative sheets are formed as floor decorative sheets with excellent scratch resistance, they are not completely free from damage and there is a problem that they are also damaged when performing damage tests under high load conditions (Patent Document 1).

[0004] Furthermore, in order to use the decorative sheet not only for residential floors but also for floors in various usage situations such as non-residential floors such as shops, it is desired to further improve the scratch resistance of the surface protective layer of the decorative sheet.

[0005] Therefore, in order to further improve the scratch resistance of the decorative sheet under high load conditions, it is proposed to harden the surface protective layer. However, if the surface protective layer is made too hard, cracks and breaks may occur in the surface protective layer when the decorative sheet is subjected to bending processing such as V-cutting and wrapping. Thus, it is not easy to achieve both bending adaptability and hardness for scratch resistance in a decorative sheet.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-74683 Summary of the invention

[0009] Problems to be solved by the invention

[0010] An object of the present invention is to provide a decorative sheet having excellent scratch resistance under high load conditions and excellent bending workability, and a decorative plate using the decorative sheet.

[0011] Methods for solving problems

[0012] The inventors of the present invention have conducted intensive studies to achieve the above-mentioned object and have found that the following decorative sheets and decorative panels can solve the problems of the present invention.

[0013] 1. A decorative sheet, characterized in that:

[0014] The invention has a first olefin resin layer, a second olefin resin layer and a surface protection layer in this order,

[0015] The indentation hardness H of the second olefin resin layer IT 2 The indentation hardness H of the surface protective layer IT 1 Satisfies the following equations (1) and (2):

[0016] H IT 2 ≥100MPa (1);

[0017] H IT 1 >H IT 2 (2).

[0018] 2. The decorative sheet as described in item 1 above, wherein:

[0019] The indentation hardness H of the surface protective layer IT 1 Satisfies the following formula (3):

[0020] 450MPa>H IT 1 (3).

[0021] 3. The decorative sheet according to item 1 or 2 above, wherein:

[0022] The indentation hardness H of the second olefin resin layer IT 2 The indentation hardness H of the first olefin resin layer is IT 3 Satisfies the following formula (4):

[0023] H IT 2 >H IT 3 (4).

[0024] 4. The decorative sheet according to any one of items 1 to 3 above, wherein

[0025] The second olefin resin layer is a microcrystallized olefin resin layer.

[0026] 5. The decorative sheet according to any one of items 1 to 4 above, wherein

[0027] The surface protection layer contains inorganic fine particles having an average particle size of 10 μm or less.

[0028] 6. A decorative board comprising a laminate having a decorative board base material and the decorative sheet according to any one of items 1 to 5 above in this order in the thickness direction.

[0029] Effects of the Invention

[0030] According to the present invention, a decorative sheet having excellent scratch resistance under high load conditions and excellent bending workability and a decorative plate using the decorative sheet can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram showing a cross section of one embodiment of the decorative sheet of the present invention.

[0032] Figure 2 This is a schematic diagram showing a cross section of another embodiment of the decorative sheet of the present invention.

[0033] Figure 3 This is a schematic diagram showing a cross section of a decorative board formed by combining the decorative sheet of the present invention and a decorative board base material.

[0034] Figure 4 This is a diagram for explaining the method of measuring the indentation hardness in this specification.

[0035] Explanation of symbols

[0036] 1: surface protection layer; 2: second olefin resin layer; 3: first olefin resin layer; 4: recess (embossed recess); 10: decorative sheet; 11: decorative board substrate; 12: decorative board; 20: measurement sample; 21: Berkovich indenter; 22: direction of load application. DETAILED DESCRIPTION

[0037] 1. Decorative sheet

[0038] Hereinafter, the decorative sheet and decorative board of the present invention will be described in detail.

[0039] Figure 1 1 is a schematic diagram showing a cross section of one embodiment of the decorative sheet of the present invention, and shows a decorative sheet 10 having a first olefin resin layer 3, a second olefin resin layer 2, and a surface protection layer 1 in this order in the thickness direction. Figure 2 In the embodiment, the embossed recessed portion 4 is formed at least from the surface protection layer side. Hereinafter, the present invention will be described with reference to the drawings as appropriate.

[0040] In this manual, Figure 1 For example, the direction in which the surface protection layer 1 is laminated when viewed from the second olefin resin layer 2 is referred to as "upper" or "front side", and the direction in which the first olefin resin layer 3 is laminated when viewed from the second olefin resin layer 2 is referred to as "lower" or "back side". Furthermore, the "front (side) surface" or "surface protection layer (side) surface" of a decorative sheet or decorative board refers to the surface that can be identified after the construction of the decorative sheet or decorative board.

[0041] In addition, in this specification, the numerical range indicated by "to" means "above" or "below." For example, the notation of α to β mm means α mm or more and β mm or less.

[0042] (Decorative piece)

[0043] The decorative sheet 10 of the present invention is characterized in that Figure 1 The decorative sheet shown in the figure has a first olefin resin layer 3, a second olefin resin layer 2 and a surface protection layer 1 in sequence,

[0044] Indentation hardness H of the second olefin resin layer 2 IT 2 The indentation hardness H of the surface protection layer 1 IT 1 Satisfies the following equations (1) and (2):

[0045] H IT 2 ≥100MPa (1);

[0046] H IT 1 >H IT 2 (2).

[0047] (Indentation hardness)

[0048] In this specification, the "indentation hardness" of each layer refers to the nanoindentation hardness measured using a surface film physical property testing machine Triboindenter (registered trademark) "TI-950" (manufactured by HYSITRON Corporation).

[0049] In addition, the indentation hardness (H) of each layer was obtained using Triboindenter (registered trademark) "TI-950". IT ) is measured as follows.

[0050] (1) Use Figure 4 The Berkovich indenter shown in (a) is Figure 4 As shown in (b), the Berkovich indenter is pressed into the test sample under the indentation conditions described later, and the "contact projection area (Ap) (mm) corrected by the method of the device standard is calculated from the geometric shape of the triangular hammer formed on the surface. 2 )”, by setting the maximum test load (F max ) divided by the above Ap to calculate the hardness.

[0051] That is, H IT =F max / Ap.

[0052] (2) Here, regarding the pressing conditions, the first olefin resin layer and the second olefin resin layer are pressed at room temperature (laboratory ambient temperature). Figure 4 As shown in (c), first, a load of 0 μN is applied for 5 seconds to 50 μN (i.e., 10 μN / s), and then 50 μN (F max ) for 5 seconds, and finally, the load was removed from 50 μN in 10 seconds to 0 μN. In addition, for the surface protection layer, first, a load of 0 μN was applied in 10 seconds to 100 μN (i.e., 10 μN / s), and then 100 μN (F max ) for 5 seconds, and finally, the load is removed from 100 μN for 10 seconds to 0 μN. Usually, the indentation amount (h) is about 100 to 150 nm, so the thickness of the layer in the indentation direction of the measurement sample is 1.0 μm or more (preferably 1.5 μm or more).

[0053] Ap through 24.50〔h max -ε(h max -h r )〕 2 Calculate (here, ε is the correction factor set according to the geometric shape of the indenter, h r It is the depth of the triangular pyramidal geometric shape remaining on the surface after the load is removed. ).

[0054] (3) In addition, when measuring the hardness, in order to avoid the influence of the hardness of layers other than the layer used as the measurement sample, the hardness of the cross section of the layer to be measured is measured. That is, the decorative sheet is embedded with a resin (cold-curing type epoxy two-component curing resin), and after being left at room temperature for more than 24 hours to cure, the cured embedded sample is mechanically polished to expose the cross section of the layer to be measured, and the cross section of the layer to be measured (when the layer contains particles of filler material, etc., at a position avoiding the particles) is pressed with the above-mentioned Berkovich indenter, thereby measuring the hardness of the cross section of each layer.

[0055] (4) For each layer, the indentation hardness was measured at 10 locations to avoid deviation, and the average value of the 10 locations was taken as the "indentation hardness H of the surface protective layer". IT 1 ", " ", "The indentation hardness H of the second olefin resin layer IT 2 " and "indentation hardness H of the first olefin resin layer IT 3 ”.

[0056] In the present invention, the indentation hardness H of the second olefin resin layer is required to be IT 2 The indentation hardness H of the surface protective layer IT1 The following formulas (1) and (2) are satisfied. If the indentation hardness of the second olefin resin layer and the surface protective layer does not satisfy the following formulas (1) and (2), excellent scratch resistance and bending workability under high load conditions cannot be obtained.

[0057] H IT 2 ≥100MPa (1);

[0058] H IT 1 >H IT 2 (2)

[0059] In order to demonstrate the scratch resistance under a relatively high load, the indentation hardness H of the surface protection layer needs to be IT 1 Greater than the indentation hardness H of the second olefin resin layer IT 2 , and exceeds 100MPa.

[0060] In addition, from the viewpoint of obtaining excellent scratch resistance and good bending workability, the indentation hardness H of the surface protection layer is preferably IT 1 Satisfies the following formula (3):

[0061] 450MPa>H IT 1 (3).

[0062] In addition, from the viewpoint of obtaining excellent scratch resistance and good bending workability, the indentation hardness H of the second olefin resin layer is preferably IT 2 and the indentation hardness H of the first olefin resin layer IT 3 Satisfies the following formula (4):

[0063] H IT 2 >H IT 3 (4).

[0064] (First olefin resin layer)

[0065] The first olefin resin layer is a layer containing an olefin resin, and examples of the olefin resin include: homopolymers of olefins such as ethylene, propylene, and butene; block copolymers and random copolymers of ethylene-propylene; copolymers of at least one of ethylene and propylene with at least one other olefin such as butene, pentene, and hexene; copolymers of at least one of ethylene and propylene with at least one other monomer such as vinyl acetate and vinyl alcohol; etc. Among them, polyethylene and polypropylene are preferred, and polyethylene is particularly preferred from the viewpoint of obtaining excellent scratch resistance and good bending processability.

[0066] Polyethylene may be a homopolymer of ethylene or a copolymer of ethylene and other comonomers copolymerizable with ethylene (e.g., α-olefins such as propylene, 1-butene, 1-hexene, 1-octene, vinyl acetate, vinyl alcohol, etc.). As polyethylene resins, for example, high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (VLDPE), ultra-high molecular weight polyethylene (UHMWPE), cross-linked polyethylene (PEX), etc. may be cited. These polyethylenes may be used alone or in combination of two or more.

[0067] The polypropylene may be a homopolymer of propylene or a copolymer of propylene and other comonomers copolymerizable with propylene (e.g., α-olefins such as ethylene, 1-butene, 1-hexene, 1-octene, etc.; vinyl acetate, vinyl alcohol, etc.). These polypropylenes may be used alone or in combination of two or more.

[0068] It is preferred that the indentation hardness H of the first olefin resin layer IT 3 The indentation hardness H of the second olefin layer IT 2 It has the relationship of the above formula (4).

[0069] Among them, from the viewpoint of obtaining excellent scratch resistance and good bending workability, the indentation hardness H of the first olefin resin layer is IT 3 It is preferably 10 to 80 MPa, more preferably 15 to 70 MPa, further preferably 20 to 60 MPa, and particularly preferably 30 to 55 MPa. By being within such a range, the scratch resistance and impact resistance (especially dent resistance) of the decorative sheet can be well maintained, and the first olefin resin layer can be prevented from stretching due to the tension applied during printing or coating by a printing machine. In addition, cracking and breaking of the surface protective layer during bending can be easily suppressed, and the impact resistance (especially crack resistance) can be well maintained.

[0070] In addition, the indentation hardness can be appropriately set by mixing two or more resins having different hardnesses or by mixing an elastomer into a resin.

[0071] From the viewpoint of excellent scratch resistance and bending workability, the thickness of the first olefin resin layer is preferably 30 to 120 μm, more preferably 40 to 110 μm, further preferably 50 to 100 μm, particularly preferably 55 to 85 μm.

[0072] In addition, the thickness of the first olefin resin layer, the second olefin resin layer, and the surface protection layer in this specification is an average value when the thickness is measured at 10 locations.

[0073] (Second olefin resin layer)

[0074] The second olefin resin layer is a layer containing olefin resin and is required to have an indentation hardness H IT 2 A layer satisfying the above formulae (1) and (2).

[0075] The olefin resin forming the second olefin resin layer may be the same as the olefin resin forming the first olefin resin layer. Among them, polyethylene and polypropylene are preferred, and polypropylene is particularly preferred from the viewpoint of excellent scratch resistance and bending workability.

[0076] Polypropylene may be a homopolymer of propylene or a copolymer of propylene and other comonomers copolymerizable with propylene (e.g., α-olefins such as ethylene, 1-butene, 1-hexene, 1-octene, etc.; vinyl acetate, vinyl alcohol, etc.). These polypropylenes may be used alone or in combination of two or more. In the present invention, a homopolymer of propylene (homopolypropylene) is particularly preferred from the viewpoint of excellent scratch resistance and bending workability.

[0077] The second olefin resin layer is required to have an indentation hardness H IT 2 An olefin resin layer that satisfies the following formulae (1) and (2), and preferably satisfies the following formula (4).

[0078] H IT 2 ≥100MPa (1);

[0079] H IT 1 >H IT 2 (2)

[0080] H IT 2 >H IT 3 (4)

[0081] From the viewpoint of the balance between abrasion resistance and bending workability, the indentation hardness H of the second olefin resin layer is IT 2 It is preferably from 100 MPa to 200 MPa, more preferably from 105 MPa to 150 MPa, and even more preferably from 110 MPa to 130 MPa.

[0082] H IT 2 When the pressure is less than 100 MPa, the scratch resistance and impact resistance (particularly dent resistance) may be deteriorated, or the second olefin resin layer may be stretched due to the tension applied during printing or coating by a printer. When the pressure exceeds 200 MPa, the surface protective layer may crack or break during bending, resulting in deterioration of impact resistance (particularly crack resistance).

[0083] In order to easily adjust the indentation hardness H IT 2 For example, it can be appropriately set by mixing two or more resins having different hardnesses, mixing an elastomer into a resin, making the second olefin resin layer a microcrystalline olefin resin layer, and the like.

[0084] In order to obtain the microcrystalline olefin resin layer, for example, a crystal nucleating agent may be added to the olefin resin composition forming the second olefin resin layer, melted, and then cooled. In this case, as a cooling method, for example, cooling using a chill roll may be cited: during extrusion molding, the material extruded from the die is brought into contact with a chill roll (chill roll) through which cooling water flows to cool it.

[0085] As crystal nucleating agents, for example, metal salt crystal nucleating agents such as fatty acid metal salts, metal salts of phosphonic acid, metal salts of phosphonate esters, metal salts of benzoic acid, metal salts of pimelic acid, and metal salts of rosin can be cited; organic crystal nucleating agents such as fatty acid esters, aliphatic amides, sorbitan benzyl esters, quinacridone, and phthalocyanine blue can be cited; inorganic crystal nucleating agents such as talc can be cited; and the like.

[0086] In addition, as the crystal nucleating agent, the crystal nucleating agent in which the above-mentioned crystal nucleating agent is enclosed in a nanoshell can also be used. By using the crystal nucleating agent enclosed in the nanoshell, since the crystal nucleating agent is more uniformly dispersed in the second olefin resin layer, it is possible to easily and stably adjust the indentation hardness H without being restricted by various conditions such as melting conditions and cooling conditions. IT 2 , and obtain excellent scratch resistance and good bending workability.

[0087] In the present invention, "nanoshell" refers to "a hollow small cell body with a nanometer-sized closed shell-like membrane structure", preferably less than 380nm, more preferably less than 375nm. The average primary particle size is a value calculated by statistical processing of an observation image measured by a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM). The calculation is performed by statistical processing, specifically, the diameter of 1000 particles randomly selected from the SEM image is measured, and a histogram divided by 3nm is prepared. At this time, the following formula (A) is used for calculation. The number average primary particle size D obtained by the formula (A) is np It is referred to as the average primary particle size in this specification.

[0088] D np =Σn i D i / Σn i (A)

[0089] D np : Number average molecular weight

[0090] D i : The diameter of the i-th histogram

[0091] n i : Frequency

[0092] In the present invention, the average primary particle size of the nanoshell is preferably lower than the wavelength region of visible light (380 to 750 nm) and is about 1 / 2 or less of the wavelength of visible light, that is, lower than 380 nm, more specifically, preferably 1 nm or more and lower than 380 nm, more preferably 1 to 375 nm, further preferably 5 to 300 nm, further preferably 10 to 250 nm, and particularly preferably 15 to 200 nm. When the average primary particle size is within the above range, the indentation hardness of the second olefin resin layer can be more easily adjusted, and excellent scratch resistance and bending processability can be obtained.

[0093] As a nanoshell, there is no particular limitation as long as it can enclose the above-mentioned crystal nucleating agent, and it can be a single-layer film or a multi-layer film. From the perspective of further reducing the average primary particle size and improving the dispersibility of the crystal nucleating agent, thereby more efficiently improving the excellent scratch resistance and bending processability, a single-layer film is preferred. In addition, as a material for forming the nanoshell, from the perspective of more easily adjusting the indentation hardness of the second olefin resin layer and obtaining excellent scratch resistance and bending processability, phospholipids are preferred.

[0094] In the present invention, as the form of the nanoshell, a monolayer film composed of phospholipids is preferred. By forming the nanoshell composed of phospholipids, the compatibility with the resin forming the second olefin resin layer is improved, so it is advantageous in adjusting the indentation hardness of the second olefin resin layer to obtain excellent scratch resistance and bending processability. In addition, by making the nanoshell a monolayer film, the average primary particle size is smaller, so the dispersibility of the crystal nucleating agent can be improved through the synergistic effect of the improved dispersibility obtained by the phospholipids forming the nanoshell, and the indentation hardness of the second olefin resin layer can be adjusted more efficiently, and excellent scratch resistance and bending processability can be obtained.

[0095] Examples of the phospholipids include phosphatidylcholine, phosphatidyldiethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiolipin, egg yolk phosphatidylcholine, hydrogenated egg yolk phosphatidylcholine, soybean phosphatidylcholine, hydrogenated soybean phosphatidylcholine, and the like glycerophospholipids; sphingomyelin, phosphoethanolamineceramide, phosphoglycerolceramide, and the like sphingomyelins; etc. These phospholipids can be used alone or in combination or in combination of two or more.

[0096] Examples of the method for encapsulating the above-mentioned crystal nucleating agent in a nanoshell include the Bangham method, the extrusion method, the hydration method, the surfactant dialysis method, the reverse phase evaporation method, the freeze-melt method, and the supercritical reverse phase evaporation method.

[0097] Here, the Bangham method is a method in which phospholipids are added to a solvent such as chloroform or methanol and dissolved, and then the solvent is removed by an evaporator to form a thin film composed of phospholipids. After adding the above-mentioned crystal nucleating agent, a stirrer is used to stir at a high speed of, for example, about 1000 to 2500 rpm, thereby hydrating and dispersing the crystal nucleating agent, and the crystal nucleating agent is encapsulated in the nanoshell. The extrusion method is a method in which a stirrer is replaced as an external agitator and the mixture is passed through a filter. The hydration method is a method in which a stirrer is not used in the Bangham method, but gentle stirring is performed to disperse the mixture, and the crystal nucleating agent is encapsulated in the nanoshell. The reverse phase evaporation method is a method in which phospholipids are dissolved in a solvent such as diethyl ether or chloroform, and the above-mentioned crystal nucleating agent is added (it can be made into a dispersion state.) to make a W / O emulsion, and the solvent is removed from the emulsion under reduced pressure, and water is added to encapsulate the crystal nucleating agent in the nanoshell. The freeze-melt method is a method of performing at least one of cooling and heating as external agitation, and is a method of enclosing a crystal nucleating agent in a nanoshell by repeating cooling and heating.

[0098] In addition, by adopting the supercritical reverse phase evaporation method, the nanoshell can be more reliably and easily formed into a monolayer membrane composed of phospholipids. The supercritical reverse phase evaporation method is a method of encapsulating a crystal nucleating agent in a nanoshell using carbon dioxide under supercritical conditions, or temperature conditions above the critical point, or pressure conditions. Here, supercritical carbon dioxide refers to carbon dioxide in a supercritical state above the critical temperature (30.98°C) and the critical pressure (7.3773±0.0030MPa), and carbon dioxide under temperature conditions above the critical point or pressure conditions refers to carbon dioxide under conditions where only the temperature or critical side exceeds the critical condition.

[0099] Specifically, the supercritical reverse phase evaporation method is a method in which water is added to the mixture of the above-mentioned crystal nucleating agent, supercritical carbon dioxide and phospholipids, and an emulsion of supercritical carbon dioxide and water phase is formed by stirring, and then the carbon dioxide is expanded and evaporated by reducing pressure, and a phase transfer occurs to form a nanoshell whose surface of the crystal nucleating agent is covered by a monolayer membrane of phospholipids, thereby obtaining a crystal nucleating agent enclosed in the nanoshell. In addition, as in the prior art, when multiple membranes are to be formed, in the above-mentioned method, supercritical carbon dioxide can be added to the mixture of the crystal nucleating agent, phospholipids and water.

[0100] In the present invention, the nanoshell can be composed of the following dispersants: materials other than phospholipids, such as aliphatic polycarboxylic acids, polycarboxylic acid alkylamines, poly (meth) acrylic acid, etc., with a molecular weight of 10,000 to 500,000, preferably 15,000 to 300,000, and more preferably 20,000 to 200,000 high molecular surfactants; lauric acid, palmitic acid, stearic acid, behenic acid, montanic acid, ricinoleic acid, etc., preferably saturated or unsaturated fatty acids with 10 to 30 carbon atoms, more preferably 12 to 28 carbon atoms, and lithium, sodium, potassium, magnesium fatty acid metal salts obtained by combining with metals such as calcium, barium, zinc, and aluminum; (meth)acryloxy-based silane coupling agents such as (meth)acryloxypropyltriethoxysilane and (meth)acryloxypropyltrimethoxysilane, vinyl-based silane coupling agents such as vinyltriethoxysilane and vinyltrimethoxysilane, epoxy-based silane coupling agents such as (ethoxycyclohexyl)ethyltrimethoxysilane and glycidoxypropyltrimethoxysilane, isocyanates such as isocyanatepropyltriethoxysilane, Silane coupling agents such as phenyl-based silane coupling agents such as phenyltrimethoxysilane; titanate coupling agents such as tetrakis[bis(allyloxymethyl)butoxy]titanium, diisostearate dipropoxytitanium, (butoxycarbonylbenzyloxy)tributoxytitanium, triisostearate isopropyl titanium, dibutoxy-bis(triethanolamine)titanium, tetrakis(ethylhexyloxy)titanium, dipropoxy-bis(acetylacetonate)titanium; dimethyl silicone oil, methylphenyl silicone oil, methyl hydrogen silicone oil, cyclic dimethyl silicone oil, alkyl modified silicone oil Silicone oils such as polypropylene wax, polyethylene wax, polypropylene polyethylene copolymer wax, microcrystalline wax, liquid paraffin, Fischer-Tropsch wax, Sasol wax, etc., hydrocarbon waxes such as ester waxes of aliphatic carboxylic acids having preferably 10 to 30 carbon atoms, more preferably 12 to 24 carbon atoms and dipentaerythritol, carnauba wax, montan wax, etc., deoxidized waxes such as polyolefin resins modified with organic acids such as maleic acid, sulfonic acid, carboxylic acid, rosin acid, etc., etc. These dispersants can be used alone or in combination of two or more.

[0101] As an example of a method for producing a crystal nucleating agent encapsulated in a nanoshell, a case where a phosphonate metal salt-based crystal nucleating agent (sodium 2,2′-methylenebis-(4,6-di-tert-butylphenyl)phosphonate) is used as the crystal nucleating agent will be described in more detail.

[0102] 100 parts by mass of an organic solvent such as methanol, 60 to 100 parts by mass of the above-mentioned phosphonate metal salt crystal nucleating agent as a crystal nucleating agent, and 2 to 10 parts by mass of phosphatidylcholine as a phospholipid are added to a container maintained at 40 to 70°C and sealed, and carbon dioxide is supplied to the container in such a way that the internal pressure reaches 7.5 to 25 MPa to make it a supercritical state. After that, the container is stirred at a high speed of about 1000 to 2500 rpm, and 50 to 150 parts by mass of ion exchange water are supplied. While maintaining the temperature and pressure in a supercritical state, stirring will continue for about 10 to 25 minutes, and then, carbon dioxide is discharged from the container to restore the atmospheric pressure in the container, thereby making it possible to prepare a crystal nucleating agent (phosphonate metal salt crystal nucleating agent) of a nanoshell enclosed in a single-layer membrane composed of phospholipids. The primary average particle size of the obtained crystal nucleating agent enclosed in the nanoshell is about 10 to 250 nm.

[0103] The content of the crystal nucleating agent in the second olefin resin layer is preferably 0.01 to 5 parts by mass, more preferably 0.02 to 3 parts by mass, further preferably 0.03 to 1 part by mass, and particularly preferably 0.05 to 0.5 parts by mass relative to 100 parts by mass of the resin component forming the second olefin resin layer. By setting the content of the crystal nucleating agent within the above range, it is easy to disperse uniformly in the resin forming the second olefin resin layer, it is easy to obtain the effect as a crystal nucleating agent, and the indentation hardness H can be easily and stably adjusted. IT 2 , and obtain excellent scratch resistance and bending workability.

[0104] From the viewpoint of obtaining excellent scratch resistance and bending processability, the thickness of the second olefin resin layer is preferably 30 to 120 μm, more preferably 40 to 110 μm, further preferably 50 to 100 μm, and particularly preferably 55 to 85 μm. When the thickness is less than 30 μm, there is a concern that the scratch resistance and impact resistance (particularly dent resistance) may be poor, or the second olefin resin layer may be stretched due to the tension applied during printing or coating by a printer. In addition, when the thickness exceeds 120 μm, there is a concern that the surface protective layer may crack or break during bending, resulting in a deterioration in impact resistance (particularly crack resistance).

[0105] (Surface protection layer)

[0106] Surface protection layer such as Figure 1 and 2 As shown in FIG. 1 , it is a layer provided on the outermost surface of the decorative sheet and exposed to the outside, and is provided to improve the surface properties of the decorative sheet such as anti-fouling, anti-scratch, and anti-chemical. In addition, the indentation hardness H of the surface protective layer is required to be IT 1 The following formula (2) is satisfied.

[0107] H IT 1 >H IT 2 (2)

[0108] In order to exhibit abrasion resistance under a relatively high load, the indentation hardness H of the surface protective layer needs to be IT 1 Greater than the indentation hardness H of the second olefin resin layer IT 2 , and exceeds 100MPa.

[0109] In addition, the indentation hardness can be appropriately set by mixing two or more resins having different hardnesses or by mixing an elastomer into a resin.

[0110] In addition, from the viewpoint of scratch resistance, the indentation hardness H IT 1 It is preferably 170 MPa or more, more preferably 250 MPa or more, further preferably 300 MPa or more, and further preferably 350 MPa or more.

[0111] In addition, from the viewpoint of bending workability, the indentation hardness H IT 1 It preferably satisfies the following formula (3), is more preferably 400 MPa or less, further preferably 350 MPa or less, and further preferably 320 MPa or less.

[0112] 450MPa>H IT 1 (3)

[0113] In addition, the above indentation hardness H IT 1 The upper and lower limits of the multi-level preferred range can be combined respectively. For example, the maximum value of the lower limit and the maximum value of the upper limit can be combined to make H IT 1 The range is 350 MPa or more and less than 450 MPa.

[0114] From the viewpoint of improving the surface properties of the decorative sheet such as stain resistance, scratch resistance, and chemical resistance and satisfying the above-mentioned indentation hardness, the surface protection layer is preferably composed of a cured product of a curable resin composition. As the curable resin composition, for example, there can be mentioned resin compositions containing curable resins such as thermosetting resins, two-component curable resins, and ionizing radiation curable resins. From the viewpoint of obtaining more excellent surface properties, as the curable resin, a resin composition containing a two-component curable resin and an ionizing radiation curable resin is preferred.

[0115] The two-component curable resin is not particularly limited as long as it is a resin that can be cured by a main component and a curing agent, but preferably, a two-component curable polyurethane resin in which a main component is a polyol (multivalent alcohol) and a curing agent is an isocyanate curing agent is mentioned.

[0116] Preferred examples of the main agent include polyols such as polyethylene glycol, polypropylene glycol, butanediol, neopentyl glycol, and 1,6-hexanediol; polyols having a hydroxyl group as a functional group such as acrylic polyol, polyester polyol, and polyether polyol; etc. These can be used alone or in combination of two or more.

[0117] In addition, as the isocyanate curing agent, any known compound may be used as appropriate, for example, aromatic isocyanates such as 2,4-toluene diisocyanate (TDI), xylylene diisocyanate (XDI), and naphthalene diisocyanate; aliphatic (or alicyclic) isocyanates such as 1,6-hexamethylene diisocyanate (HMDI), isophorone diisocyanate (IPDI), methylene diisocyanate (MDI), and hydrogenated toluene diisocyanate; and polyisocyanates such as the above. In addition, adducts or polymers of these various isocyanates, such as adducts of toluene diisocyanate, toluene diisocyanate trimers, etc. may be used.

[0118] Ionizing radiation curable resin is a resin that is cured by irradiation with ionizing radiation, i.e., radiation having energy quanta that can polymerize or crosslink molecules among electromagnetic waves or charged particle radiation, such as ultraviolet rays (UV) or electron beams (EB), and electromagnetic waves such as X-rays and gamma rays, alpha rays, and charged particle radiation such as ion beams. Specifically, as the ionizing radiation curable resin, it is possible to appropriately select and use from among conventional polymerizable monomers, polymerizable oligomers, and prepolymers.

[0119] As polymerizable monomers, (meth)acrylate monomers having free radical polymerizable unsaturated groups in the molecule are preferred, wherein multifunctional (meth)acrylate monomers are preferred. As multifunctional (meth)acrylate monomers, as long as they are (meth)acrylate monomers having two or more ethylenically unsaturated bonds in the molecule, for example, diethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. can be preferably cited. These (meth)acrylate monomers can be used alone or in combination of two or more.

[0120] Preferred examples of polymerizable oligomers include oligomers having a free radical polymerizable unsaturated group in the molecule, such as (meth)acrylate oligomers such as polyurethane (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, polyester (meth)acrylate oligomers, polyether (meth)acrylate oligomers, and acrylic (meth)acrylate oligomers. These polymerizable oligomers can be used alone or in combination of two or more.

[0121] The curable resin composition may contain a dispersant or the like described below in addition to the curable resin described above.

[0122] In addition, in the curable resin composition, as additives, within the scope of not impairing the purpose of the present invention, ultraviolet absorbers, ultraviolet shielding agents, light stabilizers, wear resistance improvers, polymerization inhibitors, crosslinking agents, infrared absorbers, antistatic agents, adhesion improvers, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, defoamers, fillers, anti-blocking agents, lubricants, solvents, etc. can be added. Among them, in order to improve weather resistance, weathering agents such as ultraviolet absorbers and light stabilizers are preferably contained.

[0123] Examples of the ultraviolet absorber include benzophenone-based, benzotriazole-based, triazine-based, salicylate-based, and acrylonitrile-based agents, and examples of the light stabilizer include hindered amine-based, acrylate-based, oxalamide-based, and cyanoacrylate-based agents.

[0124] The surface protection layer can contain a dispersant.

[0125] Examples of the dispersant include the above-mentioned materials that can form nanoshells, polymer surfactants, fatty acid metal salts, silane coupling agents, titanate coupling agents, silicone oils, waxes, modified resins, etc. These dispersants can be used alone or in combination of two or more.

[0126] In addition, as the dispersant, a dispersant encapsulated in a nanoshell may also be used. The nanoshell in the dispersant encapsulated in the nanoshell may be the same nanoshell as the crystal nucleating agent encapsulated in the nanoshell in the second olefin resin layer, and the preparation method thereof is also the same as the preparation method of the crystal nucleating agent encapsulated in the nanoshell.

[0127] By including a dispersant encapsulated in a nanoshell and inorganic fine particles described later, the indentation hardness can be easily increased.

[0128] As an example of a method for preparing a dispersant encapsulated in a nanoshell, a case where methacryloxypropyltrimethoxysilane is used as a dispersant is given as an example and described in more detail.

[0129] 100 parts by mass of an organic solvent such as methanol, 40 to 80 parts by mass of methacryloxypropyltrimethoxysilane as a dispersant, and 2 to 10 parts by mass of phosphatidylcholine as a phospholipid are added to a container maintained at 40 to 70°C and sealed, and carbon dioxide is provided in the container so that the internal pressure reaches 7.5 to 25 MPa to form a supercritical state. Next, the container is stirred at a high speed of about 1000 to 2500 rpm, and 50 to 150 parts by mass of ion exchange water are provided. While maintaining the temperature and pressure in a supercritical state, stirring is continued for about 10 to 25 minutes, and then carbon dioxide is discharged from the container to restore the atmospheric pressure in the container, thereby making it possible to prepare a nanoshell enclosed in a single-layer membrane composed of phospholipids and a dispersant (methacryloxypropyltrimethoxysilane).

[0130] The average primary particle size of the dispersant encapsulated in the nanoshell obtained in this way is the same as the average primary particle size of the dispersant encapsulated in the nanoshell described above, preferably less than 380 nm, more specifically, preferably 1 nm or more and less than 380 nm, more preferably 1 to 375 nm, further preferably 5 to 300 nm, further preferably 10 to 250 nm, particularly preferably 15 to 200 nm,

[0131] The content of the dispersant is preferably 0.01 to 30 parts by mass, more preferably 0.05 to 15 parts by mass, further preferably 0.1 to 10 parts by mass, and particularly preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the resin component forming the surface protection layer.

[0132] From the viewpoint of further improving the scratch resistance, the surface protection layer preferably contains inorganic fine particles. Examples of the inorganic fine particles include silicon dioxide, aluminum oxide, aluminum silicate, kaolin, calcium carbonate, barium sulfate, and glass.

[0133] The average particle size of the inorganic fine particles is not limited, but is preferably 20 μm or less, more preferably 1 to 20 μm, and more preferably 2 to 15 μm.

[0134] The average particle size of inorganic fine particles is the 50% particle size (d50: median diameter) when the particle size distribution is expressed as volume cumulative distribution by measuring the particles in the solution by dynamic light scattering. The 50% particle size can be measured using, for example, Microtrac particle size analyzer (manufactured by Nikkiso Co., Ltd.).

[0135] The content of the inorganic fine particles is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 5 to 20 parts by mass, based on 100 parts by mass of the resin component forming the surface protection layer.

[0136] The thickness of the surface protection layer is preferably 3 to 45 μm, more preferably 5 to 35 μm, and further preferably 10 to 30 μm. When the thickness of the surface protection layer is within the above range, excellent surface properties can be obtained in combination with the first olefin resin layer and the second olefin resin layer.

[0137] (Other layers)

[0138] The decorative sheet of the present invention may further include, for example, a decorative layer, a base layer, an adhesive layer, etc., depending on the application, in addition to the first olefin resin layer, the second olefin resin layer, and the surface protective layer.

[0139] (Decorative layer)

[0140] From the viewpoint of improving the design, the decorative sheet of the present invention may have a decorative layer. The decorative layer may be provided, for example, between the first olefin resin layer and the second olefin resin layer, between the second olefin resin layer and the surface protection layer, or on the surface protection layer.

[0141] The decorative layer may be, for example, a coloring layer covering the entire surface (so-called full-surface coloring layer), a pattern layer formed by printing various patterns using ink and a printer, or a layer formed by combining these. In addition, the decorative layer may be provided at multiple locations within the same layer, or may be provided not only in one layer but in multiple layers.

[0142] For example, when the base color of the decorative board substrate is to be colored and shielded, the coloring and shielding can be achieved by forming a whole-surface colored layer, and the appearance design is improved. In addition, from the perspective of improving the appearance design, the whole-surface colored layer and the pattern layer can be combined, and when the base pattern of the decorative board substrate is to be generated, the whole-surface colored layer can be not provided but only the pattern layer can be provided.

[0143] The ink used for the decorative layer may be a binder appropriately mixed with a colorant such as a pigment or dye, an extender pigment, a solvent, a stabilizer, a plasticizer, a catalyst, a curing agent, an ultraviolet absorber, a light stabilizer, and the like.

[0144] The binder is not particularly limited, and preferably includes polyurethane resins, acrylic polyol resins, acrylic resins, ester resins, amide resins, butyral resins, styrene resins, polyurethane-acrylic copolymers, polycarbonate-based polyurethane-acrylic copolymers (the polyurethane-acrylic copolymers are derived from polymers having carbonate bonds in the polymer main chain and having two or more hydroxyl groups at the terminal and side chains (polycarbonate polyols)), vinyl chloride-vinyl acetate copolymer resins, vinyl chloride-vinyl acetate-acrylic copolymer resins, chlorinated propylene resins, nitrocellulose resins, cellulose acetate resins, and the like. These binders can be used alone or in combination of a plurality of types.

[0145] As a colorant, from the viewpoint of coloring and masking the base color of the decorative board substrate and improving the appearance design, for example, inorganic pigments such as white pigment, iron black, chrome yellow, titanium yellow, iron red, cadmium red, ultramarine, cobalt blue, etc.; organic pigments or dyes such as quinacridone red, isoindolinone yellow, phthalocyanine blue, etc.; metallic pigments composed of flaky foils of aluminum, brass, etc.; pearl pigments composed of flaky foils of titanium dioxide coated mica, basic lead carbonate, etc., etc.

[0146] When the decorative layer has a pattern layer, its pattern includes wood grain pattern, wood grain pattern on the surface of rock imitating marble pattern (e.g., travertine marble pattern), cloth pattern or cloth texture pattern imitating cloth-like pattern, tile pattern, brick pattern, etc., and there are also patterns of inlay wood, patchwork, etc. These patterns are formed by multi-color printing using common process colors of yellow, red, blue and black, and can also be formed by special multi-color printing using plates of each color constituting the pattern.

[0147] The thickness of the decorative layer may be appropriately selected depending on the desired pattern, and is preferably 0.5 to 20 μm, more preferably 1 to 10 μm, and even more preferably 2 to 5 μm from the viewpoint of coloring and hiding the base color of the decorative plate substrate and improving the design.

[0148] (basal layer)

[0149] The base layer is a layer mainly for improving the adhesion of each layer.

[0150] In the decorative sheet of the present invention, the base layer can be provided, for example, on one or both surfaces of the first olefin resin layer, one or both surfaces of the second olefin resin layer, etc. In addition, similarly to the base layer, in order to improve the adhesion of each layer, a physical surface treatment such as oxidation or embossing, or a surface treatment such as chemical surface treatment can be applied to one or both surfaces of the first olefin resin layer or the second olefin resin layer.

[0151] The base layer can be formed, for example, from a resin composition obtained by appropriately mixing a solvent, a stabilizer, a plasticizer, a catalyst, a curing agent, a UV absorber, a light stabilizer, and the like with the adhesive exemplified as the adhesive that can be used for the decorative layer.

[0152] From the viewpoint of improving adhesion, the thickness of the base layer is preferably 0.2 to 10 μm, more preferably 0.5 to 8 μm, and even more preferably 1 to 5 μm.

[0153] (Synthetic resin back layer)

[0154] The decorative sheet of the present invention may have a synthetic resin backing layer on the bottom layer of the decorative sheet, that is, on the first olefin resin layer side of the decorative sheet. By having a synthetic resin backing layer, the impact resistance of the decorative material is further improved.

[0155] As the resin constituting the synthetic resin back layer, for example, polypropylene, ethylene-vinyl alcohol copolymer, polymethylene, polymethylpentene, polyethylene terephthalate, heat-resistant polyalkylene terephthalate (for example, polyethylene terephthalate in which a part of ethylene glycol is substituted with 1,4-cyclohexanedimethanol, diethylene glycol, etc., so-called trade name PET-G (Eastman Chemical Company system)), polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, polycarbonate, polyacrylate, polyimide, polystyrene, polyamide, ABS, etc. can be listed. These resins can be used alone or in two or more kinds.

[0156] The thickness of the synthetic resin back layer is preferably 0.1 to 0.6 mm, more preferably 0.15 to 0.45 mm, and further preferably 0.20 to 0.40 mm. By setting the lower limit of the thickness of the synthetic resin back layer within the above range, the impact resistance of the decorative sheet is further improved. In addition, by setting the upper limit of the thickness of the synthetic resin back layer within the above range, the warping of the decorative sheet is further suppressed.

[0157] (concave part)

[0158] The decorative sheet of the present invention may have recessed portions (for example, embossed recessed portions) on the surface protection layer side. The recessed portions can provide a high-quality feel with improved texture (touch) of the decorative sheet, thereby improving the designability of the exterior.

[0159] The recessed portion may be present at least in the surface protective layer of the decorative sheet of the present invention, and the depth of the recessed portion may be limited to the surface protective layer or may be formed to reach the first olefin resin layer. From the viewpoint of obtaining an excellent texture (touch), it is preferred that the recessed portion not only be limited to the surface protective layer but also be formed to reach the second olefin resin layer and the first olefin resin layer in combination.

[0160] As the pattern of the recessed part, for example, there are wood grain conduit grooves, slate surface bumps, cloth surface texture, pear grain, sand grain, brushed, and line grooves. From the viewpoint of improving the appearance design, the pattern of the recessed part is preferably a pattern that is in tune with the pattern of the decorative layer. For example, when the pattern layer is a wood grain pattern, the wood grain plate conduit groove is selected as the pattern of the recessed part, and the wood grain of the pattern layer and the wood grain of the recessed part are coordinated, so that a more realistic and textured, high-grade decorative sheet can be obtained.

[0161] (Method for producing decorative sheet)

[0162] An example of the method for producing the decorative sheet of the present invention will be described by taking as an example a decorative sheet which is one of the preferred aspects of the decorative sheet of the present invention and has a first olefin resin layer, a decorative layer, a second olefin resin layer and a surface protection layer in this order in the thickness direction.

[0163] First, a resin composition for forming a first olefin resin layer is prepared, and the first olefin resin layer is formed into a film by a method such as a melt extrusion method, and a decorative layer is formed on the first olefin resin layer.

[0164] In addition, a resin composition for forming a second olefin resin layer is separately prepared, and the second olefin resin layer is formed into a film by a method such as a melt extrusion method. An uncured layer formed by coating a curable resin composition on the second olefin resin layer is irradiated with heat or ionizing radiation to cure it, thereby forming a surface protective layer.

[0165] Next, an adhesive is applied to at least one surface of the decorative layer and the second olefin resin layer, and the decorative layer and the second olefin resin layer are bonded together so that the decorative layer and the second olefin resin layer face each other, thereby manufacturing a decorative sheet having the first olefin resin layer, the decorative layer, the second olefin resin layer, and the surface protection layer in this order.

[0166] In addition, in the above-mentioned manufacturing method, after forming the decorative layer, the resin composition for forming the second olefin resin layer is used to bond and press-bond the second olefin resin layer via an adhesive and / or a thermoplastic resin such as an acid-modified polyolefin resin and stack them by extrusion lamination, dry lamination, wet lamination, heat lamination, etc., and then, on the second olefin resin layer, the uncured layer formed by coating the curable resin composition is irradiated with heat or ionizing radiation to cure it to form a surface protective layer. Thus, a decorative sheet having a first olefin resin layer, a decorative layer, a second olefin resin layer and a surface protective layer in sequence can be formed.

[0167] The decorative layer can be formed by coating the first olefin resin layer and the second olefin resin layer with ink for forming the decorative layer and providing a desired coloring layer and pattern layer. The ink is applied by a known method such as gravure printing, bar coating, roller coating, reverse roller coating, comma coating, etc., preferably by gravure printing.

[0168] In forming the surface protective layer, the curable resin composition is preferably applied by a known method such as gravure printing, bar coating, roll coating, reverse roll coating, comma coating, etc. so that the thickness after curing becomes a predetermined thickness, and is preferably applied by gravure printing.

[0169] When an ionizing radiation resin composition is used in the formation of the surface protection layer, the uncured resin layer formed by the coating of the resin composition is irradiated with ionizing radiation such as electron beams, ultraviolet rays to form a cured product to form a surface protection layer. Here, when electron beams are used as ionizing radiation, the acceleration voltage thereof can be appropriately selected according to the resin used and the thickness of the layer, and it is usually preferred to cure the uncured resin layer at an acceleration voltage of about 70 to 300 kV.

[0170] The irradiation dose is preferably a dose at which the crosslinking density of the ionizing radiation curable resin is saturated, and is usually selected from the range of 5 to 300 kGy (0.5 to 30 Mrad), preferably 10 to 50 kGy (1 to 5 Mrad).

[0171] The electron beam source is not particularly limited, and various electron beam accelerators such as Cockcroft-Walton type, Van der Graaf type, resonance transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type can be used.

[0172] When ultraviolet rays are used as ionizing rays, ionizing rays including ultraviolet rays with a wavelength of 190 to 380 nm are radiated. There are no particular limitations on the ultraviolet source, and for example, a high-pressure mercury lamp, a low-pressure mercury lamp, a metal halide lamp, a carbon arc lamp, etc. can be used.

[0173] When a thermosetting resin composition is used for forming the surface protection layer, the surface protection layer may be formed by subjecting the resin composition to heat treatment and curing.

[0174] When providing the undercoat layer, the resin composition for forming the undercoat layer can be applied by a known method such as gravure printing, bar coating, roll coating, reverse roll coating, or comma coating.

[0175] When a synthetic resin backing layer is provided, it can be formed by a known method such as laminating a synthetic resin backing layer produced by T-die extrusion or the like and the first olefin resin layer by heat lamination or heat lamination via an adhesive.

[0176] When forming the recessed portion, embossing is preferably used in consideration of ease of operation. The embossing may be performed by a common method using a known blade or rotary embossing machine.

[0177] 2. Decorative panels

[0178] The decorative board of the present invention is composed of a laminate having a decorative board base material and the decorative sheet of the present invention in this order in the thickness direction.

[0179] Figure 31 and 2 show an example of a decorative plate 12 in which the decorative sheet 10 of the present invention is sequentially laminated on a decorative plate base 11 (the surface opposite to the surface protection layer side and the decorative plate base 11 are bonded together).

[0180] The decorative board substrate is not particularly limited, and for example, at least one of medium-density wood fiberboard, high-density wood fiberboard, particleboard, conifer plywood, broadleaf plywood, fast-growing tree plywood, cork sheets, composite substrates containing cork, thermoplastic resin boards (resin boards with polyvinyl chloride resin, polypropylene resin, polyethylene resin, acrylic resin, ABS resin, etc. as main components, or resin boards obtained by foaming these), etc. can be listed. These decorative board substrates can be used alone or in combination of two or more and laminated.

[0181] Here, as conifers, for example, basswood, tamarisk, spruce, fir, cypress, pine, redwood, spruce, etc. can be cited. As broad-leaved trees, for example, willow, basswood, birch, cork, beech, oak, sauerkraut, etc. can be cited. In addition, as fast-growing trees, poplar, Malacca, albizzia, eucalyptus, eucalyptus, terminalia, etc. can be cited.

[0182] When using a wood plywood such as a conifer plywood, a broadleaf plywood, or a fast-growing tree plywood, the number of layers of the wood veneer is not limited, and is usually preferably 3 to 7, and more preferably 5 to 7. In addition, the adhesive used when making the wood plywood is also not limited, and a wide range of known woodworking adhesives can be used.

[0183] As adhesives, for example, adhesives containing polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ionomers, butadiene-acrylonitrile rubber, chloroprene rubber, natural rubber, etc. as active ingredients can be cited. In addition, as thermosetting adhesives, adhesives of melamine series, phenolic series, urea series (vinyl acetate-urea series, etc.) and the like can also be cited.

[0184] The thickness of the decorative plate substrate is not particularly limited, but is preferably about 2 to 15 mm, more preferably about 2 to 12 mm.

[0185] The lamination method of the laminated decorative sheet and the decorative board substrate is not particularly limited, for example, a method of laminating each with an adhesive can be adopted. The adhesive can be appropriately selected from known adhesives according to the type of the decorative board substrate. For example, reactive hot melt adhesives such as polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ionomer, polyurethane-based reactive hot melt adhesive (hereinafter referred to as "PUR-based adhesive"), butadiene-acrylonitrile rubber, chloroprene rubber, natural rubber, etc. can be listed. These adhesives can be used alone or in combination of two or more.

[0186] The decorative sheet of the present invention described above has both excellent bending workability and scratch resistance even under high load conditions, and is useful as a decorative material.

[0187] Example

[0188] Next, the present invention will be described in further detail using examples, but the present invention is not limited to these examples.

[0189] The properties and characteristics of the decorative sheets obtained in each example were evaluated by the following measuring methods.

[0190] <Evaluation Method>

[0191] (1) Indentation hardness (H IT )

[0192] According to the method described in the manual, the indentation hardness H of the surface protective layer was measured. IT 1 , the indentation hardness H of the second olefin resin layer IT 2 and the indentation hardness H of the first olefin resin layer IT 3 .

[0193] (2) Scratch resistance test (coin scratch test)

[0194] The decorative sheets prepared in Examples and Comparative Examples were bonded to a 2.5 mm thick medium density fiberboard (MDF; decorative board substrate) via a water-soluble emulsion adhesive to prepare decorative boards. The following materials were used as the water-soluble emulsion adhesive.

[0195] Water-soluble emulsion adhesive

[0196] Main agent: "BA-10L" manufactured by Japan Coating Resin Co., Ltd., modified ethylene-vinyl acetate

[0197] Curing agent: "BA-11B" manufactured by Japan Coating Resin Co., Ltd., isocyanate-based

[0198] Mixing ratio: main agent: curing agent = 100: 2.5 (mass ratio)

[0199] The scratch resistance of the decorative sheet was evaluated by a coin scratch test. Specifically, two 10-yen coins tilted at 45° were placed in contact with the surface (surface protection layer side) of the test piece decorative sheet, and a load (4 kg load, 6 kg load, and 7 kg load) was applied while pulling in the horizontal direction to evaluate the scratch state at this time. The evaluation criteria are as follows, and all B ratings or above (i.e. A or B) are qualified.

[0200] <Judgment Criteria>

[0201] A: No damage was confirmed under a load of 7kg

[0202] B: Damage was confirmed under a load of 7 kg, but no damage was confirmed under a load of 6 kg

[0203] C: No damage was found under a load of 4 kg, but damage was found under a load of 6 kg

[0204] (3) Bending workability

[0205] The bending workability of the decorative sheets produced in Examples and Comparative Examples was evaluated. Specifically, the decorative sheets were wound so that the first olefin layer was in contact with a metal bar having a diameter of 3 mm, and the presence or absence of cracks in the surface protective layer was evaluated. The evaluation criteria are as follows.

[0206] <Judgment Criteria>

[0207] A: No cracks were detected

[0208] B: Minor cracks can be observed when carefully and carefully observed, but there is no problem with performance.

[0209] C: Cracks are clearly visible

[0210] (4) Impact resistance (DuPont impact test)

[0211] The impact resistance of the decorative sheets prepared in the examples and comparative examples was evaluated using a DuPont impact tester (according to JIS K5600-5-3). Specifically, a weight of a specified weight was dropped from a height of 100 mm onto the decorative sheet surface of the decorative board to evaluate whether cracks occurred in the decorative sheet. The evaluation criteria are as follows.

[0212] A: No rupture was detected

[0213] B: When you look closely and carefully, you can see a tiny crack.

[0214] C: Clearly identified rupture

[0215] (5)Pollution resistance after DuPont impact test

[0216] The decorative sheets prepared in Examples and Comparative Examples were evaluated for stain resistance by the following method.

[0217] An oil-based black marker (manufactured by Teranishi Chemical Industry Co., Ltd.) was applied to the test implementation portion of (4), and then immediately wiped off with a solvent (ethanol), and the degree of black marker remaining after wiping was visually observed for evaluation. The evaluation criteria are as follows.

[0218] A: No contamination residue was detected

[0219] B: When you pay attention and observe carefully, you can confirm that there is a small amount of contamination left.

[0220] C: Clearly identified pollution

[0221] Example 1

[0222] A decorative sheet 10 is produced in which the first olefin resin layer 3, the second olefin resin layer 2 and the surface protection layer 1 are laminated in this order.

[0223] First, the first olefin resin layer 3 composed of a polyethylene sheet having a thickness of 80 μm and the second olefin resin layer 2 obtained by the following production method were laminated with an adhesive layer interposed therebetween.

[0224] Next, a surface protection layer coating liquid A having the following composition was applied on the second olefin resin layer 2 by roll coating so that the thickness after drying would be 15 μm.

[0225] Next, in an environment with an oxygen concentration of 200 ppm or less, an electron beam irradiation device was used to irradiate the surface with electron beams under the conditions of an acceleration voltage of 175 keV and 5 Mrad to form a surface protection layer 1 for curing.

[0226] Next, embossing was performed by hot pressing from the surface protection layer 1 side to form a concave-convex pattern of a wood grain duct pattern, thereby producing a decorative sheet of Example 1.

[0227] <Method for producing the second olefin resin layer 2>

[0228] 1000 ppm of sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphonate as a crystal nucleating agent was added to a highly crystalline homopolypropylene resin having an isotactic pentad fraction of 97.8%, an MFR of 15 g / 10 min (230° C.), and a molecular weight distribution (Mw / Mn) of 2.3, and then extruded using a melt extruder to obtain a polypropylene sheet consisting of microcrystalline homopolypropylene having a thickness of 80 μm.

[0229] <Surface protection layer coating liquid A>

[0230] 80 parts by weight of bifunctional polyurethane acrylate oligomer

[0231] (Polyol component is polyester diol, glass transition temperature: 25°C, molecular weight 1500)

[0232] 20 parts by weight of 6-functional aliphatic polyurethane acrylate oligomer

[0233] (Glass transition temperature: 200°C or higher, molecular weight: 1500, UA306H manufactured by Kyoeisha Chemical Co., Ltd.)

[0234] · Inorganic fine particles 14 parts by mass

[0235] (Silicon dioxide particles with an average particle size of 10 μm)

[0236] Implementation Example 2

[0237] A decorative sheet of Example 2 was prepared in the same manner as in Example 1 except that the amount of the hexafunctional aliphatic urethane acrylate oligomer in the surface protective layer coating liquid A was changed to 100 parts by mass and the bifunctional urethane acrylate oligomer was not added.

[0238] Example 3

[0239] A decorative sheet of Example 3 was prepared in the same manner as in Example 1 except that the amount of the bifunctional urethane acrylate oligomer in the surface protection layer coating liquid A was changed to 20 parts by mass and the amount of the hexafunctional aliphatic urethane acrylate oligomer was changed to 80 parts by mass.

[0240] Example 4

[0241] A decorative sheet of Example 4 was prepared in the same manner as in Example 1 except that the amount of the crystal nucleating agent added was changed to 2000 ppm as in Example 1.

[0242] Example 5

[0243] A decorative sheet of Example 5 was prepared in the same manner as in Example 1 except that the amount of the bifunctional urethane acrylate oligomer in the surface protective layer coating liquid A was changed to 20 parts by mass, the amount of the hexafunctional aliphatic urethane acrylate oligomer was changed to 80 parts by mass, and the amount of the crystal nucleating agent added was changed to 2000 ppm.

[0244] Comparative Example 1

[0245] A decorative sheet of Comparative Example 1 was prepared in the same manner as in Example 1 except that a polypropylene sheet extruded by a melt extruder was used without adding 1000 ppm of sodium 2,2′-methylenebis(4,6-di-tert-butylphenyl)phosphonate as a crystal nucleating agent.

[0246] Comparative Example 2

[0247] A decorative sheet of Comparative Example 2 was prepared in the same manner as in Example 3 except that a polypropylene sheet extruded by a melt extruder was used without adding 1000 ppm of sodium 2,2′-methylenebis(4,6-di-tert-butylphenyl)phosphonate as a crystal nucleating agent.

[0248] [Table 1]

[0249]

[0250] (In Table 1, the unit of indentation hardness is MPa. IT 1 , H IT 2 , H IT 3 Respectively represent the indentation hardness of the surface protection layer, the second olefin resin layer and the first olefin resin layer.)

[0251] The results in Table 1 confirm that the decorative sheets of Examples 1 to 5 have excellent scratch resistance under high load conditions and excellent bending workability. In addition, by comparing Examples 1 to 3 with Examples 4 to 5, it is confirmed that by increasing the indentation hardness H of the second olefin resin layer 2 IT 2 By setting the pressure to 100 MPa or more and less than 140 MPa (preferably 130 MPa or less), in addition to excellent scratch resistance and bending workability, excellent effects are obtained in DuPont impact resistance and stain resistance after DuPont impact.

[0252] Industrial Applicability

[0253] The decorative sheet of the present invention has excellent scratch resistance under high load conditions and excellent bending workability, and can be used as a surface material of building materials, especially a floor decorative material.

Claims

1. A decorative sheet, characterized in that: The invention has a first olefin resin layer, a second olefin resin layer and a surface protection layer in this order, and has a concave portion from the front side of the surface protection layer, The thickness of the surface protection layer is 10 to 30 μm, and the surface protection layer contains inorganic particles with an average particle size of 10 to 20 μm. The indentation hardness H of the second olefin resin layer IT 2 The indentation hardness of the surface protective layer H IT 1 Satisfies the following equations (1), (2) and (3): H IT 2 ≥105MPa (1); H IT 1 >H IT 2 (2); 450MPa>H IT 1 (3), The indentation hardness refers to nanoindentation hardness measured using a surface film property testing machine TI-950 (registered trademark: Triboindenter, manufactured by HYSITRON Corporation).

2. The decorative sheet according to claim 1, characterized in that: The indentation hardness H of the second olefin resin layer IT 2 The indentation hardness H of the first olefin resin layer IT 3 Satisfies the following formula (4): H IT 2 >H IT 3 (4)。 3. The decorative sheet according to claim 1 or 2, characterized in that: The second olefin resin layer is a microcrystallized olefin resin layer.

4. A decorative board, characterized in that: The invention comprises a laminated body including a decorative plate base material and the decorative sheet according to any one of claims 1 to 3 in this order in the thickness direction.

Citation Information

Patent Citations

  • Decoration piece

    CN101396948A

  • Decorative sheet and decorative plate using same

    CN106132706A

  • Decorated sheet

    WO2016076360A1