Preparation method of magnesium oxide sealing cavity and optical sensor

Through wet etching and direct bonding technology of magnesium oxide wafers, the problem of sensors not being able to work in extreme high temperature and high pressure environments is solved, the sealing performance and bonding strength are improved, and it is suitable for sensor applications under high temperature and high pressure conditions.

CN119018842APending Publication Date: 2024-11-26ZHONGBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411116070.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2019-10-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing sensors cannot work effectively in extreme high temperature and high pressure environments, and there is a lack of preparation methods to adapt to this environment.

Method used

Wet etching and direct bonding technology of magnesium oxide wafers are used to form a sealing body to improve sealing performance by forming a cavity with a predetermined depth and a surface-treated bonding surface, and strengthening bonding through pre-bonding and annealing. strength.

Benefits of technology

It realizes the reliability and sealing performance of sensors in high temperature and high pressure environments, and is suitable for applications under high temperature and high pressure conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018842A_ABST
    Figure CN119018842A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a magnesium oxide sealing cavity and an optical sensor, the magnesium oxide sealing cavity is applied to the sensor based on the optical principle, and the preparation method comprises the following steps: forming a mask layer on the surface of a first magnesium oxide wafer; photoetching the mask layer of the first magnesium oxide wafer to form a predetermined pattern; performing wet etching on the first magnesium oxide wafer by using a phosphoric acid solution so as to form a cavity with a preset depth on the first magnesium oxide wafer, and removing the mask layer; the first bonding surface of the first magnesium oxide wafer and the second bonding surface of the second magnesium oxide wafer are directly bonded to form a sealing body composed of the first magnesium oxide wafer and the second magnesium oxide wafer, and the first bonding surface is the surface, with the cavity, of the first magnesium oxide wafer. Therefore, the sealing performance of the sealing body can be improved, and the sealing body can well adapt to a high-temperature and high-pressure working environment by utilizing excellent mechanical properties and dynamic characteristics of magnesium oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with an application date of October 29, 2019, application number 2019110398520, and invention name: Method for preparing a magnesium oxide sealed chamber. Technical Field

[0002] The present disclosure generally relates to the field of core electronic industries, and more particularly to a method for preparing a magnesium oxide sealed cavity and an optical sensor. Background Art

[0003] At present, the combustion chamber temperature of scramjet engines is generally around 2000°C, the combustion chamber temperature of aircraft engines exceeds 1700°C, the maximum surface temperature of high-speed aircraft exceeds 1500°C during supersonic flight, and the combustion temperature of gas turbines is generally above 1350°C. In these extreme high temperature and high pressure environments, the performance requirements for sensors are also very strict. Among them, the decisive factors that determine the reliability of sensors include the manufacturing materials and manufacturing methods of sensors.

[0004] Existing sensors or sensor chips are often made by processing and treating materials such as silicon wafers. These sensors are generally made using traditional processes and are usually unable to withstand the extreme environmental conditions of high temperature and high pressure as described above. In addition, there is no preparation method for sensors that can adapt to such high temperature and high pressure environments in the prior art. Summary of the invention

[0005] The present disclosure is proposed in view of the above-mentioned state of the prior art, and in view of the excellent mechanical properties and dynamic characteristics of high-melting-point magnesium oxide in high-temperature environments. A processing technology for magnesium oxide wafers is developed, and its purpose is to provide a method for preparing a magnesium oxide sealed cavity that can be used in sensors working at high temperature and high pressure.

[0006] To this end, the first aspect of the present disclosure provides a method for preparing a magnesium oxide sealed cavity, which includes: a preparation process, preparing a first magnesium oxide wafer and a second magnesium oxide wafer, and forming a mask layer on the surface of the first magnesium oxide wafer; a patterning process, photolithography the mask layer of the first magnesium oxide wafer to form a predetermined pattern; an etching process, wet etching the first magnesium oxide wafer using a phosphoric acid solution to form a cavity of a predetermined depth in the first magnesium oxide wafer, and removing the mask layer; and a bonding process, surface treatment of a side of the etched first magnesium oxide wafer with the cavity to form a cavity with a first A first bonding surface with a predetermined roughness and a first hydrophilicity is formed, one side of the second magnesium oxide wafer is surface treated to form a second bonding surface with a second predetermined roughness and a second hydrophilicity, and the first bonding surface of the first magnesium oxide wafer is directly bonded to the second bonding surface of the second magnesium oxide wafer to form a sealed body composed of the first magnesium oxide wafer and the second magnesium oxide wafer, wherein in the bonding, the first bonding surface of the first magnesium oxide wafer is directly pre-bonded to the second bonding surface of the second magnesium oxide wafer, and the pre-bonded first magnesium oxide wafer and the second magnesium oxide wafer are annealed.

[0007] In this case, a first magnesium oxide wafer having a cavity of a predetermined depth can be made by a wet etching process, and a first bonding surface of the first magnesium oxide wafer having a first predetermined roughness and a first hydrophilicity and a second bonding surface of the second magnesium oxide wafer having a second predetermined roughness and a second hydrophilicity are bonded by a bonding process to form a sealing body. Thus, the sealing performance of the sealing body can be improved, and the sensor made by the excellent mechanical properties and dynamic characteristics of magnesium oxide can be well adapted to the working environment under high temperature and high pressure.

[0008] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the sealing body has a plurality of sealed cavities, thereby enabling the magnesium oxide sealed cavities to be mass-produced.

[0009] In addition, in the preparation method of the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, a pre-cutting process is further included, wherein the pre-cutting process is used to cut the sealed body into a plurality of chips by mechanical cutting or laser cutting, and each chip has a sealed cavity. Thus, the magnesium oxide sealed cavity can be mass-produced by mechanical cutting or laser cutting.

[0010] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, in the pre-bonding, the first magnesium oxide wafer and the second magnesium oxide wafer are pressurized, and the pre-bonded first magnesium oxide wafer and the second magnesium oxide wafer are preheated at 100 to 400° C. for 10 to 60 minutes, and then raised to 1200° C. at a rate of 10° C. per minute, and maintained for 60 to 240 minutes. Thus, the bonding strength between the first magnesium oxide wafer and the second magnesium oxide wafer can be enhanced.

[0011] In addition, in the preparation method of the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, in the bonding process, the side of the first magnesium oxide wafer with the cavity after etching is subjected to oxygen plasma activation treatment, and then the surface is treated with a wet activation solution to form the first bonding surface having the first predetermined roughness and the first hydrophilicity, and the side of the second magnesium oxide wafer is subjected to the oxygen plasma activation treatment, and then the surface is treated with the wet activation solution to form the second bonding surface having the second predetermined roughness and the second hydrophilicity. Thus, through oxygen plasma activation treatment and surface treatment, the first bonding surface and the second bonding surface can have the surface roughness and hydrophilicity that meet the requirements, and the first magnesium oxide wafer and the second magnesium oxide wafer can be better bonded.

[0012] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the first bonding surface is a hydroxyl layer, and the second bonding surface is a hydroxyl layer, thereby enhancing the hydrophilicity of the first bonding surface and the second bonding surface.

[0013] In addition, in the method for preparing the magnesium oxide sealed chamber according to the first aspect of the present disclosure, the first magnesium oxide wafer and the second magnesium oxide wafer are optionally aligned and stacked, and pre-bonded, thereby enabling the first magnesium oxide wafer and the second magnesium oxide wafer to be bonded more effectively.

[0014] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the material of the mask layer is one of silicon dioxide, silicon nitride, chromium, and gold. Thus, the material of the mask layer can be reasonably selected according to the situation.

[0015] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the concentration of the phosphoric acid solution is 25% to 85%, and the temperature of the wet etching is 20° C. to 120° C. Thus, the etched cavity and sidewall can meet the etching requirements.

[0016] In addition, in the method for preparing the magnesium oxide sealed cavity of the first aspect of the present disclosure, optionally, the concentration of the phosphoric acid solution is 50% to 85%. Thus, by selecting a phosphoric acid solution of appropriate concentration, the etched cavity and sidewall can further meet the etching requirements.

[0017] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the first predetermined roughness is less than 1 nm, and the second predetermined roughness is less than 1 nm, thereby enabling the first bonding surface and the second bonding surface to achieve a tighter bonding.

[0018] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the first magnesium oxide wafer and the second magnesium oxide wafer are single crystal wafers. Thus, the more stable properties of single crystal magnesium oxide can make the sealed body composed of the first magnesium oxide wafer and the second magnesium oxide wafer have more stable performance.

[0019] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the water contact angle of the first bonding surface is less than 5°, and the water contact angle of the second bonding surface is less than 5°. Thus, the first bonding surface and the second bonding surface can have better hydrophilicity.

[0020] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the wet activation solution comprises ammonium hydroxide, hydrogen peroxide and water, and the ratio of ammonium hydroxide, hydrogen peroxide and water is 1:1:5. Thus, the first bonding surface and the second bonding surface can have more suitable surface roughness and hydrophilicity.

[0021] In addition, in the method for preparing the magnesium oxide sealed chamber involved in the first aspect of the present disclosure, optionally, the sealed chamber is a cylinder, thereby enhancing the working performance of the magnesium oxide sealed chamber.

[0022] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, the bottom diameter of the cylinder is 2-8 mm, and the height of the cylinder is 10-100 μm. Thus, a sealed cavity that meets the requirements can be obtained.

[0023] In addition, in the method for preparing the magnesium oxide sealed cavity involved in the first aspect of the present disclosure, optionally, a third magnesium oxide wafer having a through hole is further included, and the third magnesium oxide wafer is bonded to the second magnesium oxide wafer and the first magnesium oxide wafer simultaneously. In this case,

[0024] A second aspect of the present disclosure provides a temperature-pressure integrated sensor, which uses the method for preparing the magnesium oxide sealed cavity described in any one of the first aspects of the present disclosure.

[0025] In this case, the manufactured magnesium oxide sealed cavity can be applied to the temperature-pressure integrated sensor, so that the temperature-pressure integrated sensor can be used to measure both temperature and pressure.

[0026] In the present disclosure, a first magnesium oxide wafer having a cavity of a predetermined depth can be made through a wet etching process, and a first bonding surface of the first magnesium oxide wafer having a first predetermined roughness and a first hydrophilicity and a second bonding surface of a second magnesium oxide wafer having a second predetermined roughness and a second hydrophilicity are bonded through a bonding process to form a sealing body. Thus, the sealing performance of the sealing body can be improved, and the sensor made by utilizing the excellent mechanical properties and dynamic characteristics of magnesium oxide can be well adapted to the working environment under high temperature and high pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Embodiments of the present disclosure will now be explained in further detail, by way of example only, with reference to the accompanying drawings, in which:

[0028] Figure 1 1 is a flow chart showing a method for preparing a magnesium oxide sealed cavity according to an embodiment of the present disclosure.

[0029] Figure 2 Schematic diagram showing the process flow of wet etching of magnesium oxide wafers involved in an embodiment of the present disclosure.

[0030] Figure 3 1 is a schematic diagram showing a process flow of another embodiment of wet etching of magnesium oxide wafers according to an embodiment of the present disclosure.

[0031] Figure 4 1 is a schematic diagram showing the effect of phosphoric acid solutions of different concentrations on the etching rate of a first magnesium oxide wafer at different temperatures according to an embodiment of the present disclosure.

[0032] Figure 5 1 is a perspective schematic diagram showing bonding of a first magnesium oxide wafer and a second magnesium oxide wafer according to an embodiment of the present disclosure.

[0033] Figure 6 1 is a schematic cross-sectional view showing a first magnesium oxide wafer and a second magnesium oxide wafer after bonding according to an embodiment of the present disclosure.

[0034] Figure 7 It shows the Figure 3 A top view of the first magnesium oxide wafer and the second magnesium oxide wafer after bonding.

[0035] Figure 8 is a schematic diagram showing a sealing test of a sealing body according to an embodiment of the present disclosure.

[0036] Fig. 9 1 is a schematic diagram showing the structure of Example 1 of the magnesium oxide sealed chamber according to the embodiment of the present disclosure.

[0037] Fig.10 1 is a schematic diagram showing the structure of Example 2 of the magnesium oxide sealed chamber according to the embodiment of the present disclosure.

[0038] Fig.11 1 is a schematic diagram showing the structure of Example 3 of the magnesium oxide sealed chamber according to the embodiment of the present disclosure.

[0039] Explanation of symbols:

[0040] P…sealing body, C…chip, 1…first magnesium oxide wafer, 2…mask layer (21…first mask layer, 22…second mask layer), 3…photoresist, 4…second magnesium oxide wafer, 5…sealed cavity, 6…third magnesium oxide wafer, 7…temperature and pressure integrated sensor, 8…wireless passive pressure sensor, 9…non-contact pressure sensor, 10…cavity, 11…first bonding surface, 41…second bonding surface, 61…through hole, 81…first capacitor electrode, 82…second capacitor electrode, 91…lens. DETAILED DESCRIPTION

[0041] Hereinafter, the preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In the following description, the same symbols are assigned to the same components, and repeated descriptions are omitted. In addition, the accompanying drawings are only schematic diagrams, and the ratio of the dimensions of the components or the shapes of the components may be different from the actual ones.

[0042] The present invention relates to a magnesium oxide sealed cavity P (refer to Figure 5 The preparation method of the magnesium oxide sealed cavity P may be referred to as the preparation method, and the magnesium oxide sealed cavity P may be referred to as the sealing body P.

[0043] The preparation method disclosed in the present invention utilizes the processing technology of magnesium oxide wafers to realize the manufacture of the sealing body P. The sealing body P can be applied to the manufacturing fields of optical sensors, temperature sensors and pressure sensors under high temperature and high pressure environments. The preparation method of the magnesium oxide sealed cavity P involved in this embodiment is described in detail below in conjunction with the accompanying drawings.

[0044] Figure 1 1 is a flow chart showing a method for preparing a magnesium oxide sealed cavity P according to an embodiment of the present disclosure.

[0045] In some examples, such as Figure 1As shown, the preparation method of the magnesium oxide sealed cavity P may include: a preparation process, preparing a first magnesium oxide wafer 1 and a second magnesium oxide wafer 4, and forming a mask layer 2 on the surface of the first magnesium oxide wafer 1 (step S100); a patterning process, performing photolithography on the mask layer 2 of the first magnesium oxide wafer 1 to form a predetermined pattern (step S200); an etching process, wet etching the first magnesium oxide wafer 1 using a phosphoric acid solution to form a cavity 10 with a predetermined depth on the first magnesium oxide wafer 1, and removing the mask layer 2 (step S300); and a bonding process, performing surface treatment on the side of the etched first magnesium oxide wafer 1 with the cavity 10 to form a first predetermined pattern. A first bonding surface 11 with a predetermined roughness and a first hydrophilicity is formed, and a surface treatment is performed on one side of the second magnesium oxide wafer 4 to form a second bonding surface 41 with a second predetermined roughness and a second hydrophilicity, and the first bonding surface 11 of the first magnesium oxide wafer 1 is directly bonded with the second bonding surface 41 of the second magnesium oxide wafer 4 to form a sealing body P composed of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 (step S400), wherein, in the bonding, the first bonding surface 11 of the first magnesium oxide wafer 1 and the second bonding surface 41 of the second magnesium oxide wafer 4 are firstly directly pre-bonded, and then the pre-bonded first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 are annealed.

[0046] In the present disclosure, the preparation method of the magnesium oxide sealed cavity P mainly includes the wet chemical etching technology of the magnesium oxide wafer and the direct bonding technology, and specifically involves the graphic processing technology of the magnesium oxide wafer surface and the direct bonding technology of the magnesium oxide wafer. Thus, the first magnesium oxide wafer 1 with a cavity 10 of a predetermined depth can be made through a wet etching process, and the first bonding surface 11 of the first magnesium oxide wafer 1 with a first predetermined roughness and a first hydrophilicity and the second bonding surface 41 of the second magnesium oxide wafer 4 with a second predetermined roughness and a second hydrophilicity are bonded through a bonding process to form a sealing body P. Thus, the sealing performance of the sealing body P can be improved, and the sensor made by using the excellent mechanical properties and dynamic characteristics of magnesium oxide can be well adapted to the working environment under high temperature and high pressure.

[0047] In some examples, before step S100, the first magnesium oxide wafer 1 may be polished. In this case, polishing the first magnesium oxide wafer 1 can reduce the surface roughness of the first magnesium oxide wafer 1.

[0048] In other examples, the first magnesium oxide wafer 1 after polishing can be cleaned. Specifically, the first magnesium oxide wafer 1 can be immersed in an alcohol solution for 20-120 minutes to remove the wax remaining on the surface of the magnesium oxide during the polishing process, and then the first magnesium oxide wafer 1 can be rinsed in deionized water to remove the residual alcohol; and an ammonia solution (for example, NH4OH:H2O2:H2O=1:2:7) is prepared and heated in a water bath to 60-100°C, and the first magnesium oxide wafer 1 is immersed in the ammonia solution and continued to be heated in a water bath for 10-20 minutes, and then the first magnesium oxide wafer 1 is rinsed in deionized water to remove the residual ammonia, rinsed with deionized water several times, and finally blown dry with nitrogen.

[0049] In this embodiment, there is no particular limitation on the shapes of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4. In some examples, the shapes of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 may be a cuboid, a cube, a cylinder, etc.; in some examples, the shapes of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 may be any irregular shapes that are convenient for manufacturing the overall structure of the sensor without losing the sensor function.

[0050] In some examples, the first MgO wafer 1 and the second MgO wafer 4 may be of the same shape and size. In some examples, the first MgO wafer 1 and the second MgO wafer 4 may have different thicknesses.

[0051] Steps S100 to S300 are the wet chemical etching process involved in the embodiments of the present disclosure. In the present disclosure, the wet chemical etching method can realize the etching of a specific cavity 10 on the surface of single-crystal magnesium oxide (it is worth noting here that the wet etching method can realize the processing of different patterns and different depths on the surface of magnesium oxide), and can characterize the surface roughness and light reflection characteristics of the cavity 10 respectively by atomic force microscopy and reflectivity measurement instrument, optimize the etching parameters in combination with the experimental results, explore the equilibrium conditions between the etching reaction rate and the cavity surface material removal rate, and reduce the impact on the etching surface (roughness, etching products).

[0052] In addition, in the present disclosure, since magnesium oxide is an ionic crystal, it is difficult to react with gaseous atoms or molecules. Therefore, if a dry etching method is used to perform surface patterning processing on magnesium oxide, the etching rate is very low, and the general mask layer 2 cannot withstand long-term etching, so the traditional dry etching method is abandoned. According to the chemical properties of the magnesium oxide wafer, a wet etching method is used to achieve processing on the surface of the magnesium oxide wafer, and the etching rate of wet etching along a certain crystal orientation is faster, the damage to the material surface is smaller, the cost is lower, and the production efficiency is higher. In addition, wet etching is an important clue to reveal the crystal structure and reduces the processing cost.

[0053] Figure 2 is a schematic diagram showing the process flow of wet etching of magnesium oxide wafers involved in the embodiments of the present disclosure, specifically, Figure 2 1 is a schematic diagram showing a process flow of wet etching the first magnesium oxide wafer 1 to form the first magnesium oxide wafer 1 having a single cavity 10. It should be noted that: Figure 2 It is not a strict cross-sectional view, but an omitted plan view for the convenience of explanation. For example, the cavity 10 is shown as a groove in the figure.

[0054] Reference Figure 2 The following is a schematic diagram of a process flow of wet etching the first MgO wafer 1 to form the first MgO wafer 1 having a single cavity 10 according to the present disclosure.

[0055] In step S100, a first magnesium oxide wafer 1 and a second magnesium oxide wafer 4 may be prepared, and a mask layer 2 may be formed on the surface of the first magnesium oxide wafer 1. Specifically, in the preparation process of step S100, referring to Figure 2 (a) Silicon dioxide (SiO2) with a thickness of 0.5-1.5 μm can be formed as a mask layer 2 (including a first mask layer 21 and a second mask layer 22) by chemical vapor deposition (PECVD) on the surface of the first magnesium oxide wafer 1 (i.e., the upper surface and the lower surface of the first magnesium oxide wafer 1). In this case, since silicon dioxide hardly reacts with other acids except hydrofluoric acid (HF), it is more conducive to etching the first magnesium oxide wafer 1.

[0056] In some examples, the material of the mask layer 2 may be any one of silicon nitride, chromium, gold, etc. Therefore, a corresponding material may be selected as the mask layer 2 according to specific circumstances.

[0057] In step S200, the mask layer 2 of the first magnesium oxide wafer 1 may be photolithographically formed into a predetermined pattern. In some examples, the predetermined pattern may be a regular shape such as a circle, an ellipse or a rectangle. In other examples, the predetermined pattern may also be any irregular shape.

[0058] In some examples, the photolithography in the patterning process of step S200 can be implemented by a photolithography process.

[0059] Specifically, if Figure 2 As shown in (b), 2(c) and 2(d), the photolithography process may include the following steps: (1) Spreading: The photoresist 3 may be evenly coated on the first mask layer 21 using a spreader (see Figure 2(b)); (2) Pre-baking: placing the first magnesium oxide wafer 1 coated with the photoresist 3 on a heating table at 50-150°C for pre-baking; (3) Photolithography: placing the first magnesium oxide wafer 1 after pre-baking on a film plate for exposure, thereby forming a predetermined pattern on the first magnesium oxide wafer 1 (specifically, it can be on the photoresist 3 on the first mask layer 21); (4) Development: preparing a developer to expose the exposed part, and using a microscope to observe the completeness of the pattern after development and whether the photoresist 3 in the exposed area has been completely removed; (5) Hardening: placing the first magnesium oxide wafer 1 after development on a heating table at 120°C for heating, thereby evaporating the moisture in the photoresist 3 and making the photoresist 3 and the first magnesium oxide wafer 1 more closely attached.

[0060] In step S300, the first magnesium oxide wafer 1 can be wet-etched using a phosphoric acid solution to form a cavity 10 with a predetermined depth in the first magnesium oxide wafer 1, and the mask layer 2 is removed. Figure 2 The etching step will be described in detail.

[0061] In step S300, the wet etching process may include first transferring the first magnesium oxide wafer 1 after the photolithography of step S200 to a reactive ion etcher for reactive ion etching (RIE), removing the exposed portion of the first mask layer 21 (e.g., SiO2) to expose the first magnesium oxide wafer 1 (see Figure 2 (e)). Then, the first magnesium oxide wafer 1 is stripped so that only the mask layer 2 remains on the first magnesium oxide wafer 1 after stripping (refer to Figure 2 (f)). Specifically, the photoresist 3 on the surface of the first magnesium oxide wafer 1 can be removed by soaking it in a degumming solution heated in a water bath (the heating temperature can be 60° C.) for about 30 minutes, then performing acetone ultrasound for 1-5 minutes, and then soaking it in alcohol for 10-30 minutes.

[0062] In step S300, a phosphoric acid (H3PO4) solution may be used to wet-etch the first magnesium oxide wafer 1 to form a cavity 10 of a predetermined depth in the first magnesium oxide wafer 1 (see Figure 2 (g)). After the etching is completed, the RIE process can be performed again to remove the first mask layer 21 and the second mask layer 22 on the surface of the first magnesium oxide wafer 1 (refer to Figure 2 (h)).

[0063] Figure 3 1 is a schematic diagram showing a process flow of another embodiment of wet etching of magnesium oxide wafers according to an embodiment of the present disclosure. Specifically, Figure 3 FIG. 1 is a process flow chart showing a process of wet-etching a first MgO wafer 1 to form a first MgO wafer 1 having a plurality of cavities 10 .

[0064] Reference Figure 3 In step S100, a first magnesium oxide wafer 1 and a second magnesium oxide wafer 4 may be prepared, and a mask layer 2 may be formed on the surface of the first magnesium oxide wafer 1. Specifically, in the preparation process of step S100, referring to Figure 3 (a) and Figure 3 (b) Silicon dioxide (SiO2) with a thickness of 0.5-1.5 μm can be formed as a mask layer 2 (including a first mask layer 21 and a second mask layer 22) by chemical vapor deposition (PECVD) on the surface of the first magnesium oxide wafer 1 (i.e., the upper surface and the lower surface of the first magnesium oxide wafer 1). In this case, since silicon dioxide hardly reacts with other acids except hydrofluoric acid (HF), it is more conducive to etching the first magnesium oxide wafer 1.

[0065] In step S200, the mask layer 2 of the first magnesium oxide wafer 1 may be photolithographically formed into a plurality of predetermined patterns. In some examples, the predetermined pattern may be a regular pattern such as a circle, an ellipse or a rectangle (in this embodiment, a plurality of circular patterns). In other examples, the predetermined pattern may also be any irregular pattern.

[0066] In some examples, the photolithography in the patterning process of step S200 can be implemented by a photolithography process.

[0067] Specifically, if Figure 3 As shown in (c) and 3(d), the photolithography process may include the following steps: (1) Spreading: The photoresist 3 may be evenly coated on the first mask layer 21 using a spreader (see Figure 3 (c)); (2) pre-baking: placing the first MgO wafer 1 coated with the photoresist 3 on a heating platform at 50-150°C for pre-baking; (3) photolithography: placing the first MgO wafer 1 after pre-baking on a film plate for exposure, thereby forming a plurality of predetermined patterns on the first MgO wafer 1 (specifically, on the photoresist 3 on the first mask layer 21) (see Figure 3 d); (4) Development: Prepare a developer to reveal the exposed part, and use a microscope to observe the integrity of the pattern after development and whether the photoresist 3 in the exposed area has been completely removed; (5) Hardening: Place the developed first magnesium oxide wafer 1 on a heating table at 120°C for heating, thereby evaporating the moisture in the photoresist 3 and making the photoresist 3 and the first magnesium oxide wafer 1 more closely attached.

[0068] In step S300, the first magnesium oxide wafer 1 may be wet-etched using a phosphoric acid solution to form a plurality of cavities 10 with a predetermined depth in the first magnesium oxide wafer 1, and the mask layer 2 is removed. Figure 3 The etching step will be described in detail.

[0069] In step S300, the wet etching process may include first transferring the first magnesium oxide wafer 1 after the photolithography of step S200 to a reactive ion etcher for reactive ion etching (RIE), removing the exposed portion of the first mask layer 21 (e.g., SiO2) to expose the first magnesium oxide wafer 1 (see Figure 3 (e)). Then, the first magnesium oxide wafer 1 is stripped so that only the mask layer 2 remains on the first magnesium oxide wafer 1 after stripping (refer to Figure 3 (f)). Specifically, the photoresist 3 on the surface of the first magnesium oxide wafer 1 can be removed by soaking it in a degumming solution heated in a water bath (the heating temperature can be 60° C.) for about 30 minutes, then performing acetone ultrasound for 1-5 minutes, and then soaking it in alcohol for 10-30 minutes.

[0070] In step S300, a phosphoric acid (H3PO4) solution may be used to wet-etch the first magnesium oxide wafer 1 to form a cavity 10 of a predetermined depth in the first magnesium oxide wafer 1. After the etching is completed, the RIE process may be performed again to remove the first mask layer 21 and the second mask layer 22 on the surface of the first magnesium oxide wafer 1 (see Figure 3 (g)).

[0071] and Figure 2 The difference between the magnesium oxide wet etching process and the magnesium oxide wet etching process is that in this embodiment, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be magnesium oxide wafers of the same size of 2-4 inches respectively, and then a plurality of cavities 10 (such as Figure 3 The nine cavities 10 shown have the same size and the same depth).

[0072] In some examples, any one of sulfuric acid (H2SO4), nitric acid (HNO3), and hydrochloric acid (HCl) may be used to wet etch the first magnesium oxide wafer 1. In other examples, other acidic solutions or corrosive solutions may also be used as the etchant of the present disclosure.

[0073] In some examples, the first magnesium oxide wafer 1 can be etched using different pre-configured etchants (phosphoric acid, sulfuric acid, nitric acid, and hydrochloric acid as described above), and the etching rate and the surface morphology after etching can be characterized to determine the most suitable etchant. Usually, the etching rate is only related to the temperature and concentration of the etchant, and has nothing to do with the etching time. In this case, for example, the room temperature can be maintained, and the effects of the four etchants on the etching rate and the surface morphology after etching can be characterized at different concentrations to determine the most suitable etchant.

[0074] Figure 4FIG. 2 is a schematic diagram showing the effect of phosphoric acid solutions of different concentrations on the etching rate of the first magnesium oxide wafer 1 at different temperatures according to an embodiment of the present disclosure. Figure 4 As shown, it can be a schematic diagram of the etching rate obtained by etching the first magnesium oxide wafer 1 at different temperatures using phosphoric acid solutions with concentrations of 25%, 50%, 75% and 85%, wherein the abscissa represents temperature and the ordinate represents etching rate (nm / min). Figure 4 In the figure, broken line A represents the broken line graph of the etching rate under the phosphoric acid solution with a concentration of 85%. Broken line B represents the broken line graph of the etching rate under the phosphoric acid solution with a concentration of 75%. Broken line C represents the broken line graph of the etching rate under the phosphoric acid solution with a concentration of 50%. Broken line D represents the broken line graph of the etching rate under the phosphoric acid solution with a concentration of 25%. It can be seen from the figure that for each concentration of phosphoric acid solution, the etching rate increases with the increase of temperature. In addition, at 120°C, the etching rate of 50% phosphoric acid solution as an etchant is greater than that of other concentrations.

[0075] In some examples, the concentration of the phosphoric acid solution used to etch the first magnesium oxide wafer 1 is 25% to 85%. The temperature of the wet etching is 20°C to 120°C.

[0076] In other examples, the concentration of the phosphoric acid solution can be 50% to 85%. Figure 4 , at 120°C, the etching rate of a 50% phosphoric acid solution as an etchant is greater than that of other concentrations. In this case, a 50% phosphoric acid solution can be selected as an etchant.

[0077] In this embodiment, since roughness is one of the important indicators for measuring the etching method, an atomic force microscope (AFM) can be used to detect the surface roughness of the etching area of ​​the above-mentioned different acid solutions. That is, the surface roughness of the first magnesium oxide wafer 1 after etching with phosphoric acid solutions of different concentrations at different temperatures can be observed by an atomic force microscope (AFM).

[0078] In some examples, pits and scratches may appear on the surface of the cavity 10 of the first magnesium oxide wafer 1 when etching with a high concentration solution at room temperature. Therefore, the surface of the cavity 10 of the first magnesium oxide wafer 1 under different concentrations of phosphoric acid solution can be compared to determine the appropriate concentration of phosphoric acid solution. By comparison, it can be obtained that under the condition that the concentration of phosphoric acid solution is 50%, the surface roughness of the etched cavity 10 changes little and is not affected by temperature changes.

[0079] It should be noted that in actual operation, phosphoric acid solutions of other suitable concentrations may be selected according to specific circumstances and wet etching may be performed at a suitable temperature, which is not limited here.

[0080] In some examples, the wet-etched cavity 10 may be a cylinder, an elliptical cylinder, a cuboid, etc. In some examples, the cavity 10 may also be any other irregular cavity, etc. In this embodiment, the cavity 10 is preferably a cylinder (see Figure 3 ). Thus, the working performance of the magnesium oxide sealed cavity P can be enhanced, that is, the light reflection capability of the cavity 10 in the sensor can be enhanced by using the cylinder.

[0081] In some examples, the bottom diameter of the cylinder is 2-8 mm, and the height of the cylinder (ie, the depth of the etched cavity 10) can be 10-100 μm. In addition, in some examples, the height of the cylinder is preferably 80 μm. Thus, a cavity 10 that meets the requirements can be obtained.

[0082] In some examples, the depth of cavity 10 can be controlled by etching time.

[0083] Figure 5 is a perspective schematic diagram showing bonding of a first magnesium oxide wafer 1 and a second magnesium oxide wafer 4 according to an embodiment of the present disclosure; Figure 6 is a schematic cross-sectional view showing the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 after bonding according to an embodiment of the present disclosure. Figure 6 It shows Figure 5 A schematic cross-sectional view of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 after bonding, obtained by vertically cutting along the dotted line AA′. Figure 5 and Figure 6 The bonding process of step S400 is described in detail.

[0084] In some examples, reference Figure 5 and Figure 6 And the bonding process of step S400 can perform surface treatment on the side with the cavity 10 of the etched first magnesium oxide wafer 1 to form a first bonding surface 11 with a first predetermined roughness and a first hydrophilicity, and can perform surface treatment on the side of the second magnesium oxide wafer 4 to form a second bonding surface 41 with a second predetermined roughness and a second hydrophilicity, and directly bond the first bonding surface 11 of the first magnesium oxide wafer 1 with the second bonding surface 41 of the second magnesium oxide wafer 4 to form a sealed body P composed of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4. Among them, the direct bonding technology is to directly bond the etched magnesium oxide wafer with the unetched magnesium oxide wafer, and then use a scanning electron microscope and a leak detector to respectively characterize the sensitive structure after bonding in microscopic and macroscopic aspects, optimize the bonding parameters, and realize the high-strength direct bonding technology of magnesium oxide wafer / magnesium oxide wafer without an intermediate layer. Finally, a sealed body P is formed.

[0085] In some examples, the shapes of the first bonding surface 11 and the second bonding surface 41 in the first MgO wafer 1 and the second MgO wafer 4 in step S400 may be the same.

[0086] In this embodiment, in the bonding process, one side of the etched first magnesium oxide wafer 1 with the cavity 10 can be subjected to oxygen plasma activation treatment (OSA), and then surface treatment (WSA) can be performed using a wet activation solution to form a first bonding surface 11 having a first predetermined roughness and a first hydrophilicity, and one side of the second magnesium oxide wafer 4 can be subjected to oxygen plasma activation treatment, and then surface treatment can be performed using a wet activation solution to form a second bonding surface 41 having a second predetermined roughness and a second hydrophilicity.

[0087] In some examples, the first bonding surface 11 after OSA and WSA treatment may be a hydroxyl layer, and the second bonding surface 41 after OSA and WSA treatment may be a hydroxyl layer. Thus, the hydrophilicity of the first bonding surface 11 and the second bonding surface 41 can be enhanced. In some examples, by controlling the time of OSA and WSA treatment or by configuring the ratio of each component in the wet activation solution, the first bonding surface 11 and the second bonding surface 41 can form a high-density hydroxyl layer to form a super-hydrophilic surface, which can further enhance the hydrophilicity of the first bonding surface 11 and the second bonding surface 41.

[0088] In some examples, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be aligned and stacked for pre-bonding. Specifically, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be contacted from the edge until they are completely overlapped, and then a certain pressing force is applied with a tool such as tweezers to pre-bond the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4, thereby obtaining a pre-bonded magnesium oxide sealed cavity P. In this way, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be bonded more effectively.

[0089] In some examples, before the bonding process, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be cleaned before the above-mentioned step S100, respectively, and then placed in a plasma machine for oxygen plasma activation treatment. For example, the parameters of the plasma machine can be set as follows: the power is 180-200W, and the chamber pressure is 180-200mtorr. Then, a wet activation solution NH4OH:H2O2:H2O can be configured, and the samples of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 after OSA treatment are placed in the wet activation solution for wet activation surface treatment. In this case, different combinations of OSA treatment and WSA treatment time can be set to study the effect of treatment time on the surface roughness and hydrophilicity of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4.

[0090] In some examples, the time combination of OSA processing and WSA processing can be 5s and 5min, 5s and 10min, 15s and 10min, 15s and 10min, 30s and 5min, etc., thereby, the time combination of OSA processing and WSA processing can be reasonably selected.

[0091] In some examples, the time combination of the OSA treatment and the WSA treatment may be 5 seconds and 5 minutes. In this case, the first bonding surface 11 and the second bonding surface 41 after the OSA treatment and the WSA treatment can obtain the best surface roughness.

[0092] In some examples, the first predetermined roughness may be less than 1 nm, and the second predetermined roughness may be less than 1 nm. In addition, in some examples, the first predetermined roughness of the first magnesium oxide wafer 1 and the second predetermined roughness of the second magnesium oxide wafer 4 may be the same. Thus, the first bonding surface 11 and the second bonding surface 41 can be more tightly bonded.

[0093] It should be noted that the first predetermined roughness and the second predetermined roughness are important factors affecting the bonding between the first MgO wafer 1 and the second MgO wafer 4 and the light reflection rate in the optical sensor made of the first MgO wafer 1 and the second MgO wafer 4, and are also important indicators for measuring the effectiveness of the etching method, and the roughness is kept as close as possible to the roughness of the untreated first MgO wafer 1 and the second MgO wafer 4. Therefore, in the wet etching, an etching solvent and an etching temperature with little effect on the first predetermined roughness are selected to reduce the effect of the wet etching on the first MgO wafer 1; when the first MgO wafer 1 and the second MgO wafer 4 are bonded, the OSA and WSA treatments on the first MgO wafer 1 and the second MgO wafer 4 should also keep the effect on the first predetermined roughness and the second predetermined roughness to a minimum.

[0094] In some examples, the water contact angle of the first bonding surface 11 may be less than 5°, and the water contact angle of the second bonding surface 41 may be less than 5°. In addition, in some examples, the water contact angle of the first bonding surface 11 of the first magnesium oxide wafer 1 and the water contact angle of the second bonding surface 41 of the second magnesium oxide wafer 4 may be the same. In this case, after the two-step treatment of OSA and WSA, the first bonding surface 11 and the second bonding surface 41 can be further cleaned, the hydrophilicity of the first bonding surface 11 and the second bonding surface 41 can be improved, and the surface energy of the first bonding surface 11 and the second bonding surface 41 can be enhanced to reduce the gap of the subsequent bonding interface and increase the bonding strength.

[0095] In some examples, the first MgO wafer 1 and the second MgO wafer 4 may be single crystal wafers. In this case, the more stable properties of single crystal MgO enable the sealed body P composed of the first MgO wafer 1 and the second MgO wafer 4 to have more stable performance.

[0096] In addition, in some examples, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 may also be polycrystalline wafers.

[0097] In some examples, the wet activation solution may include ammonium hydroxide, hydrogen peroxide and water, and the ratio of ammonium hydroxide, hydrogen peroxide and water may be 1:1:5. Thus, the first bonding surface 11 and the second bonding surface 41 treated by WSA can have a more suitable surface roughness and hydrophilicity.

[0098] In this embodiment, the first bonding surface 11 of the first magnesium oxide wafer 1 and the second bonding surface 41 of the second magnesium oxide wafer 4 can be directly pre-bonded. During the pre-bonding, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be pressurized, and the pre-bonded first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be preheated at a temperature of 100 to 400° C. for 10 to 60 minutes, and the temperature is increased to 1200° C. at a rate of 10° C. per minute, and maintained for 60 to 240 minutes. Thus, the bonding strength of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be enhanced.

[0099] In some examples, the pre-bonded first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 are annealed. That is, the pre-bonded sample (i.e., the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4) can be placed in a graphite mold, and then transferred to a high-temperature hot press furnace for pressurized heating (i.e., annealing). Specifically, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be preheated at 200°C for 30 minutes, and then the temperature in the high-temperature hot press furnace is increased to about 1200°C at a rate of 10°C per minute, and maintained for about 120 minutes (the temperature and holding time here are not fixed values, and can be adjusted according to specific circumstances). In addition, the pressure in the high-temperature hot press furnace can be set to 6MPa (the pressure here is not a fixed value, and can be adjusted within a certain range) while reaching 1200°C, and the sample can be pressurized and maintained for 120 minutes.

[0100] In some examples, after annealing, the first MgO wafer 1 and the second MgO wafer 4 are cooled naturally, and then a tensile test is performed on the first MgO wafer 1 and the second MgO wafer 4 to test the bonding strength. If the bonding strength is about 7 MPa, the bonding strength requirement in the MEMS process is met.

[0101] In some examples, the bonding interface can be observed using a scanning electron microscope (SEM). If there is no large gap in the bonding interface and no obvious collapse at the sealing cavity 5, it can be determined that the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 are tightly bonded.

[0102] Figure 7 It shows the Figure 3 A top view of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 after bonding.

[0103] The above is a description of the preparation process of the sealing body P having a single sealing cavity 5, that is, a description of the bonding process of the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 having a single cavity 10. Figure 7 In some examples, the sealing body P may also have a plurality of sealing cavities 5. Thus, the magnesium oxide sealing cavities P can be mass-produced.

[0104] Specifically, in some examples, the method for preparing the magnesium oxide sealed cavity P may further include a cutting process. At this time, after the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 are bonded by the bonding step described above, a pre-cutting process may be performed to pre-scribe the bonded first magnesium oxide wafer 1 and the second magnesium oxide wafer 4, and then the sealed body P may be cut into a plurality of chips C (for example, Figure 7 There are 9 chips C shown, and each chip C has a sealed cavity 5.

[0105] In some examples, the encapsulation body P can be cut into 4 (2×2) chips C by pre-scribing. In some examples, the encapsulation body P can also be cut into 16 (4×4) chips C by pre-scribing. In some examples, the encapsulation body P can also be cut into 25 (5×5) chips C by pre-scribing. And so on.

[0106] In some examples, reference Figure 7 The sealing body P can be cut into a 10×10 mm cube-shaped chip C by pre-scribing.

[0107] In some examples, the cutting method may be mechanical cutting or laser cutting.

[0108] Figure 8 2 is a schematic diagram showing a sealing test of a sealing body P according to an embodiment of the present disclosure.

[0109] In this embodiment, if Figure 8As described above, the sealed body P composed of the first MgO wafer 1 and the second MgO wafer 4 that have been bonded or the sensor made of the MgO sealed cavity P of this embodiment can be tested. In some examples, the sensor can be tested using the rough inspection function of the helium fluorine oil pressurized leak detection device HF-4.

[0110] Specifically, the prepared sealed body P or sensor to be inspected can be placed in a pressure vessel (can be referred to as a container), and then the container is sealed, and then the gas in the pressure vessel is extracted so that the pressure vessel maintains a low pressure state or a vacuum state, for example, the sealed body P can be made to wait for 20-40min in a pressure environment lower than 50Pa. Then fluorine oil F113 (light fluorine oil) is injected into the airtight container until the sealed body P is submerged, and then nitrogen is filled into the container so that the sensor is kept for 50-60min under the effect of 2 atmospheric pressures (0.2MPa). If the sensor is not sealed (i.e., there is a gap between the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4), the pressure in the pressure vessel will squeeze the light fluorine oil into the sealed cavity 5 of the magnesium oxide sealed cavity P through the gap, and for the sensor with a good seal, its sealed body P is clean. After the pressurization is completed, the pressure in the container is slowly released, and then the light fluorine oil in the container is also released, and the sealed body P is taken out with a tool and placed in the atmosphere for 2min. Finally, immerse the sealed body P with a dry surface in heavy fluorine oil heated to 125°C in advance, and observe the bubble generation around it for at least 30 seconds. If it is found that some sealed bodies P quickly produce a stable bubble flow after being placed in heavy fluorine oil, and the bubbles are large and gradually increase in size during the rise, such sensors (or magnesium oxide sealed chambers P) are unqualified samples for sealing (such as Figure 8 If some sealing bodies P do not have bubbles or slowly generate bubbles after being placed in heavy fluorine oil, and the bubbles are small, dense and of constant size, and the bubbles are caused by defects or contamination on the surface of the sensor (or magnesium oxide sealing chamber P), then such sensors (or magnesium oxide sealing chambers P) can be considered to have qualified sealing properties (such as Figure 8 (Seal No. ① in the figure).

[0111] In some examples, the present disclosure can utilize the preparation method of the magnesium oxide sealed cavity P as described above to make a magnesium oxide sealed cavity P, and further use the magnesium oxide sealed cavity P to make optical fiber temperature sensors, optical fiber pressure sensors, optical fiber vibration sensors, optical fiber temperature and pressure integrated sensors, wireless passive temperature sensors, wireless passive pressure sensors 8, and wireless passive temperature and pressure integrated sensors and other sensors.

[0112] Fig. 9 1 is a schematic diagram showing the structure of Example 1 of the magnesium oxide sealed chamber P according to the embodiment of the present disclosure. Specifically, Fig. 91 is a schematic diagram showing the structure of an optical fiber type temperature and pressure integrated sensor made of a magnesium oxide sealed cavity P.

[0113] In some examples, reference Fig. 9 The magnesium oxide sealed cavity P of the present disclosure may further include a third magnesium oxide wafer 6 having a through hole 61. In some examples, the third magnesium oxide wafer 6 may be punched with a through hole 61 by laser or mechanical processing. The third magnesium oxide wafer 6 may be directly bonded to the second magnesium oxide wafer 4 to form a sealed body P consisting of the first magnesium oxide wafer 1, the second magnesium oxide wafer 4, and the third magnesium oxide wafer 6. Furthermore, a temperature-pressure integrated sensor 7 may be manufactured by fixing an optical fiber in the through hole 61.

[0114] In some examples, the temperature and pressure integrated sensor 7 may also include components such as a charge coupled device (CCD), a broadband light source (SLED), and a microlens. In the specific application of the temperature and pressure integrated sensor 7, the SLED emits a light beam, and the collimated transmission of the light beam is achieved by optical fiber. When the first light beam a1 passes through the sealed cavity 5 and reaches the bottom of the sealed cavity 5, when the sealed cavity 5 is deformed due to the external pressure, the intensity, wavelength, frequency, phase and other optical properties of the first light beam a1 reflected by the bottom of the sealed cavity 5 will change. The temperature and pressure integrated sensor 7 can detect the pressure by demodulating the change of the reflected first light beam a1.

[0115] On the other hand, changes in temperature in the working environment of the temperature-pressure integrated sensor 7 will cause changes in mechanical parameters such as the thermal expansion coefficient of the second magnesium oxide chip 4. When the second light beam a2 is reflected by the second bonding surface 41 of the second magnesium oxide chip 4, the temperature-pressure integrated sensor 7 can detect the temperature by demodulating changes in optical properties such as intensity, wavelength, frequency, and phase of the reflected second light beam a2.

[0116] Fig.10 1 is a schematic diagram showing the structure of Example 2 of the magnesium oxide sealed chamber P according to the embodiment of the present disclosure. Specifically, Fig.10 1 is a schematic diagram showing the structure of a wireless passive pressure sensor 8 made using a magnesium oxide sealed cavity P.

[0117] Fig.10 (a) is a schematic diagram showing a surface of the wireless passive pressure sensor 8 having the first capacitor electrode 81 . Fig.10 (b) is a schematic diagram showing a side of the wireless passive pressure sensor 8 having the second capacitor electrode 82 . Fig.10 (c) is a schematic cross-sectional view showing the wireless passive pressure sensor 8 .

[0118] In some examples, reference Fig.10The method for preparing the magnesium oxide sealed cavity P as described above can be used to first prepare the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 into the magnesium oxide sealed cavity P, and then the platinum slurry can be printed on the front and back surfaces of the magnesium oxide sealed cavity P using screen printing technology. In this way, the wireless passive pressure sensor 8 can be prepared.

[0119] When the wireless passive pressure sensor 8 is used, when the sealed cavity 5 is deformed by pressure, the capacitance between the first capacitor electrode 81 and the second capacitor electrode 82 changes. The wireless passive pressure sensor 8 can detect the temperature in the working environment by detecting the change in capacitance.

[0120] Fig.11 1 is a schematic diagram showing the structure of Example 3 of the magnesium oxide sealed chamber P according to the embodiment of the present disclosure. Specifically, Fig.11 1 is a schematic diagram showing the structure of a non-contact pressure sensor 9 made of a magnesium oxide sealed cavity P.

[0121] In some examples, a magnesium oxide sealed cavity P can be first made using the preparation method of the magnesium oxide sealed cavity P as described above, and then an optical fiber is placed at one end of the magnesium oxide sealed cavity P close to the second magnesium oxide chip 4, and the lens 91 at one end of the optical fiber is non-contact with the magnesium oxide sealed cavity P, and the optical fiber and the magnesium oxide sealed cavity P are in a vertical structure.

[0122] In some examples, referring to the working principle of the temperature and pressure integrated sensor 7 in Example 1, the non-contact pressure sensor 9 may also include components such as a charge coupled device (CCD), a broadband light source (SLED), and a microlens. In the specific application of the non-contact pressure sensor 9, the SLED emits a light beam, and the collimated transmission of the light beam is achieved by optical fiber. When the sealed cavity 5 is deformed due to the pressure, the third light beam a3 passes through the sealed cavity 5 to the bottom of the sealed cavity 5, and the intensity, wavelength, frequency, phase and other optical properties of the third light beam a3 reflected by the bottom of the sealed cavity 5 will change. The non-contact pressure sensor 9 can detect the pressure by demodulating the change of the reflected third light beam a3.

[0123] Similarly, referring to the working principle of the temperature-pressure integrated sensor 7 in Example 1, the non-contact pressure sensor 9 can also detect the temperature.

[0124] In some embodiments, the second magnesium oxide wafer 4 with a specific structure may also be formed by wet etching the second magnesium oxide wafer 4 .

[0125] In some examples, a cross beam structure can be etched on the second bonding surface 41 of the second magnesium oxide wafer 4, and a cylindrical deep cavity can be etched on the opposite surface of the second bonding surface 41. Then, the first magnesium oxide wafer 1 and the second magnesium oxide wafer 4 can be bonded by the preparation method described above, and a third magnesium oxide wafer 6 is bonded on a side close to the second magnesium oxide wafer 4 to form a magnesium oxide sealed cavity P. A light source is further placed above the magnesium oxide sealed cavity P to make a vibration sensor, and the vibration signal can be detected by means of the vibration sensor.

[0126] Similarly, in other embodiments, other types of sensors may be made based on the magnesium oxide sealed cavity P, which are not listed one by one here.

[0127] Although the present disclosure is specifically described above in conjunction with the accompanying drawings and embodiments, it is to be understood that the above description does not limit the present disclosure in any form. Those skilled in the art may modify and change the present disclosure as needed without departing from the essential spirit and scope of the present disclosure, and these modifications and changes all fall within the scope of the present disclosure.

Claims

1. A method for preparing a magnesium oxide sealed cavity, wherein the magnesium oxide sealed cavity is applied to a sensor based on optical principles, characterized in that: The preparation method comprises: forming a mask layer on the surface of a first magnesium oxide wafer; Performing photolithography on the mask layer of the first magnesium oxide wafer to form a predetermined pattern; Wet-etching the first magnesium oxide wafer using a phosphoric acid solution to form a cavity with a predetermined depth in the first magnesium oxide wafer, and removing the mask layer; and directly bonding the first bonding surface of the first magnesium oxide wafer to the second bonding surface of the second magnesium oxide wafer to form a sealed body consisting of the first magnesium oxide wafer and the second magnesium oxide wafer, Wherein, the first bonding surface is a side of the first magnesium oxide wafer having the cavity.

2. The preparation method according to claim 1, characterized in that: The sensor is suitable for an ambient temperature of 1350°C-2000°C.

3. The preparation method according to claim 1, characterized in that: The depth of the cavity is 10-100 μm, and the depth of the cavity can be adjusted by controlling the wet etching time.

4. The preparation method according to claim 1, characterized in that: The roughness of the first bonding surface and the roughness of the second bonding surface are both less than 1 nm, and the water contact angle of the first bonding surface and the water contact angle of the second bonding surface are both less than 5°.

5. The preparation method according to claim 1, characterized in that: The concentration of the phosphoric acid solution is 25% to 85%, and the temperature of the wet etching is 20° C. to 120° C.

6. An optical fiber temperature and pressure integrated sensor, characterized in that: The magnesium oxide sealed cavity is prepared using the preparation method of any one of claims 1 to 5.

7. The optical fiber temperature and pressure integrated sensor according to claim 6, characterized in that: A third magnesium oxide wafer is included, and the third magnesium oxide wafer is bonded to the second magnesium oxide wafer and the first magnesium oxide wafer simultaneously.

8. The optical fiber temperature and pressure integrated sensor according to claim 7, characterized in that: It also includes an optical fiber. The third magnesium oxide wafer is provided with a through hole, and the optical fiber is fixed in the through hole.

9. A wireless passive pressure sensor, characterized in that: The magnesium oxide sealed cavity is prepared using the preparation method of any one of claims 1 to 5.

10. A non-contact pressure sensor, characterized in that: The magnesium oxide sealed cavity is prepared using the preparation method of any one of claims 1 to 5.

11. The non-contact pressure sensor according to claim 10, characterized in that: The invention comprises an optical fiber and a lens arranged at one end of the optical fiber.

12. The non-contact pressure sensor according to claim 11, characterized in that: The optical fiber is placed at one end of the magnesium oxide sealed cavity close to the second magnesium oxide wafer, and the lens at one end of the optical fiber is in non-contact with the magnesium oxide sealed cavity. The optical fiber and the magnesium oxide sealed cavity are in a vertical structure.