Sodium tetrafluoroborate non-aqueous electrolyte and preparation method and application thereof
By reacting sodium fluoride with boron trifluoride complex in a high-purity organic solvent, a high-purity sodium tetrafluoroborate non-aqueous electrolyte is solved, and the problems of high energy consumption and low solubility of the preparation of sodium tetrafluoroborate non-aqueous electrolyte are solved. Achieve high performance and low cost production of sodium ion batteries.
Patent Information
- Application Number
- CN202310589023.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The existing preparation methods for sodium tetrafluoroborate non-aqueous electrolyte require high energy consumption, resulting in high production cost of sodium ion batteries, and the solubility of sodium tetrafluoroborate in commonly used electrolytes is low, making it difficult to achieve satisfactory battery performance.
By reacting sodium fluoride with boron trifluoride complex in a high-purity organic solvent, high-purity sodium tetrafluoroborate non-aqueous electrolyte is obtained by filtration, using specific organic solvents such as tetraethylene glycol dimethyl ether and phosphate triphosphate Ethyl ester, etc., improve the solubility of electrolytes and battery performance.
The production cost of sodium tetrafluoroborate non-aqueous electrolyte is reduced, and the charge and discharge characteristics and cycle characteristics of sodium ion batteries are improved. The electrolyte is well dissolved in organic solvents, and precipitation is inhibited for a long time, showing better performance than the electrolyte prepared in traditional methods.
Smart Images

Figure CN119018906A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and in particular relates to a sodium tetrafluoroborate non-aqueous electrolyte and a preparation method and application thereof. Background Art
[0002] At present, the sodium salt of non-aqueous electrolyte of sodium ion battery mainly adopts sodium hexafluorophosphate, but sodium hexafluorophosphate is sensitive to moisture and easily generates HF, which causes continuous damage to SEI film and positive electrode active materials, thereby leading to a continuous decline in battery performance. Compared with sodium hexafluorophosphate, sodium tetrafluoroborate is not sensitive to moisture, can passivate the commonly used current collector aluminum foil, and has good high temperature performance. In addition, sodium tetrafluoroborate-based electrolyte has a good film-forming effect on carbon negative electrode. For example, the applicant's prior patent applications 202210802720.4 and 202110908583.8 use a higher proportion of sodium tetrafluoroborate, and patent CN110140253A also uses sodium tetrafluoroborate as a sodium salt.
[0003] At present, most methods for preparing sodium tetrafluoroborate-based non-aqueous electrolytes are to dissolve sodium tetrafluoroborate in an organic solvent. For example, this method is used in the above three patent applications. The main problem with this preparation method is that the process of producing sodium tetrafluoroborate requires high energy consumption. The production of sodium tetrafluoroborate is mainly gas-solid reaction method, aqueous solution reaction method and non-aqueous solution method. Among them, the sodium tetrafluoroborate generated by the gas-solid reaction method will wrap NaF, the reaction is not thorough, and a large amount of organic solvent is required for washing, and the removal of the solvent requires high energy consumption; the aqueous solution reaction method is difficult to prepare high-purity NaBF4, mainly because the sodium tetrafluoroborate in the primary product contains crystal water, and the removal of crystal water requires a temperature of more than 200°C, which will cause the sodium tetrafluoroborate to decompose; the solution method also requires a concentration and recrystallization process, and these methods will bring high energy consumption.
[0004] CN102803142A mentions that the mother liquor of lithium tetrafluoroborate is used directly as an electrolyte. However, sodium tetrafluoroborate is different from lithium tetrafluoroborate in that the solubility of sodium tetrafluoroborate in commonly used organic solvents for electrolytes is very low (usually less than 0.3 M), while the solubility of lithium tetrafluoroborate in commonly used carbonate electrolytes can be as high as 5 M. Therefore, attempts to directly apply the solvent system of lithium tetrafluoroborate electrolyte to sodium tetrafluoroborate electrolyte have failed to achieve satisfactory results.
[0005] Therefore, it is necessary to develop a new method for preparing sodium tetrafluoroborate non-aqueous electrolyte to reduce the energy consumption of the production process, thereby reducing the production cost of sodium ion batteries. Summary of the invention
[0006] Therefore, the object of the present invention is to provide a method for preparing sodium tetrafluoroborate non-aqueous electrolyte by a simple method, while reducing the production cost of the sodium tetrafluoroborate non-aqueous electrolyte and making the sodium ion battery using the electrolyte have sufficient charge and discharge characteristics.
[0007] After in-depth research, the inventor of the present invention unexpectedly found that when a specific organic solvent (such as tetraethylene glycol dimethyl ether, triethyl phosphate, trimethyl phosphate, etc.) is selected, the reaction solution obtained by in-situ reaction of sodium fluoride and boron trifluoride complex is directly used as an electrolyte, and the obtained battery performance is better than the traditional preparation method (directly dissolving sodium tetrafluoroborate in the corresponding solvent). Specifically, high-purity sodium fluoride is reacted in a high-purity organic solvent containing a boron trifluoride complex, and the sodium fluoride is filtered out. The obtained solution with sodium tetrafluoroborate as the sodium salt and the high-purity organic solvent as the solvent can be directly used as a non-aqueous electrolyte for sodium ion batteries, and its performance is better than the electrolyte prepared in the traditional way.
[0008] The first aspect of the present invention provides a method for preparing a sodium tetrafluoroborate non-aqueous electrolyte, the method comprising: reacting sodium fluoride with a boron trifluoride complex in an organic solvent, filtering out unreacted sodium fluoride after the reaction is completed, and obtaining the sodium tetrafluoroborate non-aqueous electrolyte, wherein:
[0009] The organic solvent includes one or more first solvents selected from ether solvents and phosphate ester solvents;
[0010] The boron trifluoride complex is a complex formed by boron trifluoride and one or more of the organic solvents.
[0011] According to the preparation method provided by the present invention, preferably, the sodium fluoride is high-purity sodium fluoride with a purity greater than 99%, more preferably greater than 99.9%; preferably, the organic solvent is a high-purity organic solvent with a purity greater than 99%, more preferably greater than 99.9%.
[0012] The inventors of the present invention unexpectedly found that when high-purity sodium fluoride, a specific high-purity organic solvent, and a corresponding organic solvent-boron trifluoride complex are selected, a non-aqueous electrolyte containing sodium tetrafluoroborate can be constructed in situ. The sodium tetrafluoroborate non-aqueous electrolyte produced by this method has high quality and can be directly used as an electrolyte for sodium batteries (including sodium ion batteries), and its effect is better than the sodium tetrafluoroborate non-aqueous electrolyte prepared by the traditional method.
[0013] According to the preparation method provided by the present invention, in addition to the first solvent, the organic solvent may further include one or more second solvents selected from carbonate solvents and carboxylate solvents. The volume percentage content of the first solvent in the organic solvent is preferably greater than 50%, for example, 55-100%, 60-90% or 70-80%.
[0014] According to the preparation method provided by the present invention, the ether solvent can be selected from one or more of tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, dimethoxymethane, 1,2-dimethoxyethane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether.
[0015] The phosphate solvent may be selected from one or more of triphenyl phosphate, trimethyl phosphate, triethyl phosphate, tripropyl phosphate, and tributyl phosphate.
[0016] The carbonate solvent may be a cyclic carbonate solvent and / or a chain carbonate solvent.
[0017] Preferably, the cyclic carbonate may be propylene carbonate; the chain carbonate may be a carbonate synthesized from a straight-chain or branched aliphatic monoalcohol having a carbon number of 3 to 8 and carbonic acid, preferably, the chain carbonate may be one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate and methyl ethyl carbonate.
[0018] Preferably, the carboxylate solvent may be a cyclic carboxylate solvent and / or a chain carboxylate solvent. The cyclic carboxylate may be γ-butyrolactone, and the chain carbonate may be a chain carboxylate with a carbon number of 3 to 8; preferably, the chain carboxylate may be one or more of methyl acetate, ethyl acetate, propyl acetate, propyl propionate and ethyl propionate.
[0019] In some embodiments of the present invention, a solution containing a boron trifluoride complex can be used as a reactant, and the solvent of the solution can be the organic solvent described in the present invention or the first solvent described in the present invention. In some embodiments of the present invention, the reaction can be carried out without adding other solvents (reaction solvents).
[0020] In some embodiments of the present invention, the preparation method comprises: after completing the reaction of the boron trifluoride complex and sodium fluoride in a system using the first solvent as a reaction solvent, adding the second solvent.
[0021] In a preferred embodiment of the present invention, the molar concentration of the boron trifluoride complex in the organic solvent is 0.05-2M.
[0022] In a preferred embodiment of the present invention, the molar ratio of boron trifluoride to sodium fluoride in the boron trifluoride complex is 1 to 3:1.
[0023] As the boron trifluoride complex used in the present invention, one kind can be used alone or a mixture of multiple kinds can be used. When two or more kinds are used, their combination and ratio can be appropriately selected according to the purpose. In some embodiments of the present invention, the boron trifluoride complex can be prepared by charging boron trifluoride gas into the organic solvent. Preferably, the amount of boron trifluoride gas charged is such that the molar concentration of boron trifluoride in the formed boron trifluoride complex in the organic solvent (comprising the organic solvent combined in the boron trifluoride complex) is 0.05 to 2M.
[0024] According to the preparation method provided by the present invention, the temperature for the reaction of the boron trifluoride complex with sodium fluoride can be 5 to 100° C., preferably 5 to 30° C.; the reaction time can be 0.5 to 48 hours, preferably 8 to 40 hours.
[0025] Normally, the reaction is almost complete within 24 hours, which can be confirmed by sampling the reaction solution and analyzing it using known methods such as various ion chromatography methods.
[0026] In the reaction process, other components not belonging to the boron trifluoride complex, sodium fluoride and organic solvent can be added without affecting the effect of the present invention, but other components are usually not required. In addition, in the reaction process, the order of adding the boron trifluoride complex and sodium fluoride is not particularly limited and can be appropriately adjusted. In some embodiments, other sodium salts can be further mixed and / or other solvent additives can be added to the prepared basic electrolyte containing sodium tetrafluoroborate for use as a commercial electrolyte.
[0027] The second aspect of the present invention provides a sodium tetrafluoroborate nonaqueous electrolyte prepared by the above method.
[0028] The third aspect of the present invention provides the use of the sodium tetrafluoroborate nonaqueous electrolyte prepared by the above method as a sodium ion battery electrolyte.
[0029] The present invention prepares an electronic grade sodium tetrafluoroborate non-aqueous electrolyte in an in-situ manner, which can significantly reduce the production cost compared with the existing method of first preparing sodium tetrafluoroborate and then dissolving it in a non-aqueous solvent. In addition, the electrolyte obtained in this way is superior to the traditional electrolyte. Because the preparation process uses a high-purity solvent and sodium salt, the obtained electrolyte is of high quality and can give full play to the charge and discharge characteristics of the sodium ion battery, and the sodium tetrafluoroborate as an electrolyte is well dissolved in an organic solvent, and its precipitation can be suppressed for a long time, so the sodium ion battery using the electrolyte has better cycle characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, wherein:
[0031] Figure 1 The first two charge-discharge curves of the battery prepared using the electrolyte of Example 1.
[0032] Figure 2 The cycle capacity retention rate of the battery prepared using the electrolyte of Example 1. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0034] The raw materials used in the examples are described as follows:
[0035] Solvent: TMP: trimethyl phosphate; TEP: triethyl phosphate; TEGDME: tetraethylene glycol dimethyl ether; DEGDME: diethylene glycol dimethyl ether, the purity of the above solvents is greater than 99%, and the water content is less than 50ppm.
[0036] The purity of high-purity sodium fluoride is greater than 99.5% and the water content is less than 300ppm.
[0037] Example 1
[0038] Preparation of the electrolyte of the present invention
[0039] (1) Boron trifluoride gas is charged into trimethyl phosphate to prepare a solution containing a boron trifluoride trimethyl phosphate complex, so that the concentration of boron trifluoride in trimethyl phosphate (including trimethyl phosphate bound in the complex) is 1M.
[0040] (2) Add high-purity sodium fluoride (the molar ratio of boron trifluoride to sodium fluoride is 1:2) to the solution obtained in step (1), and react at a temperature of 10° C. for 40 hours.
[0041] (3) After the reaction is completed, the unreacted sodium fluoride is filtered off to obtain a NaBF4TMP electrolyte with a concentration of about 1 M.
[0042] (4) Take 100 mL of the 1 M NaBF4 TMP electrolyte obtained in step (3), add 0.2 M NaPF6 and 2.5% by mass of vinylene carbonate (VC) to prepare 1 M NaBF4 + 0.2 M NaPF6 TMP + 2.5% VC electrolyte, denoted as A1.
[0043] Example 2
[0044] Preparation of the electrolyte of the present invention
[0045] (1) Boron trifluoride gas is introduced into triethyl phosphate to prepare a solution containing a boron trifluoride triethyl phosphate complex, so that the concentration of boron trifluoride in triethyl phosphate (including triethyl phosphate bound in the complex) is 0.8 M.
[0046] (2) Add high-purity sodium fluoride (the molar ratio of boron trifluoride to sodium fluoride is 1:2) to the solution obtained in step (1), and react at a temperature of 5° C. for 24 hours.
[0047] (3) After the reaction is completed, the unreacted sodium fluoride is filtered off to obtain a NaBF4TEP electrolyte with a concentration of about 0.8 M.
[0048] (4) Take 100 mL of the 1 M NaBF4 TEP electrolyte obtained in step (3), add 0.2 M NaPF6 and 2.5% by mass of vinylene carbonate (VC) to prepare 1 M NaBF4 + 0.2 M NaPF6 TEP + 2.5% VC electrolyte, recorded as A2.
[0049] Example 3
[0050] Preparation of the electrolyte of the present invention
[0051] (1) Boron trifluoride gas is introduced into a mixed solvent of trimethyl phosphate and ethylene carbonate (volume ratio 7:3) to prepare a solution containing a boron trifluoride complex, so that the concentration of boron trifluoride in the complex in the mixed solvent (including trimethyl phosphate and ethylene carbonate combined in the complex) is 1.2 M.
[0052] (2) Add high-purity sodium fluoride (the molar ratio of boron trifluoride to sodium fluoride is 1:1.5) to the solution obtained in step (1), and react at a temperature of 12° C. for 24 hours.
[0053] (3) After the reaction is completed, the unreacted sodium fluoride is filtered off to obtain a NaBF4TMP / EC (7 / 3) electrolyte with a concentration of about 1.2 M, which is recorded as A3.
[0054] Example 4
[0055] Preparation of the electrolyte of the present invention
[0056] (1) Boron trifluoride gas is charged into tetraethylene glycol dimethyl ether to prepare a solution containing a boron trifluoride tetraethylene glycol dimethyl ether complex, so that the concentration of boron trifluoride in the complex in tetraethylene glycol dimethyl ether solvent (including tetraethylene glycol dimethyl ether bound in the complex) is 1M.
[0057] (2) Add high-purity sodium fluoride (the molar ratio of boron trifluoride to sodium fluoride is 1:3) to the solution obtained in step (1), and react at a temperature of 12° C. for 24 hours.
[0058] (3) After the reaction is completed, the unreacted sodium fluoride is filtered off to obtain a NaBF4TEGDME electrolyte with a concentration of about 1 M, which is recorded as A4.
[0059] Example 5
[0060] Preparation of the electrolyte of the present invention
[0061] (1) Boron trifluoride gas is charged into diethylene glycol dimethyl ether to prepare a solution containing a boron trifluoride diethylene glycol dimethyl ether complex, so that the concentration of boron trifluoride in the complex in the diethylene glycol dimethyl ether solvent (including tetraethylene glycol dimethyl ether bound in the complex) is 0.2 M.
[0062] (2) Add high-purity sodium fluoride (the molar ratio of boron trifluoride to sodium fluoride is 1:1.2) to the solution obtained in step (1), and react at 7° C. for 24 hours.
[0063] (3) After the reaction is completed, the unreacted sodium fluoride is filtered off to obtain a NaBF4DEGDME electrolyte with a concentration of about 0.2 M.
[0064] (4) Take 100 mL of the 0.2 M NaBF4 DEGDME electrolyte obtained in step (3), add 1 M NaPF6 to prepare a 0.2 M NaBF4 + 1 M NaPF6 DEGDME electrolyte solution, recorded as A5.
[0065] Comparative Examples 1-5
[0066] By conventional means, the sodium salt is directly dissolved in a solvent to prepare an electrolyte having a composition corresponding to that of Examples 1-5:
[0067] Comparative Example 1 (B1): 1M NaBF4+0.2M NaPF6 TMP+2.5% VC
[0068] Comparative Example 2 (B2): 1M NaBF4+0.2M NaPF6 TEP+2.5% VC
[0069] Comparative Example 3 (B3): 1M NaBF4 TMP / EC (7 / 3)
[0070] Comparative Example 4 (B4): 1M NaBF4 TEGDME
[0071] Comparative Example 5 (B5): 0.2M NaBF4+1M NaPF6 DEGDME
[0072] Comparative Examples 6-7
[0073] The electrolytes were prepared in the same manner as in Example 1, except that a solvent or sodium fluoride with a purity lower than 99% was used to prepare electrolytes C1 and C2, wherein the purity of trimethyl phosphate used in C1 was 98%, and the purity of sodium fluoride used in C2 was 98%.
[0074] Comparative Examples 8-10
[0075] Sodium tetrafluoroborate electrolytes C3-C5 were prepared using conventional solvents, respectively. C3 used a carbonate solvent with a volume ratio of 1:1 between ethylene carbonate and propylene carbonate, C4 used a carbonate solvent with a volume ratio of 1:1 between ethylene carbonate and diethyl carbonate, and C5 used a carbonate solvent with a volume ratio of 1:1:1 between ethylene carbonate, propylene carbonate and diethyl carbonate, to prepare saturated solutions of NaBF4 in different solvents.
[0076] Performance Characterization
[0077] Preparation of electrodes and batteries:
[0078] O3-Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 ]O2 is the positive electrode active material, acetylene black is the conductive agent, and polytetrafluoroethylene is the binder. They are evenly mixed in a mass ratio of 90:6:4, and N-methylpyrrolidone is added to form a slurry; the slurry is coated on aluminum foil and vacuum dried overnight at 120°C; the positive electrode sheet can be obtained after rolling.
[0079] Take hard carbon as negative electrode active material, acetylene black as conductive agent, polytetrafluoroethylene as binder, mix them evenly in a mass ratio of 90:5:5, add N-methylpyrrolidone to make slurry; coat the slurry on aluminum foil, vacuum dry overnight at 120°C; and roll to obtain negative electrode sheet.
[0080] The matched positive and negative electrodes are assembled into a full battery (the capacity of the negative electrode is 10% more than that of the positive electrode). A button 2032 battery with positive electrode / / separator / / negative electrode is assembled, and the electrolyte prepared in the embodiment or comparative example is used as the electrolyte.
[0081] Test method: The battery test was first cycled 2 times at 0.1C (1C = 100 mAh / g, based on the positive electrode loading) (voltage range 1.5V-4V), and then cycled 500 times at 0.5C rate (1.5-4V). The results are shown in Table 1.
[0082] Table 1
[0083] Electrolytes Capacity retention rate Electrolytes Capacity retention rate Electrolytes Capacity retention rate A1 83.8% B1 62.5% C1 40.2% A2 81.2% B2 63.6% C2 35.7% A3 83.7% B3 72.4% C3 26.7% A4 72.3% B4 51.3% C4 13.9% A5 65.2% B5 31.7% C5 20.4%
[0084] Figure 1These are the first two charge and discharge curves of a battery made using the electrolyte of Example 1. Figure 2 is the cycle capacity retention rate of the battery made with the electrolyte of Example 1. Figure 1 and Figure 2 It can be seen that the electrolyte prepared by the method of the present invention is of high quality and can give full play to the charge and discharge characteristics of the sodium ion battery, and the first coulomb efficiency reaches 84.2%; in addition, sodium tetrafluoroborate as an electrolyte is well dissolved in an organic solvent and can suppress its precipitation for a long time, so the sodium ion battery using the electrolyte shows good cycle characteristics in 500 cycles.
[0085] It can be seen from the examples and comparative examples that when high-purity sodium fluoride, a specific high-purity organic solvent, and a complex of an organic solvent and boron trifluoride are selected, a non-aqueous electrolyte containing sodium tetrafluoroborate can be constructed in situ. And the performance of the electrolyte constructed in situ is better than that of the electrolyte configured in a traditional way.
[0086] The above embodiments are only preferred embodiments of the present invention and are only used to explain the present invention, rather than to limit the present invention. Modifications, substitutions, changes, etc. made by those skilled in the art without departing from the spirit of the present invention should all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a sodium tetrafluoroborate nonaqueous electrolyte, the preparation method comprising: Sodium fluoride and a boron trifluoride complex are reacted in an organic solvent, and after the reaction is completed, unreacted sodium fluoride is filtered off to obtain the sodium tetrafluoroborate nonaqueous electrolyte, wherein: The organic solvent includes one or more first solvents selected from ether solvents and phosphate ester solvents; The boron trifluoride complex is a complex formed by boron trifluoride and one or more of the organic solvents.
2. The preparation method according to claim 1, wherein The purity of the sodium fluoride is greater than 99%, preferably greater than 99.9%; the purity of the high-purity organic solvent is greater than 99%, preferably greater than 99.9%.
3. The preparation method according to claim 1 or 2, wherein The organic solvent further comprises a second solvent selected from one or more of carbonate solvents and carboxylate solvents; preferably, the volume percentage content of the first solvent in the organic solvent is greater than 50%, such as 60-90%.
4. The preparation method according to any one of claims 1 to 3, wherein The ether solvent is selected from one or more of tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, dimethoxymethane, 1,2-dimethoxyethane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether; the phosphate ester solvent is selected from one or more of triphenyl phosphate, trimethyl phosphate, triethyl phosphate, tripropyl phosphate and tributyl phosphate; Preferably, the carbonate solvent is a cyclic carbonate solvent and / or a chain carbonate solvent, wherein the cyclic carbonate is propylene carbonate; the chain carbonate is a carbonate synthesized from a straight-chain or branched aliphatic monoalcohol having a carbon number of 3 to 8 and carbonic acid, preferably, the chain carbonate is one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate and methyl ethyl carbonate. Preferably, the carboxylate solvent is a cyclic carboxylate solvent and / or a chain carboxylate solvent, wherein the cyclic carboxylate is γ-butyrolactone, and the chain carbonate is a chain carboxylate with a carbon number of 3 to 8; preferably, the chain carboxylate is one or more of methyl acetate, ethyl acetate, propyl acetate, propyl propionate and ethyl propionate.
5. The preparation method according to any one of claims 1 to 4, wherein The molar concentration of the boron trifluoride complex in the organic solvent is 0.05-2M.
6. The preparation method according to any one of claims 1 to 5, wherein The molar ratio of boron trifluoride to sodium fluoride in the boron trifluoride complex is 1 to 3:
1.
7. The preparation method according to any one of claims 1 to 6, wherein The preparation method further comprises: preparing the boron trifluoride complex by charging boron trifluoride gas into the organic solvent.
8. The preparation method according to any one of claims 1 to 7, wherein The temperature for the reaction of the boron trifluoride complex with sodium fluoride is 5 to 100° C., preferably 5 to 30° C.; the reaction time is 0.5 to 48 hours, preferably 8 to 40 hours.
9. The sodium tetrafluoroborate nonaqueous electrolyte prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the sodium tetrafluoroborate nonaqueous electrolyte prepared by the preparation method according to any one of claims 1 to 8 as an electrolyte for sodium ion batteries.