Large scale synthesis of solid electrolyte material particulate powder for solid state batteries, and systems and methods thereof
Through the CNC stoichiometric liquid mixture injection and dynamic crystallization process, the problem of insufficient energy density and safety performance in large-scale manufacturing of solid-state battery materials is solved, and efficient and low-cost solid-state battery materials are achieved.
Patent Information
- Application Number
- CN202411014602.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-24
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult for the prior art to manufacture solid-state battery materials with high energy density and excellent safety performance on a large scale, especially in terms of cycle life, thermal stability and production efficiency, and conventional processes consume high energy, complex steps and are not economical.
CNC stoichiometric amounts of a liquid mixture containing lithium salt and metal inorganic salt are used to form a gas-liquid mixture, and high-speed spraying and drying are performed through a power jet chamber, followed by a dynamic crystallization process in the annealing chamber to obtain a high-purity solid state Electrolyte material.
Solid-state battery materials with high energy density, long cycle life and excellent thermal stability are achieved, reducing production costs and step complexity and improving production efficiency.
Smart Images

Figure CN119018934A_ABST
Abstract
Description
[0001] This application is a divisional application of an invention patent application with an application date of November 25, 2022, application number 202280078468.5, and invention name “Large-scale synthesis of solid electrolyte material particle powder for solid-state batteries and its system and method”.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims the benefit of U.S. Provisional Patent Application Serial No. 63 / 283,214, filed on November 25, 2021, which is incorporated herein by reference in its entirety. Technical Field
[0004] The present invention generally relates to compositions, methods and systems for large-scale synthesis and manufacture of battery materials, including electrolyte powders, anode or cathode active material particles for rechargeable lithium-ion batteries and solid-state batteries. Background Art
[0005] In the clean energy industry (e.g., batteries for electric vehicles), there is a continuous demand for lightweight, compact, and high energy density batteries, requiring dramatic improvements in battery safety, energy density, cycle life, large-scale production, and low cost. Typically, conventional lithium-ion batteries (LIBs) contain a non-aqueous electrolyte, which is a liquid-based electrolyte with a lithium salt in a flammable organic solvent. However, the use of liquid-based electrolytes has its disadvantages. For example, serious safety issues are caused by its flammability and the presence of volatile organic solvents used in the electrolyte; lithium dendrites inevitably grow in LIB liquid electrolytes, leading to short circuit problems (especially at high charge / discharge cycle rates); high resistance solid electrolyte interfaces (SEI) at the electrodes lead to capacity loss, leakage, leakage at the electrodes, and / or corrosion; electrolyte decomposition at high voltages limits the use of high voltage cathode materials; and the formation of hydrogen fluoride (HF) during thermal runaway.
[0006] Solid-state batteries offer opportunities for large battery cells, particularly in electric vehicle applications. Since solid systems do not require any cooling systems, solid-state batteries are lighter and require less space than the lithium-ion batteries that power electric vehicles.
[0007] Generally, there are various synthesis methods for solid electrolyte materials, such as pulsed laser deposition, RF magnetron sputtering, solid pyrolysis synthesis, sol-gel method, combustion synthesis, ball milling, electrostatic spinning, molten salt method, spark plasma sintering route, atomic layer deposition, etc. However, all of these methods are very expensive and uneconomical for large-scale manufacturing, because the method takes a long time to obtain the final product (too many production steps), and a large amount of products (for example, compared to grams or kilograms, in tons) cannot be provided, and close solid-solid contact cannot be achieved and maintained. Therefore, it is necessary to develop a new method for manufacturing solid-state battery materials for large-scale synthesis and manufacture of solid-state secondary batteries with high energy density and excellent safety performance.
[0008] Most conventional processes for making solid electrolyte materials include many steps: mixing, adding excess lithium to make up for lithium loss during the high-heat sintering process, and many steps cannot be performed continuously in large-scale production lines. In addition, most conventional processes are static in nature and have the following disadvantages: consuming a lot of sintering energy, long cycle life, short chamber life, complex operating steps, low production efficiency, uneven heating, and difficulty in controlling cooling time, so that the resulting battery materials are overheated or underheated.
[0009] Therefore, there is an urgent need for an improved method and system to mass-produce solid-state battery materials, especially properly crystallized solid-state electrolyte materials, to achieve high-power battery performance, high capacity, high energy density, long cycle life, and excellent thermal stability. Summary of the invention
[0010] Embodiments of the present invention generally provide solid-state battery materials, methods and systems for producing solid-state battery materials. One embodiment of the present invention provides a method for producing a solid-state electrolyte (SSE) material, the method comprising: causing a first flow of a first gas to flow in a controlled stoichiometric amount of a lithium-containing salt, a material containing one or more metals D 1 , D 2 ,…,D N A liquid mixture of one or more inorganic salts is mixed to form a gas-liquid mixture and a mist of the liquid mixture is sprayed into a power spray chamber at a high power velocity, and a second gas stream of heated gas is delivered into the power spray chamber. 1 , D 2 ,…,D N Examples include La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br, and combinations thereof.
[0011] The method also includes drying the gas-liquid mixture for a first reaction time period of less than 20 minutes, performing one or more oxidation reactions in the presence of a second gas stream and forming a gas-solid mixture, conveying the gas-solid mixture out of the kinetic jet chamber, separating the gas-solid phase mixture into one or more solid particles of SSE material, and conveying the one or more solid particles to an annealing chamber. In one example, the first reaction time is less than 3 minutes. In another example, the powdered particles are annealed in the presence of an oxygen stream during a dynamic crystallization process.
[0012] Next, the method further comprises annealing the one or more solid particles of the SSE material for a second reaction period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas stream and obtain a crystallized product. The method optionally comprises grinding the crystallized product of the ceramic material to obtain nano-sized particles.
[0013] In one embodiment, the method further comprises sintering the crystallized product of the ceramic material at an annealing temperature above 900° C. to further process the ceramic material, and measuring the ionic conductivity of the ceramic material.
[0014] Examples of ceramic SSE materials include Li 7 La 3 Zr 2 O 12 , Li doped with one or more metals 7 La 3 Zr 2 O 12 , Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 2 Al 0.25 O 12 , Li 6.5 La 3 Zr 2 Al 0.24 O 12 , Li 6.5 La 3 Zr 2 Al 0.22 O 12 , Li 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35 , Li 6.74 La 2.96 Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.45 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.27 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.22 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.3 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.39 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.4 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 2.86 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.24 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 11.98 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.43 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 2.93 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.24 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.08 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.32 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.2 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.46 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.9 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.57 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 2.99 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.22 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.22 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.4 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.54 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 2.82 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.24 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.08 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.49 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.28 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.31 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.7 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.28 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.24 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.25 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.01 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.22 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 11.92 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.49 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.02 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.23 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.2 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.5 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 1.5 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.5 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.15 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 1.75 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.25Al 0.2 O 12 , Li 6.25 La 3 Zr 2 Al 0.25 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.25 La 3 Zr 2 Ta 0.25 Ga 0.2 O 12 , Li 6.4 La 3 Zr 2 Ga 0.2 O 12 , Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 , Li 5 La 3 Nb 2 O 12 , Li 5 La 3 Ta 2 O 12 , Li 5 La 3 Ti 2 O 12 , Li 6 La 3 Sr 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ti 2 O 12 , Li 1.26 La 2.24 Ti 4 O 12 , Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2.24 Ti3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 , Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 and combinations thereof.
[0015] In one embodiment, the crystallized product of the SSE material is in the form of spherical clusters under scanning electron microscopy (SEM) analysis. In another embodiment, the tap density of the SSE material is greater than 1.0 g / ml. For example, after annealing the SSE material at more than 900° C. for more than 8 hours, the tap density of the SSE material is greater than 1.4 g / ml.
[0016] In yet another embodiment, the ionic conductivity (σ) of the SSE material is greater than 10 at 25°C. -4S / cm. One example of the crystallized product is a garnet-type ceramic material having a cubic structure as measured by X-ray diffraction (XRD) analysis. In another example, the liquid mixture contains a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and the crystallized product of the SSE material as measured by XRD analysis is a garnet-type ceramic material having a cubic structure. In yet another example, the liquid mixture contains a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and an aluminum-containing salt, and the crystallized product of the SSE material as measured by XRD analysis is a garnet-type ceramic material having a cubic structure. Another example of the liquid mixture contains a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and the crystallized product of the SSE material as measured by XRD analysis is a garnet-type ceramic material having a tetragonal structure.
[0017] In yet another embodiment, the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a tantalum-containing salt, and the crystallized product of the SSE material as measured by XRD analysis is a garnet-type ceramic material having a cubic structure. Another example of a liquid mixture comprises a lithium-containing salt, an aluminum-containing salt, a phosphorus-containing salt, and the crystallized product of the SSE material as measured by XRD analysis is a sodium superionic conductor (NASICON)-type ceramic material having a hexagonal structure.
[0018] In another embodiment, the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a titanium-containing salt, and the crystallized product of the SSE material is a perovskite-type ceramic material. Still further, the liquid mixture comprises a lithium-containing salt, a germanium-containing salt, and the SSE material is a ceramic material. In another embodiment, the liquid mixture comprises a lithium-containing salt, a sulfur-containing salt, and the SSE material is a sulfide material.
[0019] One embodiment of the present invention includes a method of producing a solid electrolyte ceramic material having a temperature greater than 10°C. -4 S / cm measurement of ionic conductivity (σ) and Li a La b Zr c D1 d D2 e …DN n O v The chemical composition of the present invention is as follows: 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and D 1 , D 2 ,…,D N At least one of the above is a metal, N≥0, 0≤d≤0.8, 0≤e≤0.8, and 0≤n≤0.8. The method comprises: forming a stoichiometric amount of a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and a salt containing one or more metals D 1 , D 2 ,…,DN A liquid mixture of one or more inorganic metal salts of the present invention is prepared by mixing with a first gas stream to form a gas-liquid mixture, spraying a mist of the liquid mixture into a power jet chamber; and drying the gas-liquid mixture for a first reaction period of less than 20 minutes to perform one or more oxidation reactions in the presence of a second gas stream of heated gas and form a gas-solid mixture. Next, the gas-solid mixture is transported out of the power jet chamber and the gas-solid mixture is separated into one or more solid particles of the SSE material. Then, the one or more solid particles are transported to an annealing chamber, and the one or more solid particles of the SSE material are annealed for a second reaction period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas stream, thereby obtaining a final crystalline product of the SSE material.
[0020] Another embodiment of the present invention provides a solid electrolyte material, wherein the solid electrolyte material comprises a chemical composition of Li a La b Zr c D1 d D2 e …DN n O v Ceramic material, wherein 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and wherein D 1 , D 2 ,…,D N At least one of them is a metal, N≥0, 0≤d≤0.8, 0≤e≤0.8, and 0≤n≤0.8. The SSE material is synthesized on a large scale by a method comprising: forming a numerically controlled stoichiometric amount of a liquid mixture containing a lithium salt, a lanthanum salt, a zirconium salt, and one or more inorganic salts containing one or more metals. The method also includes mixing the liquid mixture with a first gas stream to form a gas-liquid mixture, spraying a mist of the gas-liquid mixture into a power jet chamber at a high speed, drying the gas-liquid mixture for a first reaction time period of less than 20 minutes to perform one or more oxidation reactions by conveying a second gas stream of heated gas and forming a gas-solid mixture in the power jet chamber, conveying the gas-solid mixture out of the power jet chamber to obtain powdered particles of a ceramic material; and annealing the powdered particles for a second reaction time period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas stream and form a crystalline product, wherein the crystalline product of the ceramic material is clustered under SEM analysis, wherein D 1 , D 2 ,…,D NSelected from the group consisting of Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br and combinations thereof.
[0021] In one example, the method for preparing a solid electrolyte material further comprises grinding a crystallized product of a ceramic material to obtain nano-sized particles, wherein the tap density of the ceramic material is greater than 1.0 g / ml. In another example, the method further comprises sintering the crystallized product of the ceramic material at an annealing temperature above 900° C. to further process the ceramic material; and measuring the ionic conductivity of the ceramic material. In yet another example, as measured by XRD analysis, the crystallized product of the solid electrolyte material obtained from the present invention is a garnet-type ceramic material having a cubic structure and having an ionic conductivity (σ) greater than 10 at 25° C. -4 S / cm.
[0022] Another embodiment of the present invention provides a solid electrolyte material, wherein the solid electrolyte material comprises a chemical composition of Li a La b Zr c Al d D1 e …DN n Ov ceramic material, wherein 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and wherein D 1 ,…,D N At least one of the above is a metal, N≥0, 0≤d≤0.8, 0≤e≤0.8, and 0≤n≤0.8, and is synthesized by a method comprising: forming a liquid mixture of a stoichiometric amount of a lithium salt, a lanthanum salt, a zirconium salt, and one or more inorganic salts, wherein the one or more inorganic salts include one or more metal D 1 , D 2 ,…,D N ; spraying a mist of the liquid mixture into a power jet chamber by mixing the liquid mixture with a first gas stream at a high speed to form a gas-liquid mixture; drying the gas-liquid mixture for a first reaction time period of less than 20 minutes to carry out one or more oxidation reactions by delivering a second gas stream of heated gas and forming a gas-solid mixture in the power jet chamber; delivering the gas-solid mixture out of the power jet chamber to obtain powdered particles of the ceramic material; and annealing the powdered particles for a second reaction time period of more than 2 hours to carry out a dynamic crystallization process in the presence of a third gas stream and form a crystalline product.
[0023] In another embodiment, a solid electrolyte material is synthesized by a method comprising: forming a liquid mixture of a controlled stoichiometric amount of a lithium salt, a lanthanum salt, a zirconium salt, and one or more inorganic salts, wherein the one or more inorganic salts contain one or more metal D 1 , D 2 ,…,D N ; spraying a mist of the liquid mixture into a power spray chamber to mix with a first gas stream to form a gas-liquid mixture; drying the lithium salt, the lanthanum salt and the zirconium salt together for a first reaction time period of less than 20 minutes to perform one or more oxidation reactions and form powdered particles of the ceramic material by conveying a second gas stream of heated gas; and annealing the powdered particles for a second reaction time period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas stream and form a crystalline product of the ceramic material, wherein the final crystalline product of the ceramic material is in the form of clusters under SEM analysis, and wherein the crystalline product is a garnet-type ceramic material having a cubic structure as measured by XRD analysis, and its ionic conductivity (σ) measured at 25° C. is greater than 10 -4 S / cm.
[0024] Various solid electrolyte materials that can be formed using the method of the present invention include, but are not limited to, ceramic solid electrolyte materials, garnet-type solid oxide electrolyte materials, lithium lanthanum zirconium oxide materials, Li 6 ALa 3 Ta 2 O 12 (A=Sr、Ba)、NASICON(NaM 2 (PO 4 ) 3 M=Ge, Ti, Zr), LLTO perovskite-type electrolyte, synthesis and transport properties of two-dimensional Li x M 1 / 3 Nb 1-x Ti x O 3 (M=La, Nd) perovskite (ABO 3 ) type oxides, lithium superionic conductor (LISICON) type structured oxide electrolytes, lithium phosphorus oxynitride (LiPON)) and combinations thereof. In addition, the method of the present invention can be used to synthesize and form solid sulfide electrolyte materials such as Argyrodit electrolytes, lithium phosphorus sulfide (Li 3 PS 4 , LPS) electrolyte, Li 7 P 3 S 11 , Li 7 P 2 S 8, Li 11-x M 2-x P 1+x S 12 (M=Ge, Sn, Si) (LGPS) type structure: LGPS and its combination.
[0025] The present invention also provides a method for manufacturing a solid-state battery by forming an anode material layer, a solid electrolyte material layer and a cathode material layer, wherein one or more of the anode material layer, the solid electrolyte material layer, the cathode material layer or a combination thereof comprises a material prepared by the method of the present invention. The material formed by the method of the present invention can be a ceramic solid electrolyte material, a garnet-type solid oxide electrolyte material, a lithium lanthanum zirconium oxide material, a Li 6 ALa 3 Ta 2 O 12 (A=Sr、Ba)、NASICON(NaM 2 (PO 4 ) 3 M=Ge, Ti, Zr), LLTO perovskite-type electrolyte, synthesis and transport properties of two-dimensional Li x M 1 / 3 Nb 1-x Ti x O 3 (M=La, Nd) perovskite (ABO 3 ) type oxides, lithium superion conductor (LISICON) type structured oxide electrolytes, lithium phosphorus oxynitride (LiPON)) and combinations thereof. In addition, solid sulfide electrolyte materials such as Argyrodit electrolytes, lithium phosphorus sulfide (Li 3 PS 4 , LPS) electrolyte, Li 7 P 3 S 11 , Li 7 P 2 S 8 , Li 11-x M 2-x P 1+x S 12 (M=Ge, Sn, Si) (LGPS) type structure: LGPS and its combination.
[0026] As an example, the material formed by the method of the present invention can be used as a material in a solid electrolyte material layer. As another example, the material formed by the method of the present invention can be used as a material for coating (e.g., using a dry coating process and / or a wet coating process) a cathode material. The resulting cathode material coated with a solid electrolyte material can be used to form a cathode material layer. Such coated cathode materials can be used to manufacture solid-state batteries together with conventional solid electrolyte materials or using solid electrolyte materials formed by the method of the present invention.
[0027] In one embodiment, a solid electrolyte material containing lithium (Li) and one or more metals is synthesized by forming a stoichiometric liquid mixture containing a lithium salt and one or more metal salts, and spraying the liquid mixture into a power jet reactor for a lithium salt and one or more metal salts to oxidize these salts together at a high temperature of 350°C to 1200°C for only a few minutes to react rapidly and form the final product of the reaction of the solid electrolyte material.
[0028] An example of a solid electrolyte material is lithium lanthanum zirconium oxide (Li 7 La 3 Zr 2 O 12 ) (LLZO) material. The LLZO solid material is obtained by forming a lithium-containing salt (e.g., lithium nitrate (La(NO 3 ) 3 )、Lanthanum nitrate (La(NO) 3 ) and a liquid mixture of one or more metal-containing salts, and spraying the liquid mixture into a power jet reactor so that the lithium-containing salt and the one or more metal-containing salts react together in less than 30 minutes, and react rapidly, and form a reaction final product of a solid electrolyte material. The resulting solid electrolyte material exhibits a crystalline structure comparable to that of a solid electrolyte material prepared by an existing solid phase reaction and / or reaction-gelation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to understand in detail the manner in which the above-recorded features of the present invention are described in more detail with reference to embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the accompanying drawings illustrate only typical embodiments of the present invention and are therefore not to be considered as limiting the scope thereof, as the present invention may admit of other equally effective embodiments.
[0030] Figure 1A is a cross-sectional view of an exemplary solid-state battery according to one embodiment of the present invention.
[0031] Figure 1Bis a cross-sectional view of an exemplary solid-state battery according to another embodiment.
[0032] Figure 1C is a cross-sectional view of an exemplary solid-state battery according to another embodiment.
[0033] Figure 1D is a cross-sectional view of an exemplary solid-state battery according to another embodiment.
[0034] Figure 2 One embodiment of a method of producing a battery material is illustrated.
[0035] Figure 3 is another embodiment of a method of producing a battery material.
[0036] Figure 4 Another embodiment of a method of wet coating a battery material with another material is illustrated.
[0037] Figure 5 Another embodiment of a method of dry coating a battery material with another material is illustrated.
[0038] Figure 6 is a schematic diagram of an exemplary processing system for preparing materials for a battery electrochemical cell according to one embodiment of the present invention.
[0039] Figure 7 is a schematic diagram of another exemplary processing system according to another embodiment.
[0040] Fig. 8A is a perspective view of one embodiment of a processing system for producing battery particulate material.
[0041] Figure 8B is a cross-sectional view of another embodiment of a processing system for producing particulate material.
[0042] Figure 8C Another embodiment of an exemplary motive jetting module disposed in a dispersion chamber of a processing system is illustrated in perspective view.
[0043] Fig.8D An exemplary motive jetting module configured in a processing system according to another embodiment is illustrated.
[0044] Fig. 8E An exemplary motive jetting module according to another embodiment is illustrated in perspective view.
[0045] Figure 8F An exemplary motive jetting module configured in a processing system is illustrated in perspective.
[0046] Fig. 9An X-ray diffraction (XRD) pattern of an example of the crystallized solid electrolyte material of the present invention is shown.
[0047] Fig.10 An XRD pattern of an example of the crystallized solid electrolyte material of the present invention is shown.
[0048] Fig.11 is an XRD pattern of an exemplary crystalline solid electrolyte material of the present invention.
[0049] Fig.12 is an XRD pattern of another exemplary crystalline solid electrolyte material of the present invention.
[0050] Fig.13 is an XRD pattern of another exemplary crystalline solid electrolyte material of the present invention.
[0051] Fig.14A is a SEM image of exemplary solid particles of a solid-state electrolyte material after one or more annealing processes.
[0052] Fig. 14B is a SEM image of exemplary solid particles of the solid-state electrolyte material.
[0053] Fig. 14C is a SEM image of exemplary solid particles of the solid-state electrolyte material.
[0054] Fig.15A is a SEM image of exemplary solid particles of the solid-state electrolyte material.
[0055] Fig. 15B yes Fig.15A A higher magnification SEM image of an exemplary solid electrolyte material particle in FIG.
[0056] Fig.16A is a SEM image of an exemplary solid electrolyte material particle.
[0057] Fig. 16B yes Fig.16A A higher magnification SEM image of an exemplary solid electrolyte material particle in FIG.
[0058] Fig.17A is a SEM image of exemplary solid electrolyte material particles after one or more annealing processes.
[0059] Fig. 17B is a SEM image of another example of solid electrolyte material particles.
[0060] Fig. 17C is a SEM image of an exemplary solid electrolyte material particle.
[0061] Fig.17D is a SEM image of an exemplary solid electrolyte material particle. DETAILED DESCRIPTION
[0062] The present invention generally relates to compositions, battery oxide materials, battery SSE materials, devices and dynamic crystallization processes (DCP) thereof at appropriate molar solution ratios for precisely and digitally controlling the stoichiometric amount of metal material content and obtaining appropriate atomic level ratios of metal components and battery active materials for solid-state batteries. The battery materials, methods and devices provided herein produce high-purity, precisely stoichiometric phased battery cathode materials and can be used in turn to manufacture lithium-ion batteries having properties associated with high battery cycle performance, including high electrical capacity.
[0063] Solid-state batteries generally contain a positive electrode, a negative electrode, and a solid electrolyte / separator (i.e., a solid electrolyte can act as a separator between the positive electrode (i.e., cathode) and the negative electrode (i.e., anode)). The positive electrode generally contains a positive electrode active material (i.e., cathode material), and the negative electrode contains a negative electrode active material (i.e., anode material). The SSE in a solid-state battery can be a simple solid electrolyte material or a composite material of a polymer and SSE material. The cathode material can be LiCoO 2 (LCO), Li(Ni x Mn y Co z ) 2 (NMC), LiFePO 4 (LFP) or LiMn 2 O 4 (LMO), and in some cases intercalation binary oxides, while Li metal, Li-In alloys, graphite, Li 4 Ti 5 O 12 (LTO) or Si, Sn-Co-C mixed composite materials are used as anode materials. In addition, the electrode preparation technology of solid-state batteries is different from that of existing lithium-ion batteries.
[0064] Figure 1A An exemplary solid-state battery is shown, which shows an exemplary layer structure of a solid-state battery layer structure 10A according to one aspect of the present invention. The solid-state battery layer structure 10A includes a positive electrode layer 90A, a negative electrode layer 30A, and a solid electrolyte layer 50A sandwiched between the positive electrode layer 90A and the negative electrode layer 30A.
[0065] In one embodiment, the solid electrolyte layer 50A contains a solid electrolyte material 52A therein, which is used as follows: Figure 2 , 3, 6, 7, 8A, 8B, 8C, 8D, 8E, 8F or another suitable process according to one or more embodiments. In another embodiment, the positive electrode layer 90A contains a cathode active material 92A therein, and the cathode active material 92A can be used as follows in Figure 2 , 3 , 6, 7, 8A, 8B, 8C, 8D, 8E, 8F or another suitable process according to one or more embodiments. In addition, the negative electrode layer 30A contains an anode material 32A therein, which can be prepared using any suitable anode material preparation process and system.
[0066] Figure 1B Another example of a solid-state battery layer structure 10B according to one aspect of the present invention is shown. The solid-state battery layer structure 10B includes a positive electrode layer 90B, a negative electrode layer 30B, and a solid electrolyte layer 50B sandwiched between the positive electrode layer 90B and the negative electrode layer 30B. In one embodiment, the solid electrolyte layer 50B includes a solid electrolyte material 52B therein, and the solid electrolyte material 52B is used as follows Figure 2 , 3 , 6, 7, 8A, 8B, 8C, 8D, 8E, 8F or prepared according to another suitable process of one or more embodiments. In addition, the negative electrode layer 30B contains the anode material 32B therein, and the solid electrolyte layer 50B contains the solid electrolyte material 52B prepared according to the method and system of the present invention.
[0067] In another embodiment, the positive electrode layer 90B comprises a mixture of cathode active material 92B and solid electrolyte material 94B, wherein they are prepared according to the method and system of the present invention. The cathode active material 92B and the solid electrolyte material 94B can be mixed together by a blending method using a blender or any other suitable device. It is envisioned that the solid electrolyte material 94B is included in the positive electrode layer 90B to contribute to the conductivity of the cathode active material 92B within the solid-state battery layer structure 10B.
[0068] Figure 1C An exemplary solid-state battery, a solid-state battery layer structure 10C according to one aspect of the present invention is shown. The solid-state battery layer structure 10C includes: a positive electrode layer 90C having a coated cathode active material 92C therein, a negative electrode layer 30C having an anode material 32C therein, and a solid electrolyte layer 50C sandwiched between the positive electrode layer 90C and the negative electrode layer 30C. In one embodiment, the solid electrolyte layer 50C includes a solid electrolyte material 52C therein, which is used as follows in Figure 2 ,3 , 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or prepared by another suitable process according to one or more embodiments.
[0069] In another embodiment, the coated cathode active material 92C is prepared according to one or more embodiments of the present invention and comprises particles of cathode active material 96C (e.g., battery cathode material prepared using the methods and systems of the present invention or any other suitable battery cathode material, etc.) coated with an outer layer of solid electrolyte material 94C (e.g., battery SSE material prepared using the methods and systems of the present invention or any other suitable battery SSE material, etc.). Figure 4 and 5 The coating of the particles of the cathode active material 96C with the solid electrolyte material 94C may be performed using the methods and systems described in, or another suitable dry coating or wet coating process. It is contemplated that the blending of the particles of the solid electrolyte material 94C with the cathode active material 96C within the coated cathode active material 92C helps promote conductivity within the solid-state battery layer structure 10C.
[0070] Figure 1D Another example of a solid-state battery layer structure 10D is shown, which includes a positive electrode layer 90D, a negative electrode layer 30C having an anode material 32D therein, and a solid electrolyte layer 50D sandwiched between the positive electrode layer 90D and the negative electrode layer 30D. According to one or more embodiments, the solid electrolyte layer 50D includes a solid electrolyte material 52D, which is used as follows in Figure 2 , 3 , 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or prepared by another suitable process according to one or more embodiments.
[0071] In one embodiment, the positive electrode layer 90D comprises a mixture of a coated cathode active material 92D and a solid electrolyte material 98D, wherein they are mixed by a blending method using a blender or any other suitable device. In another embodiment, the coated cathode active material 92D is prepared using the methods and systems described herein according to one or more embodiments of the present invention. For example, the coated cathode active material 92D can include particles of a cathode active material 96D coated with an outer layer of a solid electrolyte material 94D (e.g., a battery SSE material prepared using the methods and systems of the present invention or any other suitable battery SSE material, etc.). Using as described below in Figure 4 and Figure 5Coating of particles of cathode active material 96D with solid electrolyte material 94D may be performed using the methods and systems described in, or another suitable dry coating or wet coating process.
[0072] exist Figures 1A-1D In the solid-state battery layer structure, the thickness of the positive electrode layer, the solid electrolyte layer and the negative electrode layer is not particularly limited. For example, the solid-state battery layer structure 10A, 10B, 10C, 10D may include one or more solid electrolyte layers (e.g., 2-3 or 10 layers of SSE layers, etc.) sandwiched between the positive electrode layer 90A, 90B, 90C, 90D and the negative electrode layer 30A, 30B, 30C, 30D.
[0073] Embodiments of the present invention provide for preparing solid electrolyte materials 52A, 52B, 52C, 52D, 94B, 94C, 94D, 98D and cathode active materials 92A, 92B, 96C, 96D using the methods and systems of the present invention as described below or another suitable process, which can be used to manufacture and synthesize solid-state batteries. Additional embodiments for producing solid electrolyte materials or cathode active materials can be found in U.S. Patent Application Nos. 13 / 900,915, 16 / 114,114, 16 / 747,450, 17 / 319,974, 17 / 319,974, 17 / 901,796, 13 / 901,035, 16 / 104,841, 17 / 133,478, 17 / 970,342, 13 / 901,121, 15 / 846,094, 16 / 679,085, and 17 / 899,048, and the disclosures of each of the above patent applications are incorporated herein in their entirety.
[0074] In one embodiment, the solid electrolyte material in the solid-state battery according to one aspect of the present invention includes solid electrolyte layers 50A, 50B, 50C, 50D including solid electrolyte materials 52A, 52B, 52C, 52D. In another embodiment, the positive electrode layer in the solid-state battery may also include both cathode active materials and solid electrolyte materials, and the solid electrolyte material is mixed with the cathode active material by direct blending, dry coating or wet coating process.
[0075] In another embodiment, a solid electrolyte material (e.g., Figures 1A-1D Examples of the solid electrolyte materials 52A, 52B, 52C, 52D, 94B, 94C, 94D, 98D) shown may include, but are not limited to: oxide-based solid electrolytes, garnet-type solid electrolytes, sodium superionic conductor (NASICON) type (NaM 2 (PO 4 ) 3M=Ge, Ti, Zr) structure (for example, lithium aluminum titanium phosphate material, Li(Al,Ti) 2 (PO 4 ) 3 , LTAP, such as Li 1.5 Al 0.5 Ti 1.5 P 3 O 12 , Li 1.4 Al 0.4 Ti 1.6 P 3 O 12 , Li 1.6 Al 0.6 Ti 1.4 P 3 O 12 etc.), perovskite-type solid electrolytes (e.g., Li x La y TiO 3 , LLTO, etc.), two-dimensional Li x M 1 / 3 Nb 1-x Ti x O 3 (M=La, Nd) perovskite (ABO 3 ) type oxide, Li 1.5 Al 0.5 Ge 1.5 P 3 O 12 , Li 1.4 Al 0.4 Ge 1.6 P 3 O 12 , Li 1.6 Ge 0.6 Ti 1.4 P 3 O 12 , Li 12 Ge 0.5 Al 1.0 Si 0.5 P 1.0 O 12 , Li 10.59 Ge 1.58 V 0.9 P 0.53 O 12 , sulfide SSE electrolyte materials (such as Li 7 P 3 S 11 , Li 3 P 1 S 4 , Li 6 P1 WITH 5 Cl、Li 6 P 1 WITH 5 No. 1 、Li 6 P 1 WITH 5 l、Li 6 P 1 WITH 5 F 1 、Li 7 P 2 WITH 8 AND 1 、Li 7 P 2 WITH 8 No. 1 、Li 7 P 2 WITH 8 Cl 1 、Li 7 P 2 WITH 8 F 1 、Li 15 P 4 WITH 16 Cl 3 、Li 14.8 Mg 0.1 P 4 WITH 16 Cl 3 、Li 9.54 Yes 1.74 P 1.44 WITH 11.7 Cl 0.3 、Li 10 Ge 1 P 2 WITH 12 、Li 10 Yes 1 P 2 WITH 12 、Li 10 Sn 1 P 2 WITH 12 、Li 10 Yes 0.3 Sn 0.7 P 2 WITH 12 、Li 10 Al 0.3 Sn 0.7 P 2 WITH 12 、Li 11 Al 1 P 2 WITH12 , Li 10 SiP 2 S 11.3 O 0.7 , Li 9.42 Si 1.02 P 2.1 S 9.96 O 2.04 etc.), lithium superion conductor (LISICON) type structured oxide electrolytes, amorphous thin film solid electrolytes (e.g., lithium phosphorus oxynitride (LiPON), Li 2.88 P 1.0 O 3.73 N 0.14 , Li 1.9 Si 0.28 P 1.0 O 1.1 N 1.0 etc.), Argentum-type solid electrolytes, lithium phosphosulfide (Li 3 PS 4 , LPS) solid electrolyte, Li 7 P 3 S 11 , Li 7 P 2 S 8 , Li 11-x M 2-x P 1+x S 12 (M=Ge, Sn, Si, etc.) (LGPS) type structure, lithium-argyrodite type solid electrolyte (e.g., Li x PS y X (wherein X = Cl, Br or I), Li 6 PS 5 Cl, Li 6 PS 5 Br, Li 6 PS 5 I, etc.) and combinations thereof.
[0076] The SSE material can be an undoped SSE material or an SSE material doped with one or more metals or other atoms (e.g., La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, P, S, Os, Ir, Au, F, Cl, I, Br, and combinations thereof, etc.), such as those lithium oxide-based garnet-type SSE materials doped with Al, Ge, Ti, Ta, etc.
[0077] like Figures 1A-1DExamples of the solid electrolyte materials 52A, 52B, 52C, 52D, 94B, 94C, 94D, 98D shown may include, but are not limited to: one or more lithium-containing garnet-type oxide-based solid electrolyte (SSE) materials having a cubic or tetragonal crystal structure, lithium lanthanum zirconium oxide garnet, lithium lanthanum zirconium oxide garnet doped with Al, Ge, Ti, Ta, etc., such as Li 7 La 3 Zr 2 O 12 , Li doped with one or more metals 7 La 3 Zr 2 O 12 , Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 2 Al 0.25 O 12 , Li 6.5 La 3 Zr 2 Al 0.24 O 12 , Li 6.5 La 3 Zr 2 Al 0.22 O 12 , Li 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35 , Li 6.74 La 2.96 Zr 2.0 Al 0.25 O 12.45 , Li 6.27 La 3.22 Zr 2.0 Al 0.3 O 12.39 , Li 6.4 La 2.86 Zr 2.0 Al 0.24 O 11.98 , Li 6.43 La 2.93 Zr 2.0 Al 0.24 O 12.08 , Li 6.32 La 3.2 Zr 2.0 Al 0.46 O<h2 style=";text-align:left;direction:ltr"> 12.9 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.57 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 2.99 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.22 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.22 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.4 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.54 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 2.82 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.24 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.08 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.49 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.28 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.31 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.7 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.28 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.24 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.25 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.01 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.22 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 11.92 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.49 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3.02 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2.0 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.23 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12.2 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.5 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 1.5 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.5 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.15 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 1.75 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.25 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.15 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 1.75 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> Ga<h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.25 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> Ga<h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.4 <h2 style=";text-align:left;direction:ltr"> No<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 2Ga 0.2 O 12 , Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 , Li 5 La 3 Nb 2 O 12 , Li 5 La 3 Ta 2 O 12 , Li 5 La 3 Ti 2 O 12 , Li 6 La 3 Sr 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ti 2 O 12 , Li 1.26 La 2.24 Ti 4 O 12 , Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 , Li1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 and combinations thereof.
[0078] In one embodiment, the chemical composition of the solid electrolyte material may be Li a La b Zr c D1 d D2 e …DN n O v , where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and D 1 , D 2 ,…D N At least one of them is a metal, N ≥ 0, 0 ≤ d ≤ 0.8, 0 ≤ e ≤ 0.8, and 0 ≤ n ≤ 0.8, wherein D 1 , D 2 ,…,D N Selected from the group consisting of Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br and combinations thereof. For example, the solid electrolyte material is a garnet-type lithium lanthanum zirconium oxide material, including Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 1.5 Ta 0.5 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li 6.25 La 3 Zr 2 Al 0.25 O 12, Li 6.15 La 3 Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.25 La 3 Zr 2 Ta 0.25 Ga 0.2 O 12 .
[0079] In another embodiment, the solid electrolyte material is Li a La b D1 c D2 d …DN n O v , where 4.5≤a≤7.2, 2.8≤b≤3.5, 1.5≤c≤2.5, 0≤d≤1.2, 0≤n≤1.2, and 2≤v≤12, and D 1 , D 2 ,…,D N At least one of them is a metal, and N ≥ 1. For example, the solid electrolyte material can be Li 5 La 3 Nb 2 O 12 , Li 5 La 3 Ta 2 O 12 , Li 5 La 3 Ti 2 O 12 , Li 6 La 3 Sr 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ti 2 O 12 , Li 1.26 La 2.24 Ti 4 O 12 In another example, the chemical composition of the solid electrolyte material is Li a Al b P c D1 d…DN n O v , where 1≤a≤2, 0.2≤b≤1.5, 1.0≤c≤3.5, 0≤d≤2.0, 0≤n≤2.0, and 0.2≤v≤12, and where D 1 , D 2 ,…,D N At least one of them is a metal, and N ≥ 1; for example, and Li 1.5 Al 0.5 Ti 1.5 P 3 O 12 , Li 1.5 Al 0.5 Ge 1.5 P 3 O 12 .
[0080] In another embodiment, the chemical composition of the solid electrolyte material can be Li a P b S c D1 d …DN n X v , where 5≤a≤16, 0.5≤b≤4.5, 3≤c≤16, 0≤d≤1.5, 0≤n≤1.5, O≤v≤4, and D 1 , D 2 ,…,D N At least one of is a metal, N ≥ 0 and X is a halogen; for example, Li 7 P 3 S 11 , Li 3 P 1 S 4 , Li 6 P 1 S 5 Cl, Li 6 P 1 S 5 Br 1 , Li 6 P 1 S 5 I. Li 6 P 1 S 5 F 1 , Li 7 P 2 S 8 I 1 , Li 7 P 2 S 8 Br 1 , Li 7 P2 S 8 Cl 1 , Li 7 P 2 S 8 F 1 , Li 15 P 4 S 16 Cl 3 , Li 14.8 Mg 0.1 P 4 S 16 Cl 3 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 Ge 1 P 2 S 12 , Li 10 Si 1 P 2 S 12 , Li 10 Sn 1 P 2 S 12 , Li 10 Si 0.3 Sn 0.7 P 2 S 12 , Li 10 Al 0.3 Sn 0.7 P 2 S 12 , Li 11 Al 1 P 2 S 12 In another embodiment, the solid electrolyte material is Li a Ge b P c D1 d …DN n O v , where 10≤a≤13, 0.1≤b≤2.0, 0.1≤c≤1.5, 0.1≤d≤2.0, 0.1≤n≤2.0, 2≤v≤12, and D 1 , D2, …, D N At least one of them is a metal, N ≥ 0, N ≥ 0; for example, Li 12 Ge 0.5 Al 1.0 Si 0.55 P 1.0 O12 , Li 10.59 Ge 1.58 V 0.9 P 0.53 O 12 In one embodiment, the lithium ion (Li+) conductivity of the solid electrolyte is 0.01 to 10 mS / cm at 300 K. The obtained solid electrolyte material can be further processed into powders of smaller sizes (e.g., by jet milling or other milling techniques) to obtain nano-sized particles of the solid electrolyte material.
[0081] exist Figures 1A-1D In the embodiment, the cathode active materials 92A, 92B, 94C, 94D may be used as Figure 2-8F The metal oxide material prepared by the method and system of the present invention described in or other suitable processes, and may include a lithium oxide material with an embedded metal, preferably with three or four embedded metals. Exemplary cathode active materials are metal oxide materials containing one or more lithium (Li), nickel (Ni), manganese (Mn), cobalt (Co), aluminum (Al), titanium (Ti), sodium (Na), potassium (K), rubidium (Rb), vanadium (V), cesium (Cs), copper (Cu), magnesium (Mg), iron (Fe), etc. In addition, the cathode material can present a crystal structure of a metal in the shape of a layer, spinel, olivine, etc. In addition, the cathode active materials 92A, 92B, 94C, 94D are typically solid powders with a particle size ranging from 10nm to 100um.
[0082] Exemplary cathode active materials include, but are not limited to, lithium transition metal oxides (LiMeO 2 ), lithium titanium oxide (e.g., Li 4 Ti 5 O 12 ), lithium cobalt oxide (e.g., LiCoO 2 ), lithium manganese oxide (e.g., LiMn 2 O 4 ), nickel lithium oxide (e.g., LiNiO 2 ), olivine-type lithium metal phosphates (e.g., LiFePO 4 、LiNiPO 4 、LiCoPO 4 、LiMnPO 4 , Li 3 Fe 2 (PO 4 ) 3 and Li 3 V 2 (PO 4 ) 3 ), sodium iron oxide (e.g., NaFe2 O 3 ), sodium iron phosphate (such as NaFeP 2 O 7 ) etc. Including but not limited to lithium nickel cobalt oxide (e.g., Li x Ni y Co z O 2 ), lithium nickel manganese oxide (e.g., Li x Ni y Mn z O 2 , Li x Ni y Mn z O 4 、LiCoMnO 4 , Li 2 NiMn 3 O 8 etc.), lithium nickel manganese cobalt oxide (for example, Li a Ni b Mn c Co d O e ; and / or LiNi x Mn y Co z O 2 , NMC oxide materials, where x+y+z=1, such as LiNi 0.33 Mn 0.33 Co 0.33 O 2 、LiNi 0.9 Mn 0.05 Co 0.05 O 2 、LiNi 0.6 Mn 0.2 Co 0.2 O 2 、LiNi 0.5 Mn 0.3 Co 0.2 O 2 、LiNi 0.4 Mn 0.4 Co 0.2 O 2 、LiNi 0.7 Mn 0.15 Co 0.15 O 2 、LiNi 0.8 Mn 0.1 Co 0.1 O 2etc.; and / or mixed metal oxides with doped metals, etc. Other examples include lithium cobalt aluminum oxide (e.g., Li x Co y Al z O n ), lithium nickel cobalt aluminum oxide (e.g., Li x Ni y Co z Al a O b , such as LiNi 0.85 Co 0.1 Al 0.05 O 2 ), sodium iron manganese oxide (e.g., Na x Fe y Mn z O 2 ) etc. In another example, a mixed metal oxide with a doped metal is obtained; for example, Li a (Ni x Mn y Co z )MeO b (where Me = doping metal of Al, Mg, Fe, Ti, Cr, Zr or C), Li a (Ni x Mn y Co z )MeO b F c (where Me = doping metal of Al, Mg, Fe, Ti, Cr, Zr or C), etc. Other examples of cathode active materials can be found in U.S. Patent Application Nos. 13 / 900,915, 16 / 114,114, 16 / 747,450, 17 / 319,974, 17 / 319,974, 17 / 901,796, 13 / 901,035, 16 / 104,841, 17 / 133,478, 17 / 970,342, 13 / 901,121, 15 / 846,094, 16 / 679,085, 17 / 899,048, all of which are incorporated herein by reference in their entirety.
[0083] exist Figures 1A-1DIn the embodiment, the anode materials 32A, 32B, 32C, 32D can be alkali metals (such as lithium, sodium, potassium, etc.), other metals or transition metals (such as tantalum, titanium, zinc, iron, elements of Group 2 of the periodic table (such as magnesium, calcium, etc.), elements of Group 13 of the periodic table such as aluminum (Al), germanium (Ge), etc.), carbonaceous materials and / or metal alloys of two or more of the above metals. Exemplary anode materials include, but are not limited to, lithium metal, lithium alloys (such as lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys), lithium-containing metal oxides (such as lithium titanium oxide), lithium-containing metal sulfides, lithium-containing metal nitrides (such as lithium cobalt nitride, lithium iron nitride, lithium manganese nitride), and carbonaceous materials (such as graphite), carbon-based materials (such as lithium titanate (Li 4 Ti 5 O 12 )), SiO-based composites, SiO-Sn-Co / graphite (G) composites, Si, Sn-Co-C mixed composites and lithium coated with solid electrolyte.
[0084] Figure 2 1 is a flow chart of a digital dynamic crystallization process of a method 100 for producing battery materials for solid-state batteries. The method 100 includes flowing a first gas into a power jet chamber (e.g., as described below in Figure 6-8F In a step 120, the gas-liquid mixture is sprayed into a mist in a power jet chamber. The gas stream can be pumped through an air filter to remove any particles, droplets or contaminants, and the flow rate of the gas can be adjusted by a valve or other device. In one embodiment, the gas is heated to a temperature to mix with the mist and remove moisture from the mist. The first gas can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, an inert gas, a rare gas, and a combination thereof, and can be at room temperature or heated to, for example, about 40°C or more, such as about 80°C or more, for example 20°C to 200°C, or more than 50°C.
[0085] In one example, the mist of the liquid mixture is mixed with a carrier gas stream inside the mist generator before being delivered to the power jet chamber. In another example, the mist of the liquid mixture is mixed with a dry gas stream in the power jet chamber and carried through the power jet chamber for drying. In another example, the mist of the liquid mixture is mixed with a gas stream of gas in the mist generator to form a gas-liquid mixture. In addition, the liquid mixture is mixed with a gas stream of another gas in the power jet chamber. It is envisioned that these gas streams are provided to thoroughly mix the liquid mixture, thereby uniformly forming the mixture and facilitating the carrying of the gas-liquid mixture in the power jet chamber.
[0086] The liquid mixture may include a stoichiometric amount of a lithium-containing salt, one or more inorganic salts containing one or more metal D 1 , D 2 ,…,D N In one embodiment, D 1 , D 2 ,…,D N Selected from the group consisting of La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br and combinations thereof. In another embodiment, a lithium-containing salt is mixed with one or more salt-containing compounds M Li盐 :M 盐1 :M 盐2 :M 盐3 :…:M 盐N The molar ratio of is adjusted to a ratio of about a:b:c:...:n so that the battery material has a desired atomic ratio of Li salt:salt 1:salt 2:salt 3...:salt N equal to a:b:c:...:n. In one embodiment, a liquid mixture is prepared using stoichiometric amounts of a lithium-containing salt and one or more inorganic salts, which is then mixed with a gas. The salt is prepared into a solution, and the molar ratio of the solution containing the lithium salt to the solution of one or more inorganic metal salts is numerically controlled by the processing system of the present invention, thereby obtaining a large-scale synthesis of SSE materials.
[0087] Before and / or after the liquid mixture is positioned at the power jet chamber, the mist of the liquid mixture is mixed with the first gas stream to form a gas-liquid mixture. The mist is formed by the liquid mixture dissolved and / or dispersed in a suitable liquid solvent. One or more gas streams and the mist stream are mixed together to form a gas-liquid mixture. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, inert gas, rare gas and combination thereof etc. The gas can be pumped through an air filter to remove any particle, droplet or pollutant, and the flow rate of the gas can be regulated by a valve or other device.
[0088] For example, M Li盐 :M 盐1 :M 盐2 :M 盐3 :…:M 盐NThe desired molar ratio of can be achieved by measuring and preparing appropriate amounts of lithium-containing salt (Li salt), first salt (Salt 1), second salt (Salt 2), tri-salt (Salt 3), ... and N-th salt (Salt N) according to the final composition of the SSE to be synthesized. For example, the M of lithium-containing salt (Li salt), first salt (Salt 1), second salt (Salt 2), tri-salt (Salt 3), ... and N-th salt (Salt N) can be adjusted. Li盐 :M 盐1 :M 盐2 :M 盐3 :…:M 盐N The molar ratio M of the lithium salt (Li salt), the first salt (Salt 1), the second salt (Salt 2), the third salt (Salt 3), ..., and the Nth salt (Salt N) can be adjusted while forming the mist of the liquid mixture. li :M 盐1 :M 盐2 :M 盐3 :…:M 盐N Furthermore, the liquid form of one or more salt-containing compounds can be adjusted and directly prepared into a liquid mixture of the desired concentration.
[0089] The liquid form of the salt-containing compound can be dissolved or dispersed in a suitable solvent (e.g., water, alcohol, methanol, isopropyl alcohol, isopropanol, organic solvents, inorganic solvents, organic acids, sulfuric acid (H 2 SO 4 ), citric acid (C 6 H 8 O 7 ), acetic acid (CH 3 COOH), butyric acid (C 4 H 8 O 2 ), lactic acid (C 3 H 6 O 3 ), nitric acid (HNO 3 ), hydrochloric acid (HCl), ethanol, pyridine, ammonia, acetone and combinations thereof) to form a liquid mixture in the form of an aqueous solution, a slurry, a gel, an aerosol or any other suitable liquid. Moreover, the appropriate salt-containing compound can be selected depending on the desired composition of the final solid product particles containing the lithium salt by measuring and preparing an appropriate amount and the inorganic salt compound in a container containing an appropriate amount of solvent. Depending on the solubility of the lithium-containing salt and the inorganic salt in the selected solvent, the pH, temperature, and mechanical stirring and mixing can be adjusted to obtain a liquid mixture in which the lithium-containing salt and one or more metal-containing inorganic salts of the desired molar concentration are completely dissolved and / or uniformly dispersed.
[0090] Exemplary lithium-containing salts include, but are not limited to, lithium sulfate (Li 2 SO 4 ), lithium nitrate (LiNO 3 )、Lithium carbonate (Li 2 CO 3 ), lithium acetate (LiCH 3 COO), lithium hydroxide (LiOH), lithium formate (LiCHO 2 ), lithium chloride (LiCl), and combinations thereof. Exemplary inorganic salts include, but are not limited to, lithium sulfate (Li 2 SO 4 ), lithium nitrate (LiNO 3 )、Lithium carbonate (Li 2 CO 3 ), lithium acetate (LiCH 3 COO), lithium hydroxide (LiOH), lithium formate (LiCHO 2 ), lithium chloride (LiCl), lanthanum trichloride (LaCl 3 ), lanthanum acetate (C 6 H 9 LaO 6 ) and lanthanum nitrate (La(NO 3 ) 3 ), lanthanum sulfate (La 2 (SO 4 ) 3 ), lanthanum formate (C 3 H 3 LaO 6 ), cobalt sulfate (CoSO 4 ), cobalt nitrate (Co(NO 3 ) 2 ), cobalt acetate (Co(CH 3 COO 2 ), cobalt formate (Co(CHO 2 ) 2 ), cobalt chloride (CoCl 2 ), magnesium nitrate (Mg(NO 3 ) 2 )、Zr(NO 3 ) 4 ), zirconium acetate (C 8 H 12 O 8 Zr), zirconium chloride (ZrCl 4 )、Zr(SO 4 ) 2 ), zirconium formate (C 4 H 4 O 8 Zr), titanium nitrate (Ti(NO3 ) 4 ), titanium sulfate (Ti(SO 4 ) 2 、Ti(CO 3 ) 2 ), titanium acetate (Ti(CH 3 COO 4 ), titanium hydroxide (Ti(OH) 4 ), titanium formate (Ti(HCOO) 4 ), titanium chloride (TiCl 4 ), ammonium phosphate (NH 4 ) 3 PO 4 ), magnesium acetate (MgAc, Mg(CH 3 COO 2 ), magnesium chloride (MgCl 2 ), magnesium sulfate (MgSO 4 ), magnesium formate (C 2 H 2 MgO 4 ), aluminum nitrate (Al(NO 3 ) 3 ), aluminum acetate (AlAc, C 6 H 9 AlO 6 ), aluminum chloride (AlCl 3 ), aluminum sulfate (Al 2 (SO 4 ) 3 ), aluminum formate (Al(HCOO) 3 ), manganese sulfate (MnSO4), manganese nitrate (Mn(NO 3 ) 2 ), manganese acetate (Mn(CH 3 COO 2 ), manganese formate (Mn(CHO 2 ) 2 ), manganese chloride (MnCl 2 ), nickel sulfate (NiSO 4 ), nickel nitrate (Ni(NO 3 ) 2 ), nickel acetate (Ni(CH 3 COO 2 )、nickel formate (Ni(CHO 2 ) 2 ), nickel chloride (NiCl 2 ), titanium nitrate (TiO(NO 3 ) 2), (P)-containing phosphate compounds, aluminum (Al)-containing compounds, magnesium (Mg)-containing compounds, titanium (Ti)-containing compounds, tantalum (Ta)-containing compounds, sodium (Na)-containing compounds, zirconium (Zr)-containing compounds, germanium (Ge)-containing compounds, tin (Sn)-containing compounds, silicon (Si)-containing compounds, bromine (Br)-containing compounds, iodine (I)-containing compounds, potassium (K)-containing compounds, scandium (Sc)-containing compounds, niobium (Nb)-containing compounds, neodymium (Nd)-containing compounds, lanthanum (La)-containing compounds, cerium (Ce)-containing compounds, (Si)-containing compounds, rubidium (Rb)-containing compounds, vanadium (V)-containing compounds, cesium (Cs)-containing compounds, chromium (Cr)-containing compounds Compounds, copper (Cu)-containing compounds, magnesium (Mg)-containing compounds, manganese (Mn)-containing compounds, zinc (Zn)-containing compounds, gallium (Ga)-containing compounds, barium (Ba)-containing compounds, actinium (Ac)-containing compounds, calcium (Ca)-containing compounds, iron (Fe)-containing compounds, boron (B)-containing compounds, arsenic (As)-containing compounds, hafnium (Hf)-containing compounds, molybdenum (Mo)-containing compounds, tungsten (W)-containing compounds, rhenium (Re)-containing compounds, ruthenium (Ru)-containing compounds, rhodium (Rh)-containing compounds, platinum (Pt)-containing compounds, silver (Ag)-containing compounds, osmium (Os)-containing compounds, iridium (Ir)-containing compounds, gold (Au)-containing compounds, and combinations thereof.
[0091] Without wishing to be bound by theory, it is envisioned that, first, metal-containing salts are used as the source of each metal element, and all desired inorganic salt elements are mixed in the liquid phase (for example, mixed into a solution, slurry or gel) so that different metals can be uniformly mixed in a desired ratio. As an example, in order to prepare a liquid mixture of an aqueous solution, a slurry or a gel, one or more dopants with high water solubility can be used. For example, metal nitrates, metal sulfates, metal chlorides, metal acetates and metal formates etc. can be used. Organic solvents such as alcohols, isopropanol etc. can be used to dissolve and / or disperse metal-containing salts with low water solubility. In some cases, the pH value of the liquid mixture can be adjusted to increase the solubility of one or more precursor compounds. Optionally, chemical additives, gelling agents and surfactants such as ammonia, EDTA etc. can be added to the liquid mixture to help dissolve or disperse the compound in the selected solvent.
[0092] In a specific embodiment, method 100 includes a series of steps of adjusting the molar ratio M of a lithium salt (Li salt), a lanthanum salt, a zirconium salt, and optionally one or more inorganic salts containing a metal dopant by dissolving these salts in a suitable solvent to prepare a liquid mixture. Li盐 :M La盐 :M Zr盐 :M D1盐 :M D2盐 :…M DN盐, wherein each of the one or more metal salts or salts containing a metal dopant is selected according to the composition of the battery material to be prepared. The molar ratio M of the lithium salt (Li salt), the lanthanum salt, the zirconium salt and the one or more salts containing a metal dopant is adjusted. Li盐 :M La盐 :M Zr盐 :M D1盐 :M D2盐 :…M DN盐 The ratio of a:b:c:d:e: ...:n is adjusted to obtain a lithium oxide (LiaLabZrcD1) doped with one or more dopants at a ratio of Li:La:Zr:D1:D2: ...:DN equal to the desired atomic ratio of a:b:c:d:e: ...:n. d D2 e …DN n Ov), where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and where N≥0, 0≤d≤0.8, 0≤e≤0.8, …, and 0≤n≤0.8.
[0093] Next, we will have M Li盐 The molar concentration of lithium salt, M La盐 The lanthanum-containing salt, the zirconium-containing salt and optionally the one or more dopant-containing salts (e.g., M D1盐 The molar concentration of the first dopant-containing salt, M D2盐 The molar concentration of the second dopant-containing salt ... M DN盐 etc.) for producing a liquid mixture optionally having LiaLabZrcD1 d D2 e …DN n A solid electrolyte material doped with one or more metal dopants of a target composition of 0.05 V, wherein the one or more dopant-containing salts containing a first dopant, a second dopant, ..., a salt containing an Nth dopant are produced, and wherein the liquid mixture reaches an M of about a:b:c:d:.e:..:n Li盐 :M La盐 :M Zr盐 :M D1盐 :M D2盐 :…M DN盐 The mist of the liquid mixture may contain droplets of various reactant solutions, precursor solutions, etc. in uniform form, size, shape, etc. For example, depending on the desired composition of the final solid product particles, the molar ratio M of the lithium-containing salt, the lanthanum-containing salt, the zirconium-containing salt, and optionally one or more metal dopant-containing salts may be adjusted. Li盐 :M La盐 :M Zr盐 :M D1盐 :MD2盐 :…M DN盐 In one embodiment, optionally, the one or more dopants (D1, D2, ... DN) are incorporated into the solid electrolyte material, wherein D1, D2, ... DN are different dopants.
[0094] For example, each of the one or more dopants (i.e., D1, D2, ... DN) can be selected from the group consisting of Al, Ti, Ta, F, Cl, I, Br, Mg, Mn, Zr, Zn, Nb, La, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, Ge, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, and combinations thereof. Next, the solid particles of the solid electrolyte material can be adjusted manually or digitally and prepared in a desired molar ratio and mixed into a liquid mixture (such as by adjusting, measuring appropriate amounts of a lithium salt compound, a lanthanum salt compound, a zirconium salt compound, and optionally one or more dopant-containing salts and preparing them into a solution with an appropriate amount of a solvent).
[0095] Can produce the mist of liquid mixture by mist generator, such as nozzle, sprayer, atomizer or any other mist generator.Most mist generators adopt air pressure or other means to convert liquid mixture into droplet.Mist generator can be connected to a part of power jet chamber, to directly produce the mist (for example, the large collection of small-sized droplets) of liquid mixture in power jet chamber.As an example, atomizer can be attached to a part of power jet chamber, to spray or spray liquid mixture directly into the mist comprising small-sized droplets inside power jet chamber.Usually, need to produce the mist generator of the mist of single size droplet.Alternatively, can produce mist outside power jet chamber and be transported in power jet chamber.
[0096] The desired droplet size can be adjusted by adjusting the size of the liquid delivery / injection channel in the mist generator. Droplet sizes ranging from a few nanometers to hundreds of microns can be produced. Suitable droplet sizes can be adjusted based on the selection of the mist generator used, the precursor compound, the temperature of the power jet chamber, the flow rate of the gas, and the residence time in the power jet chamber. As an example, a mist with a droplet size of one tenth of a micron to one millimeter is produced in the power jet chamber.
[0097] Without wishing to be bound by theory, in the method 100 for manufacturing a battery material using a lithium-containing salt and one or more salts containing a dopant, it is envisioned that a lithium-containing salt, one or more salts, and one or more salts containing a dopant are prepared into a liquid mixture, which is then converted into droplets, each droplet having a uniform distribution of one or more liquid mixtures. The water in the liquid mixture is then removed by passing the droplets through a power jet chamber, and the mist is carried in the power jet chamber using an airflow for an appropriate residence time. It is further envisioned that the concentration of the compound in the liquid mixture and the droplet size of the mist of the liquid mixture can be adjusted to control the chemical composition, particle size, and size distribution of the final solid product particles of the battery material. It is designed that after the mist of the liquid mixture is sprayed into the power jet chamber for reaction, spherical solid particles are obtained from a fully mixed liquid mixture of two or more precursors. In contrast, conventional solid-state manufacturing processes involve mixing or grinding a solid mixture of precursor compounds, resulting in an uneven mixing of the precursors.
[0098] like Figure 2As shown, method 100 includes step 130: drying the gas-liquid mixture for a first reaction time period by delivering a second gas stream of heated gas to perform one or more oxidation reactions, thereby forming a gas-solid mixture in the power jet chamber after high-temperature drying and oxidation reactions. The first reaction time period can be advantageously carried out at a high speed, such as less than 20 minutes, for example less than 10 minutes, less than 5 minutes or even less than 2 minutes. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, inert gas, rare gas and combinations thereof, and can be heated to a high temperature, for example, above about 100°C, such as above about 200°C, for example 200°C to 500°C, or more than 250°C, such as above 350°C. The first reaction time period can be about 1 second to 1 hour. Optionally, another gas stream can be used to carry out oxidation and / or drying reactions. Another gas can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, inert gas, rare gas and combinations thereof, etc. Other airflow can be pumped through air filter to remove any particles, droplets or pollutants, and the flow rate of other gas can be adjusted by valve or other devices.At a temperature, the mist of liquid mixture is dried (for example, removing its moisture, liquid, etc.) for the desired residence time, and in the power jet chamber, a gas-solid mixture is formed together with the gas stream.Due to removing moisture from the mist of liquid mixture in the power jet chamber filled with gas, a gas-solid mixture comprising gas and compound is formed.For illustration, the liquid mixture is dried in the power jet chamber, and the temperature in the power jet chamber is maintained via the heating element coupled to the power jet chamber, wherein the heating element can be a suitable heating mechanism, such as a wall heating furnace, an electric heater, a fuel combustion heater, etc. In addition, one embodiment of the present invention provides that one or more gases flowing in the power jet chamber are used as a gas source for oxidation reaction, drying, evaporation, dehydration and / or other reactions in the power jet chamber, so that the gas-liquid mixture is dried into a gas-solid mixture.In another embodiment, the gas is heated to a temperature to mix with the mist and remove moisture from the mist.
[0099] In one configuration, the gas is preheated to a temperature of about 200° C. or more before being injected into the power jet chamber. In another configuration, the mist can be dried by directly heating the power jet chamber, such as heating the chamber body of the power jet chamber. For example, the power jet chamber can be a wall-type heating furnace to maintain the temperature within the internal plenum of the power jet chamber. The advantages of using heated gas are fast heat transfer, high temperature uniformity, easy scale-up, etc. The power jet chamber can be any chamber, a furnace with a closed chamber body, such as a dome-type ceramic power jet chamber, a quartz chamber, a tube chamber, etc. Optionally, the chamber body is made of an insulating material (e.g., ceramic, etc.) to prevent heat loss during the reaction.
[0100] In another embodiment, the gas flowing in the power jet chamber is heated, and the heat energy of the heated gas is used as an energy source for reaction, oxidation, drying, evaporation, dehydration and / or other reactions in the power jet chamber. The gas can be heated to a temperature by passing the gas through a suitable heating mechanism, such as an electric heater, a dye burning heater, etc. The temperature is about 200°C or more, for example 200°C to 300°C, such as 250°C. For example, in the power jet chamber, the liquid mixture is dried in the presence of a second gas heated to more than 200°C, and the second gas is transported to the power jet chamber to maintain the temperature in the power jet chamber. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, an inert gas, a rare gas, and a combination thereof. For example, heated air can be used as an inexpensive gas source and an energy source for drying mist. The selected gas can be a gas heated to a high temperature to mix with a gas-liquid mixture and dry the gas-liquid mixture without reacting with the compound. In some cases, the chemical substance in the droplet / mist may react to a certain degree with the gas and / or each other during the drying period, depending on the chemical composition of the temperature and the compound. In addition, the residence time of the mist of the fully mixed compound in the power jet chamber is adjustable, and can be, for example, 1 second to 1 hour, depending on the flow rate of the gas and the length and volume of the path that the mist must flow through in the power jet chamber. The air flow can be pumped through an air filter to remove any particle, droplet or pollutant, and the flow rate of the gas can be adjusted by a valve or other device. Therefore, one embodiment of the present invention provides gas as a gas source for reacting, oxidizing, drying, evaporating, dehydrating and / or other reactions. In another embodiment, the gas is heated to a temperature to mix with the mist and remove moisture from the mist. The gas-liquid mixture is dried to a gas-solid mixture in the power jet chamber using a heated gas that flows continuously and / or with an adjustable, variable flow rate.
[0101] In step 140, the gas-solid mixture is conveyed out of the power jet chamber, and in step 150, the dried gas-solid mixture is separated into one or more solid particles of battery material by a gas-solid separator. For example, the dried gas-solid mixture is carried by the gas as a well-mixed gas-solid mixture through a path in the power jet chamber, and as more gas flows in, the gas-solid mixture is conveyed out of the power jet chamber and continuously conveyed to a gas-solid separator connected to the power jet chamber to separate the gas-solid mixture into waste products and one or more solid particles of SSE battery material.
[0102] Next, in step 160, one or more solid particles of the battery material are transported to the annealing chamber for a dynamic crystallization process, and in step 170, in the presence of a third gas flow, the one or more solid particles of the battery material are annealed for a second reaction time period to form and obtain a crystallized product of the battery material to be used in a solid-state battery. The second reaction time period can be more than 1 hour, more than 2 hours, more than 4 hours, more than 8 hours, or even longer. In addition, steps 150, 160, and 170 can be repeated during the dynamic crystallization process to obtain a better crystalline structure.
[0103] The reaction of one or more solid particles of battery material in the annealing chamber may include any one of oxidation, reduction, decomposition, chemical reaction, phase change, recrystallization, single displacement reaction, double displacement reaction, combustion, isomerization and combinations thereof. For example, one or more solid particles of battery material may be oxidized and appropriately arranged into a crystal structure. Exemplary third gases include, but are not limited to, air, oxygen, carbon dioxide, oxidizing gases, nitrogen, inert gases, rare gases, hydrogen and combinations thereof. For oxidation reactions in the annealing chamber, oxidizing gases may be used as annealing gases. If necessary, the gas may be oxygen with high purity; the purity of oxygen is greater than 50%, for example greater than 80%, such as 95%. Therefore, the gas flow in the annealing chamber is used as an energy source for reactions, oxidations and / or other reactions in the annealing chamber.
[0104] The annealing temperature may be, for example, above 400°C for a dwell time to obtain a battery material. For example, the annealing temperature may be above 600°C, above 700°C, above 800°C, above 900°C, such as above 750°C, above 850°C, above 950°C, above 1050°C, above 1150°C. The dwell time is about 1 second to 30 hours.
[0105] In one embodiment, the gas flowing in the annealing chamber is heated, and the thermal energy of the heated gas is used as an energy source for annealing reactions and / or other reactions in the annealing chamber. The gas can be heated to a temperature of 550°C or more by passing the gas through an appropriate heating mechanism, such as an electric heater, a fuel combustion heater, etc. For example, one or more solid particles of the battery material are annealed in the presence of a third gas heated to more than 550°C in the annealing chamber, and the gas is transported to the annealing chamber to maintain the annealing temperature in the annealing chamber. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, an inert gas, a rare gas, and a combination thereof. For example, heated air can be used as an inexpensive gas source and an energy source for drying the mist. In addition, the residence time in the annealing chamber is adjustable and can be, for example, 1 second to 1 hour, depending on the flow rate of the gas and the length and volume of the path that the solid particles must pass through in the annealing chamber.
[0106] Another embodiment of the present invention is that one or more solid particles of battery material are annealed in an annealing chamber, and the temperature is maintained by a heating element coupled to the annealing chamber, wherein the heating element can be a suitable heating mechanism, such as a wall-type heating furnace, an electric heater, a fuel combustion heater, etc. In one configuration, the third gas is preheated to a temperature above about 550°C before flowing into the annealing chamber. In another configuration, the annealing of one or more solid particles of battery material can be performed by directly heating the annealing chamber, such as heating the chamber body of the annealing chamber. For example, the annealing chamber can be a wall-type heating furnace for maintaining the annealing temperature in the internal plenum of the annealing chamber. The advantages of using heated gas are fast heat transfer, high temperature uniformity, easy scale-up, etc. The annealing chamber can be any chamber, a furnace with a closed chamber body, such as a dome-type ceramic annealing chamber, a quartz chamber, a tube chamber, etc. Optionally, the chamber body of the annealing chamber is made of an insulating material (e.g., ceramic, etc.) to prevent heat loss during the annealing process.
[0107] Optionally, in step 180, the battery material is cooled to room temperature. In addition, the battery material is then cooled to room temperature using Figure 3 The crystallized product is ground by the process and grinding device described in or any other suitable process and device to obtain nano-sized particles of battery materials, such as SSE materials, cathode active materials, etc. For example, the battery material can be ground into a nano-size, such as 10 nanometers or more, for example, 20nm to 500μm, 100μm to 300μm, by a jet milling device.
[0108] For example, the temperature of the final solid product particles of the battery material can be slowly cooled to room temperature to avoid interfering with or destroying the process of forming a stable energy state having a uniform morphology and a desired crystal structure. In another example, the cooling stage can be performed very quickly to quench the reaction product so that the crystal structure of the solid particles of the reaction product can be formed in its stable energy state. As another example, the cooling treatment stage in a multi-stage continuous process may include a cooling module consisting of one or more cooling mechanisms. Exemplary cooling mechanisms may be, for example, a gas-solid separator, a heat exchanger, a gas-solid feeder, a fluidized bed cooling mechanism, a combination thereof, and the like.
[0109] Thus, a properly crystallized crystalline product of the desired SSE material in the form of spherical clusters with a micrometer size (such as 1 μm to 300 μm, for example, 10 μm to 100 μm) under scanning electron microscope (SEM) analysis can be obtained. It is envisioned that the size of the obtained battery material is controlled by the droplet size of the mist used in step 120 using the mist generator in the power jet chamber, and the desired size of various battery materials can be adjustably obtained.
[0110] In the method 100 for preparing solid particles of battery materials in multiple stages, it is envisaged that one or more reactions are carried out in a spraying stage, a drying stage, an oxidation stage, two or more annealing reaction stages, one or more grinding stages, one or more cooling stages, etc., so as to obtain nano-sized final solid product particles of battery materials with desired size, morphology and crystal structure for further battery applications. Without wishing to be bound by theory, it is designed that the reaction of the compounds is carried out in two or more reaction stages, so as to allow the compounds to have sufficient time and contact with each other, promote the nucleation of appropriate crystal structures and the appropriate folding of particle morphology, produce lower thermodynamic energy partial reaction pathways, ensure the complete reaction of all compounds, and finally complete the complete reaction, etc. Additional reaction modules may also be used. In one embodiment, the reaction module includes an annealing reaction to react and oxidize one or more solid particles of battery materials into reaction products, wherein a portion of them partially reacts or is oxidized. Other reaction modules include annealing the reaction products once or multiple times into final solid battery material particles to ensure that all reaction products are completely reacted. Therefore, the method 100 may include a processing stage of spraying a mist of a liquid mixture using a processing module including a power spray chamber and a gas-solid separator and obtaining one or more solid particles of a solid electrolyte material. The method 100 may also include another processing stage of reacting, oxidizing, and annealing one or more solid particles of battery material using a reaction module including an annealing chamber.
[0111] Figure 3Flow chart of a method 200 for producing an exemplary solid electrolyte material for a solid-state battery. The method 200 includes a step 202 of grinding the solid electrolyte material to obtain final solid product particles of the solid electrolyte material with a desired size, morphology and crystal structure. In one embodiment, the solid electrolyte material can be ground by jet grinding, mortar grinding, hydraulic grinding, electronic grinding, mechanical grinding or a combination thereof. In one embodiment, the solid electrolyte material is polished and / or ground to less than 900nm, less than 800nm, less than 500nm or less than 300nm, preferably less than 100nm, preferably less than 90nm, preferably less than 80nm, preferably less than 70nm, preferably less than 60nm, preferably less than 50nm, preferably less than 40nm, preferably less than 30nm, preferably less than 20nm, preferably less than 10nm, preferably less than 5nm. In another embodiment, the solid electrolyte material is polished and / or ground to nanoparticles having a size estimated to be in the range of 1 nm to 100 nm; such as 10 nm to 20 nm; such as 10 nm to 90 nm; such as 10 nm to 50 nm; such as 10 nm to 40 nm; such as 10 nm to 70 nm; such as 20 nm to 80 nm; such as 20 nm to 60 nm; such as 20 nm to 50 nm; such as 30 nm to 70 nm; such as 20 nm to 50 nm; such as 40 nm to 70 nm; such as 50 nm to 70 nm; such as 10 nm to 30 nm; such as 15 nm to 40 nm; such as 20 nm to 40 nm; such as 30 nm to 60 nm.
[0112] Secondly, solid electrolyte materials can be pressed into pellets to measure their ionic conductivity, e.g. Figure 3 As shown, method 200 includes a step 204 of pressing a powder of a solid electrolyte material into a pressed solid electrolyte material in the form of a pellet. In one embodiment, the powder of the solid electrolyte material is hydraulically, electronically or mechanically pressed within the range of a 20 mm die in a plurality of consecutive steps; the plurality of consecutive steps are, for example, more than two steps; for example, more than three steps; for example, more than four steps; for example, more than five steps; for example, more than six steps; for example, more than seven steps; for example, more than eight steps; for example, more than nine steps; for example, more than ten steps. For example, the solid electrolyte material is first pressed at 5-10 metric tons, then at 10-15 metric tons, and finally at 12-20 metric tons to form dense pellets. As another example, the solid electrolyte material is first pressed at 5-7 metric tons, then at 7-10 metric tons, and finally at 11-14 metric tons to form dense pellets. As yet another example, the solid electrolyte material is first pressed at 3-15 metric tons, then at 8-20 metric tons, and finally at 20-30 metric tons to form dense pellets.
[0113] The approximate density of the pellets is greater than 50%, preferably greater than 60%, preferably greater than 70%, preferably greater than 75%, preferably greater than 78%, preferably greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 92%, preferably greater than 95%, preferably greater than 97%, preferably greater than 99%.
[0114] In another embodiment, the diameter of the pressed solid electrolyte material in pellet form is 5 mm or more, such as 10 mm or more, 15 mm to 25 mm, preferably 17 mm to 22 mm, or any other suitable diameter, depending on the press used and its mold, such as a cold isostatic press (CIP) or any suitable press. In yet another embodiment, the thickness of the pressed solid electrolyte material in pellet form is less than 1.5 mm, or less than 1.0 mm, such as 400 μm or more, or 500 μm or more, for example 550 μm to 750 μm, or any other suitable thickness, depending on the press used and its mold.
[0115] The method 200 may optionally include a step 206 of adding the pressed solid electrolyte ("SSE") material in pellet form with additional solid electrolyte (SSE) material. In one embodiment, the pressed solid electrolyte ("SSE") material in pellet form is covered with additional solid electrolyte (SSE) material to compensate for the loss of lithium.
[0116] In step 208, the pressed solid electrolyte (SSE) material in pellet form is sintered under the desired processing conditions to obtain the final solid electrolyte material in pellet form to be used in the battery. In one embodiment, the formed pellets in pellet form are sintered in a furnace, such as an annealing reactor, a muffle furnace, a push plate furnace or a roller furnace, etc., at a temperature range of 900°C to 1300°C, such as 1000°C to 1300°C, such as 1100°C to 1300°C, such as 900°C to 1200°C, such as 900°C to 1100°C, such as 1000°C to 1200°C, such as 1100°C to 1200°C, such as 1150°C to 1200°C. Optionally, in step 210, the surface of the final solid electrolyte material in pellet form is polished to the desired thickness and surface, for example, using sandpaper or other polishing techniques.
[0117] Figure 4-5 Embodiments of methods 210 and 220 for coating a cathode active material with a solid electrolyte material and forming coated cathode active materials 92C, 92D are shown. Figure 4In the present invention, method 210 is a wet coating process, which includes a step 211 of forming a coating solution by dissolving a first amount of a solid metal salt or SSE material in a solvent. In step 213, a coating mixture is formed by mixing the coating solution with a certain amount of solid particles of a battery material to be coated with a solid metal or SSE material for a first period of time.
[0118] Generally, two or more metal salts in liquid form can be directly prepared into a liquid mixture of desired concentration. Two or more solid metal salts in solid form can be dissolved or dispersed in a suitable solvent (e.g., water, alcohol, methanol, isopropyl alcohol, isopropanol, organic solvents, inorganic solvents, organic acids, sulfuric acid (H 2 SO 4 ), citric acid (C 6 H 8 O 7 ), acetic acid (CH 3 COOH), butyric acid (C 4 H 8 O 2 ), lactic acid (C 3 H 6 O 3 ), nitric acid (HNO 3 ), hydrochloric acid (HCl), ethanol, pyridine, ammonia, acetone and combinations thereof) to form a liquid mixture in an aqueous solution, a slurry, a gel, an aerosol or any other suitable liquid form. Depending on the desired composition of the final reaction product, two or more metal salts can be used. For example, two or more solid metal salts can be prepared in a desired molar ratio and mixed into a liquid mixture, such as by measuring an appropriate amount of two or more solid metal salts and preparing them in a container containing an appropriate amount of solvent. Depending on the solubility of the precursor in the selected solvent, pH, temperature, and mechanical stirring and mixing can be adjusted to obtain a liquid mixture in which one or more precursor compounds are completely dissolved and / or uniformly dispersed at a desired molar concentration.
[0119] Another aspect of the present invention is a liquid mixture consisting of two or more different soluble solutions with a desired molar ratio, for producing a solid electrolyte material in a solid-state battery showing high capacity. This provides the ability to precisely control and obtain a specific molar ratio at the atomic level, and produces the desired composition of a solid electrolyte material as a coating solution for manufacturing solid-state battery materials. The soluble solution of the liquid mixture includes each metal-containing salt dissolved in an appropriate solvent to achieve a specific molar concentration of a metal-containing salt solution, and the metal-containing salt solution is mixed together to form a liquid mixture of a desired molar ratio for preparing a solid-state electrolyte material. The process for preparing the liquid mixture is effective for manufacturing an active material with a high purity, precise stoichiometric phase. This provides a solid-state battery with desired properties, such as high coulombic efficiency and high nominal capacity.
[0120] Next, in step 215, the coating mixture is dried in an oven or other suitable machine at a first temperature for a second period of time to obtain a dry solid powder of the coated battery material coated with the solid metal or SSE material. The first temperature is about 100° C. or above, or 150° C. or above, for example, 200° C. to 300° C., such as 250° C. The second period of time is about 10 minutes or more, for example, 10 minutes to 1 hour, such as 30 minutes.
[0121] In step 217, in a gas (e.g., oxygen (O 2 )) and at a second temperature in a furnace (e.g., a muffle furnace, an annealing chamber, etc.) to form a powder of a coated battery material. For example, a stream of high-purity gas or oxygen is flowed in an annealing reactor (e.g., a muffle furnace) to serve as an energy source for oxidizing and / or reacting various types of unreacted, partially and / or fully reacted metal-containing solid particles into a coated battery material powder of one-fifth by weight. In one aspect, the purity of oxygen is greater than 50%, for example, greater than 80%, such as 90%, 95% or 97%. In one embodiment, the second temperature is higher than 600°C, for example, 650°C to 800°C, such as 750°C. The third time period is about 15 minutes or more, such as 1 hour or more, for example 1 hour to 10 hours, such as 8 hours.
[0122] In step 219, the powder of the coated battery material is ground and sieved to obtain the final coated battery material. In one embodiment, step 219 includes grinding the powder of the coated battery material into separated material powders, and sieving the separated material powders to a desired particle size to obtain a certain amount of the final coated battery material.
[0123] Figure 5An example of a dry coating method for coating solid particles of battery material with a solid metal or SSE material is shown, namely method 220, which includes a step 222 of preparing battery cathode material particles with a pretreatment agent in preparation for dry coating. In step 224, a powder of a solid electrolyte material (SSE) is mixed with particles of a battery cathode material (BCM) in a mixer or blender (e.g., a high energy mixer) at a temperature of X. SSE :Y BCM The ratio of 100% to 100% is first blended at 500 rpm for 1 minute (so as to evenly mix the two powders) to form a mixture. After mixing, the power intensity of the blender can be increased to 2000 rpm for 6 minutes to deagglomerate the two powders into smaller aggregates, so that the SSE material can adhere to the surface of the BCM.
[0124] In one embodiment, X SSE :Y BCM The ratio can be 1-50:50-99 weight %, such as 1-40:60-99 weight %; such as 1-30:70-99 weight %; such as 5-40:60-95 weight %; such as 5-30:70-95 weight %; such as 5-20:80-95 weight %; such as 10-40:60-90 weight %; such as 10-30:70-90 weight %; such as 10-20:80-90 weight %; such as 15-50:50-85 weight %; such as 15-40:60-85 weight %; such as 15-30:70-85 weight %; such as 15-35:65- 85 wt %; such as 20-30:70-80 wt %; such as 20-40:60-80 wt %; such as 20-50:50-80 wt %; such as 20-50:50-80 wt %; such as 20-50:50-80 wt %; such as 30-50:50-70 wt %; such as 30-60:40-70 wt %; such as 30-40:60-70 wt %; such as 35-50:50-65 wt %; such as 35-30:70-65 wt %; such as 35-40:60-65 wt %; such as 40-50:50-60 wt %; such as 45-50:50-55 wt %.
[0125] In one embodiment, Y BCM :X SSEThe ratio of can be 1-50:50-99 weight %, such as 1-40:60-99 weight %; such as 1-30:70-99 weight %; such as 5-40:60-95 weight %; such as 5-30:70-95 weight %; such as 5-20:80-95 weight %; such as 10-40:60-90 weight %; such as 10-30:70-90 weight %; such as 10-20:80-90 weight %; such as 15-50:50-85 weight %; such as 15-40:60-85 weight %; such as 15-30:70-85 weight %; such as 15-35:65- 85 wt %; such as 20-30:70-80 wt %; such as 20-40:60-80 wt %; such as 20-50:50-80 wt %; such as 20-50:50-80 wt %; such as 20-50:50-80 wt %; such as 30-50:50-70 wt %; such as 30-60:40-70 wt %; such as 30-40:60-70 wt %; such as 35-50:50-65 wt %; such as 35-30:70-65 wt %; such as 35-40:60-65 wt %; such as 40-50:50-60 wt %; such as 45-50:50-55 wt %.
[0126] Next, in step 226, a final coated cathode material (FCCM) having particles of a battery cathode material (BCM) coated and surrounded by a solid electrolyte material (SSE) is obtained. In one embodiment of the dry coating process, larger core particles can be directly coated with smaller fine particles by external mechanical forces without using any solvents and adhesives. In another embodiment, a single particle of the cathode material can be successfully coated with fine particles of the solid electrolyte material. In step 228, the final coated cathode material (FCCM) is used as a cathode to make a solid-state battery.
[0127] To obtain coated positive active materials 92C, 92D, solid electrolyte materials 96C, 96D may be coated onto cathode active materials 94C, 94D using a wet coating process or a dry coating process, respectively. Figure 4 and Figure 5As shown. In one embodiment of the dry coating process, larger core particles can be directly coated with smaller fine particles by external mechanical force without the use of any solvents and adhesives. In another embodiment, a single particle of cathode material can be successfully coated with fine particles of solid electrolyte material. For example, the dry coating process includes dry powder mixing, powder to film formation, and film to current collector lamination; all of which are performed in a solvent-free manner. In another embodiment, the wet coating process includes mixing active cathode battery materials, solid electrolyte materials, and organic or inorganic solvents (such as water, alcohol, methanol, isopropyl alcohol, organic solvents, inorganic solvents, organic acids, sulfuric acid (H 2 SO 4 ), citric acid (C 6 H 8 O 7 ), acetic acid (CH 3 COOH), butyric acid (C 4 H 8 O 2 ), lactic acid (C 3 H 6 O 3 ), nitric acid (HNO 3 ), hydrochloric acid (HCl), ethanol, pyridine, ammonia, acetone and combinations thereof) are mixed into a mixture to obtain a coated solid electrolyte material.
[0128] Figure 6 A flow chart of a method 100 for preparing materials for battery electrochemical cells using a system 300 fully equipped with all the required manufacturing tools is illustrated. The system 300 generally includes a mist generator 306, a power jet chamber 310, a power jet module 314, a gas-solid separator 320, and a reactor 340. First, a liquid mixture containing two or more precursors is prepared and transported to the mist generator 306 of the system 300. The mist generator 306 is coupled to the power jet chamber 310 and is suitable for generating mist from the liquid mixture. A heated gas stream can be flowed into the power jet chamber 310 to fill and preheat the internal volume of the power jet chamber before forming the mist or while generating the mist in the power jet chamber 310. The mist is mixed with the heated gas and its moisture is removed to form a gas-solid mixture, which contains heated gas, two or more precursors and / or other gas-phase waste products or by-products, etc.
[0129] Next, the gas-solid mixture is continuously transported to the gas-solid separator 320, which separates the gas-solid mixture into solid particles and waste products. The solid particles are then transported to the reactor 340 to mix with the heated gas stream and form a gas-solid mixture. The reaction is continued in the reactor for a reaction time until the reaction product can be obtained. Optionally, the reaction product, the gas-solid mixture, can be transported to a gas-solid separator (e.g., a gas-solid separator 328) to separate and obtain the final solid product particles and gaseous by-products. In addition, one or more cooling fluid streams (e.g., gas or liquid) can be used to cool the temperature of the reaction product. The final solid product particles can be transported out of the system 300 for further analysis of their properties (e.g., specific capacity, power performance, battery charging cycle performance, etc.), particle size, morphology, crystal structure, etc., to be used as materials in battery cells. Finally, the final particles are filled into the components of the battery cell.
[0130] Figure 7 302B is a schematic diagram of a system 300, which is an example of an integrated tool / device for a fast, simple, continuous and low-cost manufacturing process for preparing materials for battery electrochemical units. System 300 is connected to a liquid mixer 304, which is in turn connected to two or more reactant sources 302A, 302B. Reactant sources 302A, 302B are provided to store various precursor compounds and liquid solvents. The desired amount of precursor compound (solid or liquid form) and solvent are dosed and transported to liquid mixer 304 from reactant sources 302A, 302B so that the precursor compound can be dissolved and / or dispersed in the solvent and fully mixed into a liquid mixture. If necessary, the liquid mixer 304 is heated to a temperature, such as 30°C to 90°C, to help uniformly dissolve, disperse and / or mix the precursor. The liquid mixer 304 is optionally connected to a pump 305 that pumps the liquid mixture from the liquid mixer 304 to a mist generator 306 of the system 300 to generate a mist.
[0131] The mist generator 306 converts the liquid mixture into a mist having a desired droplet size and size distribution. In addition, the mist generator 306 is coupled to the power jet chamber 310 to dry the mist and remove moisture from the mist, and obtain well-mixed solid precursor particles. In one embodiment, the mist generator 306 is located near the top of a vertically placed power jet chamber 310 (e.g., a dome-type power jet chamber, etc.) to spray the mist into the power jet chamber 310 and vertically downward through the power jet chamber. Alternatively, the mist generator can be located near the bottom of the vertically placed power jet chamber 310 to spray the mist upward into the power jet chamber to increase the residence time of the mist generated therein. In another embodiment, when the power jet chamber 310 is horizontally positioned (e.g., a tubular power jet chamber, etc.) and the mist generator 306 is located near one end of the power jet chamber 310, the mist stream delivered from one end of the power jet chamber 310 through the other end is allowed to traverse a path within the power jet chamber within the length of its residence time.
[0132] The motive jet chamber 310 generally includes one or more motive jet modules 314 (e.g., motive jet modules 314A, 314B, 314C, 314D, etc.), a chamber inlet 315, a chamber body 312, and a chamber outlet 317. In one configuration, the mist generator 306 is located within the motive jet chamber 310, near the chamber inlet 315, and is connected to a liquid line 303 adapted to flow therein a liquid mixture from the liquid mixer 304. For example, the liquid mixture within the liquid mixer 304 can be pumped by the pump 305 through the liquid line 303 connected to the chamber inlet 315, into the interior volume of the motive jet chamber 310. The pumping of the liquid mixture by the pump 305 can be configured, for example, continuously at a desired delivery rate (e.g., regulated by a metering valve or other device) to achieve good processing throughput of the system 300. In another configuration, mist generator 306 is located outside of motive jet chamber 310 , and the mist generated thereby is delivered to motive jet chamber 310 via chamber inlet 315 .
[0133] One or more gas lines (e.g., gas lines 331A, 331B, 331C, 331D, etc.) may be coupled to various portions of kinetic jet chamber 310 and adapted to flow gas from gas source 332 into kinetic jet chamber 310. A gas stream stored in gas source 332 may be delivered to kinetic jet chamber 310 while mist is being formed within kinetic jet chamber 310 to carry the mist through the kinetic jet chamber, remove moisture from the mist, and form a gas-solid mixture containing the precursor. A gas stream may be delivered to kinetic jet chamber 310 prior to forming the mist to fill and preheat the interior volume of kinetic jet chamber 310 prior to generating mist within kinetic jet chamber 310.
[0134] In one example, a gas line 331A is connected to the top of the power jet chamber 310 to deliver gas to the mist generator 306 located near the chamber inlet 315 to mix with the mist generated by the mist generator 306 within the power jet chamber 310. In one embodiment, the gas is preheated to a temperature of 70° C. to 600° C. to mix with the mist and remove moisture from the mist. As another example, a gas line 331B in which gas is delivered is connected to the chamber inlet 315 of the power jet chamber 310, very close to the liquid line 303 having a liquid mixture therein. Therefore, the gas can be fully mixed with the mist of the liquid mixture within the power jet chamber 310.
[0135] In another example, a gas line 331C is connected to the chamber body 312 of the motive jet chamber 310 to deliver gas therein and mix the gas with the mist generated from the mist generator 306. In addition, a gas line 331D connected to the motive jet chamber 310 near the chamber outlet 317 can be used to ensure that the gas-solid mixture formed within the motive jet chamber 310 is uniformly mixed with the gas.
[0136] The gas stream can be pumped through an air filter to remove any particles, droplets or contaminants, and the flow rate of the gas can be adjusted by a valve or other device. In one embodiment, the gas is heated to a temperature to mix with the mist and remove moisture from the mist. It is designed to obtain spherical solid particles from a fully mixed liquid mixture of two or more precursors after drying the mist of the liquid mixture. In contrast, conventional solid-state manufacturing processes involve mixing or grinding solid mixtures of precursor compounds, resulting in uneven mixing.
[0137] Once the mist of the liquid mixture is dried and forms a gas-solid mixture with the gas, the gas-solid mixture is transported out of the kinetic jet chamber 310 through the chamber outlet 317. The kinetic jet chamber 310 is coupled to a gas-solid separator 320 of the system 300. The gas-solid separator 320 collects the chamber product (e.g., a gas-solid mixture having a gas and one or more solid particles of a solid electrolyte material mixed together) from the chamber outlet 317.
[0138] The gas-solid separator 320 includes a separator inlet 321A, two or more separator outlets 322A, 324A. The separator inlet 321A is connected to the chamber outlet 317 and is suitable for collecting the gas-solid mixture and other chamber products from the power jet chamber 310. The gas-solid separator 320 separates the gas-solid mixture from the power jet chamber 310 into one or more solid particles of solid electrolyte material and waste products. The separator outlet 322A is suitable for transporting one or more solid particles of solid electrolyte material to the reactor 340 for further processing and reaction. The separator outlet 324A is suitable for transporting the waste product out of the gas-solid separator 320.
[0139] The waste products may be transported to gas abatement device 326A for treatment and release from system 300. The waste products may include, for example, water (H 2 O) steam, organic solvent vapor, nitrogen-containing gas, oxygen-containing gas, O 2 , O 3 、Nitrogen (N 2 ), NO, NO 2 、NO 2 、N 2 O、N 4 O、NO 3 、N 2 O 3 、N 2 O 4 、N 2 O 5 、N(NO 2 ) 3 , carbon-containing gases, carbon dioxide (CO 2 ), CO, hydrogen-containing gas, H 2 , chlorine-containing gas, Cl 2 , sulfur-containing gases, SO 2 , small particles of one or more solid particles of solid electrolyte materials and combinations thereof.
[0140] One or more solid particles of solid electrolyte material may include at least particles of two or more precursors that are dried and uniformly mixed together. It is envisioned that before reacting two or more precursors in reactor 340, one or more solid particles of solid electrolyte material are separated from any byproducts, gaseous products or waste products. Therefore, system 300 is designed to uniformly mix two or more precursors, dry two or more precursors, separate two or more precursors that are dried, and react two or more precursors continuously into the final solid product particles of crystalline solid electrolyte material. Suitable gas-solid separators include cyclone separators, electrostatic separators, electrostatic precipitators, gravity separators, inertial separators, membrane separators, fluidized beds, classifiers, electric screens, impactors, particle collectors, leaching separators, elutriators, air classifiers, leaching classifiers and combinations thereof.
[0141] Once one or more solid particles of the solid electrolyte material are separated and obtained, they are transported to the reactor 340 for further reaction. The reactor 340 includes a gas inlet 333, a reactor inlet 345 and a reactor outlet 347. The reactor inlet 345 is connected to the separator outlet 322A and is suitable for receiving solid particles. Optionally, the container 325 is suitable for storing solid particles before adjusting the amount of solid particles transported to the reactor 340. The gas inlet 333 of the reactor 340 is coupled to a heating mechanism 380 to heat the gas from the gas source 334 to an annealing temperature of 400°C to 1200°C. The heating mechanism 380 can be, for example, an electric heater, a gas heater, a burner, and other heaters. If necessary, an additional gas pipeline can be used to transport heated air or gas to the reactor 340. The preheated gas can fill the reactor 340 and maintain the internal temperature of the reactor 340, which is much better and energy-saving than the conventional heating of the chamber body of the reactor.
[0142] The gas flowing in the reactor 340 is designed to mix with one or more solid particles of the solid electrolyte material and form an oxidized reaction product in the reactor 340. The heat energy from the preheated gas is used as an energy source for reacting one or more solid particles of the solid electrolyte material in the reactor 340. The reaction process includes, but is not limited to, reduction, decomposition, combination reaction, phase change, recrystallization, single displacement reaction, double displacement reaction, combustion, isomerization and a combination thereof. Then, depending on the annealing temperature and the type of precursor initially delivered to the system 300, the oxidized reaction product is annealed for a continuous residence time of 1 second to 10 hours, or longer. One embodiment of the present invention provides a temperature of the reactor 340 controlled by the temperature of the heated gas.
[0143] Once the reaction within reactor 340 is complete, e.g., after the desired crystal structure, particle morphology, and particle size are formed, the oxidized reaction product is transported out of reactor 340 through reactor outlet 347 and / or reactor outlet 348. The cooled reaction product includes final solid product particles of crystallized solid electrolyte material, which include, for example, oxidized product particles of a precursor compound suitable as a material for a battery cell.
[0144] Optionally, the system 300 includes a gas-solid separator, such as a gas-solid separator 328, which collects the reaction products from the reactor outlet 347 of the reactor 340. The gas-solid separator 328 can be a particle collector, such as a cyclone separator, an electrostatic separator, an electrostatic precipitator, a gravity separator, an inertial separator, a membrane separator, a fluidized bed classifier, an electric screen, an impactor, a leaching separator, an elutriator, an air classifier, a leaching classifier, and combinations thereof.
[0145] The gas-solid separator 328 of the system 300 generally includes a separator inlet 321B, a separator outlet 322B, and a separator outlet 324B for separating the reaction products into solid particles and gaseous byproducts. The gaseous byproducts can be transported to a gas abatement device 326B for treatment and released from the system 300. The gaseous byproducts separated by the gas-solid separator 328 generally include water (H 2 O) steam, organic solvent vapor, nitrogen-containing gas, oxygen-containing gas, O 2 , O 3 、Nitrogen (N 2 ), NO, NO 2 、NO 2 、N 2 O、N 4 O、NO 3 、N 2 O 3 、N 2 O 4 、N 2 O 5 、N(NO 2 ) 3 , carbon-containing gases, carbon dioxide (CO 2 ), CO, hydrogen-containing gas, H 2 , chlorine-containing gas, Cl 2 , sulfur-containing gases, SO 2, small particles of solid particles and combinations thereof. In addition, system 300 may also include one or more cooling fluid pipelines 353, 355, which are connected to the reactor outlet 347 or the separator outlet 322A of the gas-solid separator 328 and are suitable for cooling the reaction products and / or solid particles. The cooling fluid pipeline 353 is suitable for conveying a cooling fluid (e.g., gas or liquid) from a source 352 to the separator inlet 321B of the gas-solid separator 328. The cooling fluid pipeline 355 is suitable for conveying a cooling fluid that can be filtered by a filter 354 to remove particles to the heat exchanger 350.
[0146] The heat exchanger 350 is adapted to collect and cool solid particles and / or reaction products from the gas-solid separator 328 and / or the reactor 340 by passing a cooling fluid therethrough. The temperature of the cooling fluid is lower than the temperature of the reaction products and solid particles delivered from the gas-solid separator 328 and / or the reactor 340. The temperature of the cooling fluid may be 4° C. to 30° C. The cooling fluid may be liquid water, liquid nitrogen, air, an inert gas, or any other gas that does not react with the reaction products.
[0147] The final solid product particles are collected and cooled by one or more separators, cooling fluid lines, and / or heat exchangers, and once cooled, are transported out of the system 300 and collected in a final product collector 368. The solid particles may include, in oxidized form, precursors such as oxide materials suitable for loading into battery cells 370. Additional pumps may also be installed to achieve the desired pressure gradient.
[0148] The process control system 390 can be coupled to the system 300 at various locations to automatically control the manufacturing process performed by the system 300 and adjust various process parameters (e.g., flow rate, mixture ratio, temperature, residence time, etc.) within the system 300. For example, the flow rate of the liquid mixture entering the system 300 can be adjusted near the reactant source 302A, 302B, the liquid mixer 304, or the pump 305. The droplet size and generation rate of the mist generated by the mist generator 306 can be adjusted. In addition, the flow rate and temperature of various gases flowing in the gas pipelines 331A, 331B, 331C, 331D, 333, 353, 355, 515, etc. can be controlled by the process control system 390. In addition, the process control system 390 is suitable for controlling the temperature and residence time of various gas-solid mixtures and solid particles at desired levels at different locations.
[0149] Therefore, a continuous process for producing materials for battery cells using a system having a mist generator, a power jet chamber, one or more gas-solid separators and a reactor is provided. A mist generated by a liquid mixture of one or more metal precursor compounds in a desired ratio is mixed with air and dried in a power jet chamber to form a gas-solid mixture. One or more gas-solid separators are used in the system to separate the gas-solid mixture from the power jet chamber into solid particles with one or more metal precursors, and the solid particles are continuously transported to the reactor for further reaction to obtain final solid material particles with two or more embedded metals in a desired ratio.
[0150] The present invention provides the preparation and manufacture of SSE materials or metal oxide materials. Depending on the details and proportions of the metal precursor compounds delivered to the system 300, the resulting final solid material particles obtained from the system 300 can be metal oxide materials, doped metal oxide materials, inorganic metal salts, etc. In addition, the metal oxide material can present a metal crystal structure in the shape of a layer, spinel, olivine, etc. The morphology of the solid product particles (such as the oxidized reaction product prepared using the method 100 and system 300 described herein) is a desired solid powder. The particle size of the solid powder ranges from 1nm to 100μm.
[0151] In operation, the mist in the mist generator is mixed with a gas stream to form a gas-liquid mixture, wherein the liquid mixture contains a lithium salt compound and one or more salt-containing compounds. In addition, the liquid mixture is mixed with a gas stream of another gas in the power jet chamber. It is envisioned that these gas streams are provided to fully mix the liquid mixture to uniformly form a gas-liquid mixture and to help carry the gas-liquid mixture in the power jet chamber. The liquid mixture can be digitally adjusted or manually prepared in a reactant source with a desired molar ratio of the lithium salt compound and the one or more inorganic salt compounds and delivered to one or more liquid mixers.
[0152] Before forming a mist of the liquid mixture in the liquid mixer, the molar ratio of the lithium salt-containing compound and the one or more salt-containing compounds is adjusted. The desired molar ratio of the lithium salt-containing compound to the one or more salts is digitally or manually measured and delivered from the reactant source to the liquid mixer so that the lithium salt-containing compound and the one or more salt-containing compounds can be dissolved and / or dispersed in the solvent and fully mixed into the liquid mixture in the liquid mixer. The lithium salt-containing compound and the one or more salt-containing compounds are both soluble in a suitable solvent in the liquid mixture.
[0153] In addition, while forming the mist of the liquid mixture, the molar ratio of the lithium salt-containing compound and the one or more salt-containing compounds is adjusted. The desired molar ratio of the lithium salt-containing compound and the one or more inorganic salt compounds can be digitally or manually adjusted from each reactant source and delivered to the mist generator to generate the mist of the liquid mixture within the mist generator.
[0154] A liquid mixture comprising a lithium salt compound and one or more salt-containing compounds is mixed with a gas stream to form a gas-liquid mixture in a power jet chamber. The gas-liquid mixture is then dried at a temperature in the power jet chamber to form a gas-solid mixture of solid particles of a solid electrolyte material. The gas-solid mixture is continuously conveyed to a gas-solid separator, which separates the gas-solid mixture into one or more solid particles of a solid electrolyte material and a waste product.
[0155] Then one or more solid particles of oxide material are transported to an annealing chamber to mix with the gas flow. In the annealing chamber, one or more solid particles of solid electrolyte material are reacted and annealed at an annealing temperature to obtain a high-quality solid electrolyte material having a desired size, morphology and crystal structure, optionally doped with one or more dopants.
[0156] Fig. 8A 6100 includes a system inlet 6102 for delivering one or more gases through a gas line 6106 and a system outlet 6104 for delivering particulate material out of the processing system. The one or more gases can be selected from a gas source of air, oxygen, carbon dioxide, nitrogen, hydrogen, an inert gas, a rare gas, and combinations thereof. In one embodiment, such a processing system also includes an array of one or more power injection modules for injecting a liquid mixture into one or more droplet streams and forcing the one or more droplet streams into the processing system. The processing system also includes a reaction chamber for processing the one or more droplet streams and the one or more gases into the particulate material.
[0157] A liquid mixture is prepared from two or more precursor compounds and then converted into droplets, each droplet having the two or more precursors uniformly distributed together. Water is then removed from the liquid mixture by passing the droplets through a dispersion chamber, and a gas stream is used to carry the mist within the dispersion chamber for an appropriate residence time. It is further contemplated that the concentration of the precursor compounds in the liquid mixture and the droplet size of the mist of the liquid mixture can be adjusted to control the chemical composition, particle size, and size distribution of the final product particles of the battery material.
[0158] like Fig. 8AAs shown, such treatment system also includes at least one buffer chamber, which is configured on the system inlet 6102 for conveying the gas source into multiple uniform airflows. In addition, in one embodiment, the treatment system includes a dispersion chamber 6220 and a power injection module 6240A, 6240B and 6240C for preparing the precursor liquid mixture into the desired size and conveying the desired precursor liquid mixture to the treatment system. The power injection module can be attached to a part of the dispersion chamber, and the liquid mixture is sprayed by air pressure, and directly converted into a mist containing small-sized droplets in the dispersion chamber. Alternatively, mist can be generated outside the dispersion chamber and transported to the dispersion chamber. Suitable droplet size can be adjusted according to the selection of the used power injection module, liquid mixture compound, dispersion chamber temperature, gas flow rate and residence time in the dispersion chamber. As an example, a mist with a droplet size of one tenth of a micron to one millimeter is generated in the dispersion chamber.
[0159] The power jet module 6240A is coupled to a portion of the dispersion chamber 6220 to generate a mist of the liquid mixture (e.g., a large collection of small-sized droplets) directly in the dispersion chamber. Typically, the power jet module 6240A is capable of generating a mist of single-sized droplets. In one embodiment, the dispersion chamber 6220 is connected to one or more power jet modules 6240A, 6240B, and 6240C to receive a plurality of uniform gas streams from the buffer chamber and disperse the plurality of uniform gas streams with one or more droplet streams ejected from the array of one or more power jet modules 6240A, 6220B, and 6240C into each other.
[0160] In one embodiment, the dispersion chamber 6220 is then connected to the reaction chamber 6210 for processing one or more droplet streams and one or more gases into particulate material. In addition, the reaction chamber 6210 is connected to the system outlet 6104 for transporting the particulate material out of the processing system.
[0161] Figure 8B An exemplary processing system 6100 that can be used to perform a rapid, simple, continuous, and low-cost manufacturing process for producing particulate materials is shown. The processing system 6100 includes a system inlet 6102 for delivering one or more gases into the processing system, a buffer chamber 6230 connected to the system inlet 6102, a dispersion chamber 6220 connected to the buffer chamber 6230, a reaction chamber 6210 connected to the dispersion chamber 6220, and a system outlet 104 connected to the reaction chamber 6210.
[0162] The processing system 6100 also includes a gas distributor 6232 attached to a chamber wall 6238 of the buffer chamber 6230 for distributing one or more gases F 1Transmitted into multiple uniform airflows F inside the processing system 2 The channels of the distributor 6232, the dispersion chamber 6220, and one or more power injection modules 6240A and 6240B attached to the chamber wall 6228 of the dispersion chamber 6220.
[0163] One or more gases F delivered to the buffer chamber 6230 1 The gas is pressurized downward, so that it flows through the channel 6234 of the gas distributor 6232 at a certain speed and becomes multiple uniform air flows F 2 , multiple uniform airflows F 2 Flow out of channel 6234 and into dispersion chamber 6220. In one embodiment, one or more gases F 1 The gas is pumped through an air filter to remove any particles, droplets or contaminants, and the flow rate of the gas can be adjusted by a valve or other device. In one embodiment, multiple uniform air flows F out of channel 6234 2 The flow rate will be higher than one or more gases F 1 In addition, multiple uniform airflows F 2 The direction will be centralized and unified.
[0164] The power injection module 6240A includes a power injector 6242A for injecting the liquid mixture supplied to the power injection module 6240A into one or more droplet streams. The power injection module 6240A also includes a support frame 6244A for supporting the power injection module 6240A; a module actuator 6246A attached to the inner side of the support frame 6244A for actuating and forcing one or more droplet streams F injected from the power injector 6242A attached to the inner side of the support frame 6244A. A into the dispersion chamber 6220; and a connector 6245A connecting the module actuator 6246A and the power ejector 6242A. In addition, the power ejector module 6240B includes a power ejector 6242B for ejecting the liquid mixture supplied to the power ejector module 6240B into one or more droplet streams. The power ejector module 6240B also includes a support frame 6244B for supporting the power ejector module 6240B; a module actuator 6246B attached to the inner side of the support frame 6244B for actuating and forcing one or more droplet streams F ejected from the power ejector 6242B attached to the inner side of the support frame 6244B B into the dispersion chamber 6220; and a connector 6245B connecting the module actuator 6246B and the motive ejector 6242B.
[0165] The droplet flow F injected into the dispersion chamber 6220 A With multiple uniform airflow F2 With dispersion angle α A Disperse each other and form a uniform gas flow F 2 and droplet flow F A The gas-liquid mixture F 3 In addition, the droplet flow F injected into the dispersion chamber 6220 B With multiple uniform airflow F 2 With dispersion angle α B Disperse each other and form a plurality of uniform airflows F 2 and droplet flow F B The gas-liquid mixture F 3 In one embodiment, the dispersion chamber maintains itself at a first temperature.
[0166] One or more gases are heated to a drying temperature to mix with the liquid droplet stream and remove moisture from the liquid droplet stream. It is designed that, after drying the mist of the liquid mixture, spherical solid particles are obtained from the well-mixed liquid mixture of two or more liquid mixtures. In contrast, conventional solid-state manufacturing processes involve mixing or grinding solid mixtures of liquid mixture compounds, resulting in uneven mixing of the liquid mixture.
[0167] The one or more gases can be, for example, air, oxygen, carbon dioxide, nitrogen, hydrogen, inert gases, rare gases, and combinations thereof, etc. For example, heated air can be used as a cheap gas source and energy source for drying the droplet stream. The selection of one or more gases can be a gas that mixes well with the droplet stream of the precursor and dries the mist without reacting with the precursor. In some cases, depending on the drying temperature and the chemical composition of the precursor, the chemical substances in the droplet stream may react with the one or more gases and / or to a certain extent with each other during drying. In addition, depending on the flow rate of the one or more gases and the length of the path that the droplet stream must flow in the dispersion chamber, the residence time of the droplet stream of the fully mixed precursor compound in the dispersion chamber is adjustable.
[0168] The processing system 6100 also includes a reaction chamber 6210 for receiving the gas-liquid mixture F 3 and subjecting the gas-liquid mixture F to the second temperature and reaction time. 3 The desired reaction is carried out to form the final reaction product F 4 Finally, the final reaction product F, which may be a product particle, may be 4 The particles are transported out of the system 6100 via the system outlet 6104 for further analysis of their properties (e.g., specific capacity, power performance, particle charge cycle performance, etc.), particle size, morphology, crystal structure, etc., for use as particulate materials.
[0169] The processing system 6100 is connected to the electronic control unit 6300 by the CPU 6340 for automatically controlling the processing system 6100. As shown in Figure 14, the control unit 6300 is coupled to the processing system 6100 at different positions to automatically control the manufacturing process performed by the processing system 6100, and to adjust the various process parameters (e.g., flow rate, mixture ratio, temperature, residence time, etc.) in the processing system 6100. For example, the flow rate of the liquid mixture entering the processing system 6100 can be adjusted near the liquid mixture container or pump. As another example, the droplet size and generation rate of the mist produced by the power injection modules 6240A and 6240B can be adjusted. In addition, the flow rate and temperature of various gases flowing in the gas pipeline can be controlled by the control unit 6300. In addition, the process control unit 6300 is suitable for controlling the temperature, air pressure and residence time of each gas-solid mixture and solid particles at a desired level at different positions.
[0170] In operation, the control unit 6300 can be used to control the parameters of a continuous multi-stage process (e.g., method 900 described herein) performed within the control unit 6300 to obtain high quality and consistent active battery materials with significantly less time, labor, and supervision than materials produced by conventional manufacturing processes. Figure 8B A representative processing curve performed by the control unit 6300 is shown as a graph of temperature versus time.
[0171] Optionally, the processing system 6100 further comprises a first separator connected to the dispersion chamber 6230 and adapted to collect the gas-liquid mixture F from the dispersion chamber. 3 and separates it into a first type of solid particles and waste products. Optionally, a first separator is connected to a motive jet chamber, which is connected to the dispersion chamber 6230 and is suitable for collecting the gas-liquid mixture F from the dispersion chamber. 3 and dried into gas-solid particles, which are transported and separated into solid particles of the first type and waste products in the first separator. In one embodiment, the first separator further comprises a first separator outlet and a second separator outlet, wherein the first separator outlet is connected to the reaction chamber 6210 and is suitable for transporting the solid particles of the first type into the reaction chamber 6220, and the second separator outlet is suitable for transporting the waste products out of the first separator.
[0172] Figure 8CAn example of a power jet module configured in a dispersion chamber is shown. A power jet module 1040A for jetting a liquid mixture into one or more droplet streams and forcing the one or more droplet streams into a processing system includes a power jet 1042A for jetting the liquid mixture supplied to the power jet module 1040A into one or more droplet streams. The power jet module 1040A also includes a support frame 1044A for supporting the movement of the power jet 1042A, a first module actuator 1046A for moving the power jet to be connected to an opening on the dispersion chamber accordingly, and a connector 1045A connecting the first module actuator 1046A and the power jet 1042A.
[0173] exist Figure 8C In the embodiment, the dispersion chamber 1020 includes one or more openings 1022A, 1022B, 1022C, 1022D, 1022E and 1022F, which are located on the chamber wall of the dispersion chamber 1020 and are suitable for connecting to and cooperating with the power ejector of the power nozzle module on the side of the power ejector with the nozzle array. In one embodiment, the shape of the one or more openings and the arrangement of the one or more openings are shown in Figure 8C In which one or more openings are rectangular (wherein the bottom width is shorter than the side length) and are positioned adjacent to each other at a uniform distance on the same horizontal line of the chamber wall.
[0174] like Figure 8C As shown, the dispersion chamber 1020 is filled with multiple uniform gas streams F delivered from the buffer chamber of the processing chamber. 2 In one embodiment, multiple uniform gas streams F may be injected from the power injector of the power injection module to form a droplet flow in the dispersion chamber 1020. 2 The mist is delivered to the dispersion chamber 1020 to carry the droplet stream through the dispersion chamber 1020, which may or may not remove moisture from the mist and form a directional gas-liquid mixture F containing a liquid mixture and multiple uniform gas streams. 3 Furthermore, multiple uniform gas streams F can be formed before the droplet stream is formed. 2 The flow is delivered to the dispersion chamber 1020 to fill the internal volume of the dispersion chamber 1020 and optionally preheat the internal volume of the dispersion chamber 1020 to a first temperature before generating the droplet flow in the dispersion chamber 1020.
[0175] One or more openings 1022A-1022F are located near the top of a vertically placed dispersion chamber 1020 (e.g., a dome-shaped dispersion chamber, etc.) to connect and adapt a power injection module for injecting a droplet stream into the dispersion chamber 1020 and passing vertically downward through the dispersion chamber. Alternatively, one or more openings 1022A-1022F can be located near the bottom of the vertically placed dispersion chamber 1020 and can be connected and adapted to a power injection module for injecting a droplet stream upward into the dispersion chamber by increasing the residence time of the stream generated therein. In another embodiment, when the dispersion chamber 1020 is placed horizontally (e.g., a tubular dispersion chamber, etc.) and one or more openings 1022A-1022F are located near one end of the dispersion chamber 1020 to adapt and connect to a power injection module, the injected droplet stream to be transported from one end of the dispersion chamber 1020 through the other end of the dispersion chamber 1020 can pass through the path within the dispersion chamber 1020 within the length of its residence time.
[0176] In addition, the droplet flow injected into the dispersion chamber 1020 is aligned with the plurality of uniform air flows F 2 Dispersed together into multiple uniform gas flows F 2 and droplet flow gas-liquid mixture F 3 The dispersion chamber maintains itself at the first temperature. Furthermore, the plurality of uniform gas flows F delivered to the dispersion chamber 2 The direction of the dispersion chamber 1020 is parallel to the chamber wall of the dispersion chamber 1020. The gas-liquid mixture F is transported through the dispersion chamber 1020. 3 The direction of the gas flow F is also parallel to the chamber wall of the dispersion chamber 1020. In another embodiment of the present invention, the multiple uniform gas flows F delivered to the dispersion chamber 1020 are 2 The direction and transport of the gas-liquid mixture F through the dispersion chamber 1020 3 The direction is different.
[0177] Fig.8D An example of a power jet module configured in a dispersion chamber is shown. In one embodiment, a power jet module 1140A for jetting a liquid mixture into one or more droplet streams and forcing the one or more droplet streams into a processing system includes a power jet 1142A for jetting the liquid mixture supplied to the power jet module 1140A into one or more droplet streams. The power jet module 1140A also includes a support frame 1144A for supporting the movement of the power jet 1142A, a first module actuator 1146A for moving the power jet to be connected to an opening on the dispersion chamber accordingly, and a connector connecting the first module actuator 1146A and the power jet 1142A.
[0178] like Fig.8DAs shown, the dispersion chamber 1120 includes one or more openings 1122A, 1122B, 1122C, which are located on the chamber wall of the dispersion chamber 1120 and are suitable for connecting to and cooperating with the power ejector of the power nozzle module on the side of the power ejector with the nozzle array. The shape of the one or more openings and the arrangement of the one or more openings are shown in Fig.8D In which one or more openings are rectangular (where the bottom width is longer than the side length) and are positioned adjacent to each other at a uniform distance on the same horizontal line of the chamber wall.
[0179] exist Fig.8D The dispersion chamber 1120 is filled with multiple uniform gas streams F delivered from the buffer chamber of the processing chamber. 2 The multiple uniform gas streams F can be simultaneously formed into a droplet stream in the dispersion chamber 1120 by spraying from the power sprayer of the power spray module. 2 The mist is delivered to the dispersion chamber 1120 to carry the droplet stream through the dispersion chamber 1120, which may or may not remove moisture from the mist and form a directional gas-liquid mixture F containing a liquid mixture and multiple uniform gas streams. 3 Furthermore, multiple uniform gas streams F can be formed before the droplet stream is formed. 2 The flow is delivered to the dispersion chamber 1120 to fill the internal volume of the dispersion chamber 1120 and optionally preheat the internal volume of the dispersion chamber 1120 to a first temperature before generating the droplet flow in the dispersion chamber 1120.
[0180] One or more openings 1122A-1122C are located near the top of a vertically positioned dispersion chamber 1120 (e.g., a dome-shaped dispersion chamber, etc.) to connect and adapt a power injection module for injecting a droplet stream into the dispersion chamber 1120 and vertically downward through the dispersion chamber. Alternatively, one or more openings 1122A-1122C may be located near the bottom of the vertically positioned dispersion chamber 1120 and be capable of connecting and adapting a power injection module for injecting a droplet stream upward into the dispersion chamber by increasing the residence time of the stream generated therein. In another embodiment, when the dispersion chamber 1120 is placed horizontally (e.g., a tubular dispersion chamber, etc.) and one or more openings 1122A-1122C are located near one end of the dispersion chamber 1120 to adapt and connect to the power injection module, the injected droplet stream to be transported from one end of the dispersion chamber 1120 through the other end of the dispersion chamber 1120 can pass through the path within the dispersion chamber 1120 within the length of its residence time. In one embodiment, the dispersion chamber maintains itself at a first temperature.
[0181] Multiple uniform gas flows F delivered to the dispersion chamber 2The direction is parallel to the chamber wall of the dispersion chamber 1120. 2 The gas-liquid mixture F formed by the power ejector into a droplet stream and conveyed through the dispersion chamber 1120 3 The direction is parallel to the chamber wall of the dispersion chamber 1120.
[0182] Fig. 8E An example of a power jet module configured in a dispersion chamber of a processing system is shown in perspective view. In one embodiment, a power jet module 1240A for jetting a liquid mixture into one or more droplet streams and forcing the one or more droplet streams into the processing system includes a power jet 1242A for jetting the liquid mixture supplied to the power jet module 1240A into one or more droplet streams. The power jet module 1240A also includes a support frame 1244A for supporting the movement of the power jet 1242A, a first module actuator 1246A for moving the power jet to be connected to an opening on the dispersion chamber accordingly, and a connector 1245A connecting the first module actuator 1246A and the power jet 1242A.
[0183] exist Fig. 8E In the embodiment, the dispersion chamber 1220 includes one or more openings 1222A, 1222B, 1222C, which are located on the chamber wall of the dispersion chamber 1220 and are suitable for connecting to and cooperating with the power ejector of the power nozzle module on the side of the power ejector with the nozzle array. In one embodiment, the shape of the one or more openings and the arrangement of the one or more openings are shown in Fig. 8E In which, one or more openings are rectangular (wherein the bottom width is shorter than the side length) and are positioned adjacent to each other at a uniform distance on the same vertical line of the chamber wall of the dispersion chamber 1220.
[0184] like Fig. 8E As shown, the dispersion chamber 1220 is filled with multiple uniform gas streams F delivered from the buffer chamber of the processing chamber. 2 In one embodiment, multiple uniform gas streams F may be injected from the power injector of the power injection module to form a droplet flow in the dispersion chamber 1220. 2 The mist is delivered to the dispersion chamber 1220 to carry the droplet stream through the dispersion chamber 1220, which may or may not remove moisture from the mist and form a gas-liquid mixture F comprising a liquid mixture and a plurality of uniform gas streams. 3 Furthermore, multiple uniform gas streams F can be formed before the droplet stream is formed. 2The flow is delivered to the dispersion chamber 1220 to fill the interior volume of the dispersion chamber 1220 and optionally preheat the interior volume of the dispersion chamber 1220 to a first temperature before generating the droplet flow in the dispersion chamber 1220.
[0185] One or more openings 1222A-1222C are located near the left end of the horizontally placed dispersion chamber 1220 (e.g., a tubular dispersion chamber, etc.) to connect and adapt a power injection module for injecting a stream of droplets into the dispersion chamber 1220 and passing it through the dispersion chamber from one end to the other. Alternatively, one or more openings 1222A-1222C can be located near the right end of the horizontally placed dispersion chamber 1220 and can be connected and adapted to a power injection module for injecting a stream of droplets upward into the dispersion chamber within the length of the residence time of the stream generated therein. In one embodiment, the dispersion chamber maintains itself at a first temperature.
[0186] Multiple uniform gas flows F delivered to the dispersion chamber 2 The direction is parallel to the chamber wall of the dispersion chamber 1220. 2 The gas-liquid mixture F formed by the power ejector into a droplet stream and conveyed through the dispersion chamber 1220 3 The direction is parallel to the chamber wall of the dispersion chamber 1220.
[0187] Figure 8F An example of a power jet module configured in a dispersion chamber of a processing system is shown in perspective view. In one embodiment, a power jet module 1340A for jetting a liquid mixture into one or more droplet streams and forcing the one or more droplet streams into the processing system includes a power jet 1342A for jetting the liquid mixture supplied to the power jet module 1340A into one or more droplet streams. The power jet module 1340A also includes a support frame 1344A for supporting the movement of the power jet 1342A, a first module actuator 1346A for moving the power jet to be connected to an opening on the dispersion chamber accordingly, and a connector 1345A connecting the first module actuator 1346A and the power jet 1342A.
[0188] exist Figure 8F In the embodiment, the dispersion chamber 1320 includes one or more openings 1322A, 1322B, 1322C, 1322D, 1322E and 1322F, which are located on the chamber wall of the dispersion chamber 1320 and are suitable for connecting to and cooperating with the power ejector of the power nozzle module on a side of the power ejector with a nozzle array (where the bottom width is longer than the side length). In one embodiment, the shape of the one or more openings and the arrangement of the one or more openings are shown in Figure 8F In which one or more openings are rectangular (where the bottom width is longer than the side length) and are positioned adjacent to each other at a uniform distance on the same vertical line of the chamber wall.
[0189] One or more openings 1322A-1322F are located near the left end of the horizontally placed dispersion chamber 1220 (e.g., a tubular dispersion chamber, etc.) to connect and adapt a power injection module for injecting a stream of droplets into the dispersion chamber 1320 and passing it through the dispersion chamber from one end to the other. Alternatively, one or more openings 1322A-1322F can be located near the right end of the horizontally placed dispersion chamber 1320 and can connect and adapt a power injection module for injecting a stream of droplets upward into the dispersion chamber within the length of the residence time of the stream generated therein. In one embodiment, the dispersion chamber maintains itself at a first temperature.
[0190] Multiple uniform gas flows F delivered to the dispersion chamber 2 The direction is parallel to the chamber wall of the dispersion chamber 1320. And the gas-liquid mixture F transported through the dispersion chamber 1320 3 The direction of the gas flow F is also parallel to the chamber wall of the dispersion chamber 1320. In another embodiment of the present invention, the multiple uniform gas flows F delivered to the dispersion chamber 1320 are 2 The direction and transport of the gas-liquid mixture F through the dispersion chamber 1320 3 As another example, multiple uniform air flows F delivered to the dispersion chamber 2 The direction is parallel to the chamber wall of the dispersion chamber 1320. 2 The gas-liquid mixture F formed by the power ejector into a droplet stream and conveyed through the dispersion chamber 1320 3 The direction is parallel to the chamber wall of the dispersion chamber 1220.
[0191] Example:
[0192] Exemplary material compositions are shown in Table 1A (Example #: A1-A3) and include Li a La b Zr c D1 d D2 e …DN n O v The lithium lanthanum zirconium oxide garnet of composition is designed and prepared so that the ratio of a:b:c:d:...:n is approximately the same as that of M Li盐 :M La盐 :M Zr盐 :M D1盐 :M D2盐:…:M D1盐 The same ratio, where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and D 1 , D 2 ,…,D N At least one of them is a metal, N ≥ 0, 0 ≤ d ≤ 0.8, 0 ≤ e ≤ 0.8, and 0 ≤ n ≤ 0.8, and wherein D 1 , D 2 ,…,D N Including Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br and combinations thereof. The annealing temperature and annealing time can be controlled to be 700 to 1000°C for 7 to 20 hours. In one example, the solid electrolyte material of the ceramic material is a lithium lanthanum zirconium oxide material with a garnet-type cubic structure doped with and without Al, Ti, Ta, Ge, etc. In another example, the obtained solid electrolyte material of the ceramic material is a lithium lanthanum zirconium oxide material with a garnet-type tetragonal structure doped with and without Al, Ti, Ta, Ge, etc. In yet another example: the solid electrolyte material of the ceramic material includes Li 7 La 3 Zr 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 1.5 Ta 0.5 O 12 , Li 6.25 La 3 Zr 2 Ta 0.25 Ga 0.2 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Al0.2 O 12 , Li 6.25 La 3 Zr 2 Al 0.25 O 12 .
[0193] Examples A1-A3 as shown in Table 1A were performed to prepare solid electrolyte materials at an annealing temperature exceeding 700°C; for example, 700°C to 1000°C; such as 950°C; such as 900°C; such as 850°C; such as 800°C; such as 750°C. The examples exhibit different structures and ionic conductivities, for example, ionic conductivities greater than 10 -4 S / cm, preferably greater than 5×10 -4 , or greater than 8×10 -4 S / cm, or greater than 1.0×10 -3 , or greater than 4×10 -3 S / cm, greater than 5×10 -3 S / cm, greater than 6×10 - 3 S / cm, preferably greater than 7×10 -3 S / cm, preferably greater than 8×10 -3 S / cm, preferably greater than 9×10 -3 S / cm.
[0194] Table 1A
[0195]
[0196] The exemplary material compositions in Table 1B (Example #: B1-B3) include Li a La b Zr c D1 d D2 e …DN n O v The lithium lanthanum zirconium oxide garnet of composition is designed and prepared so that the ratio of a:b:c:d:...:n is about the same as M Li盐 :M La盐 :M Zr盐 :M D1盐 :M D2盐 :…:M DN盐 The same ratio, where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and where D 1 , D 2 ,…,D NAt least one of is a metal, N ≥ 0, 0 ≤ d ≤ 0.8, 0 ≤ e ≤ 0.8, and 0 ≤ n ≤ 0.8. The annealing temperature and annealing time can be controlled to be 1000 to 1200 ° C for 7 to 20 hours. In one example, the solid electrolyte material of the ceramic material is a lithium lanthanum zirconium oxide material in a garnet-type cubic phase. In another example, the solid electrolyte material includes Li 7 La 3 Zr 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 1.5 Ta 0.5 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li 6.25 La 3 Zr 2 Al 0.25 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.25 La 3 Zr 2 Ta 0.25 Ga 0.2 O 12 In another example, the solid electrolyte material includes Li 7 La 3 Zr 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 1.5 Ta0.5 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li 6.25 La 3 Zr 2 Al 0.25 O 12 , Li 6.15 La 3 Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.25 La 3 Zr 2 Ta 0.25 Ga 0.2 O 12 Examples B1-B3 as described in Table 1B were performed to prepare solid electrolyte materials at an annealing temperature exceeding 700°C; for example, 1000°C to 1200°C; such as 1050°C; such as 1080°C; such as 1100°C; such as 1200°C; such as 1150°C.
[0197] Table 1B
[0198]
[0199] The exemplary materials in Table 1C (Example #: C1-C6) have Li a La b D1 c D2 d …DN n O v The composition is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M D1盐 :M D2盐 :M DN盐 The same ratio, where 4.5≤a≤7.2, 2.8≤b≤3.5, 1.5≤c≤2.5, 0≤d≤1.2, 0≤n≤1.2, and 2≤v≤12, and where D 1 , D 2 ,…,D NAt least one of is a metal, and N ≥ 1. The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. Examples C1-C6 in Table 1C are performed to prepare a solid electrolyte material at an annealing temperature exceeding 700°C; for example, 700°C to 1000°C; 900°C to 1200°C; such as 1050°C; such as 1080°C; such as 1100°C; such as 1200°C; such as 1150°C; such as 950°C; such as 900°C; such as 850°C; such as 800°C; such as 750°C. In one example, the solid electrolyte material of the ceramic material is a cubic structure. In another example, the solid electrolyte material includes Li 5 La 3 Nb 2 O 12 , Li 5 La 3 Ta 2 O 12 , Li 5 La 3 Ti 2 O 12 , Li 6 La 3 Sr 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ta 2 O 12 , Li 6 La 3 Ba 1 Ti 2 O 12 , Li 1.26 La 2.24 Ti 4 O 12 Embodiments may exhibit different structures and ionic conductivities, for example, ionic conductivities greater than 10 -3 -10 -4 S / cm.
[0200] Table 1C
[0201]
[0202]
[0203] Table 1D shows the Li a La b Ti c D1 d …DN n O vEmbodiment # of ceramic material of chemical composition: D1-D6, wherein 0.9≤a≤2.0, 1.5≤b≤3.0, 3.0≤c≤4.5, 0≤d≤1.2, 0≤n≤1.2, and 2≤v≤12, which is designed and prepared such that the ratio of a:b:c:d:...:n is approximately the same as M Li盐 :M La盐 :M Ti盐 :M D1盐 :…:M DN盐 The ratio is the same. The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. Examples D1-D6 described in Table 1D are carried out to prepare solid electrolyte materials at an annealing temperature exceeding 700°C; for example, 700°C to 1000°C; 900°C to 1200°C; such as 1050°C; such as 1080°C; such as 1100°C; such as 1200°C; such as 1150°C; such as 950°C; such as 900°C; such as 850°C; such as 800°C; such as 750°C.
[0204] Table 1D
[0205]
[0206] In one example, the solid electrolyte material of the ceramic material is a perovskite-type cubic structure. In another example, the solid electrolyte material of the ceramic material includes Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 In another example, the solid electrolyte material of the ceramic material is a tetragonal perovskite structure. In another example, the solid electrolyte material includes Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12In yet another example, the solid electrolyte material is a perovskite-type hexagonal structure. In another example, the solid electrolyte material includes Li 1.36 La 2.24 Ti 4 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 Embodiments may exhibit different structures and ionic conductivities, for example, ionic conductivities greater than 10 -3 -10 -4 S / cm.
[0207] Table 1E
[0208]
[0209] The exemplary material compositions shown in Table 1E (Example #: E1-E6) have Li a Al b P c D1 d …DN n O, wherein 1≤a≤2, 0.2≤b≤1.5, 1.0≤c≤3.5, 0≤d≤2.0, 0≤n≤2.0, and 0.2≤v≤12, and wherein D 1 , D 2 ,…,D N At least one of them is a metal, and N ≥ 1, which is designed and prepared so that the ratio of a:b:c:d:...:n is approximately the same as M Li :M Al :M P :M D1 :…:M DN The ratio is the same, and D 1 , D 2 ,…,D N At least one of is a metal, and N ≥ 0. The annealing temperature and annealing time can be controlled to be 700 to 1200° C. for 7 to 20 hours. In one example, the solid electrolyte material (e.g., lithium aluminum titanium phosphate oxide material) is a sodium super ion conductor (NASICON) type, with a hexagonal structure (undefined if required). In another example, the solid electrolyte material includes Li 1.5 Al 0.5 Ti 1.5 P 3 O 12, Li 1.4 Al 0.4 Ti 1.6 P 3 O 12 , Li 1.6 Al 0.6 Ti 1.4 P 3 O 12 .Li 1.5 Al 0.5 Ge 1.5 P 3 O 12 , Li 1.4 Al 0.4 Ge 1.6 P 3 O 12 , Li 1.6 Ge 0.6 Ti 1.4 P 3 O 12 and combinations thereof. Embodiments may exhibit different structures and ionic conductivities, for example, ionic conductivities greater than 10 -3 -10 -4 S / cm, or greater than 5×10 -4 , greater than 8×10 -3 S / cm, greater than 9×10 -3 S / cm.
[0210] Table 1F
[0211]
[0212] The exemplary material compositions shown in Table 1F (Example #: F1-F6) are Li a Ge b P c D1 d …DN n O v A ceramic material composed of 10≤a≤13, 0.1≤b≤2.0, 0.1≤c≤1.5, 0.1≤d≤2.0, 0.1≤n≤2.0, 2≤v≤12, and wherein D 1 , D 2 ,…,D N At least one of them is a metal, N ≥ 0, and is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li :M Ge :M P :M D1 :…:M DNThe annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. In one example, the solid electrolyte material of the ceramic material is a lithium super ion conductor (LISiCON) type structure, Li 12 Ge 0.5 Al 1.0 Si 0.5 P 1.0 O 12 , Li 10.59 Ge 1.58 V 0.9 P 0.53 O 12 and combinations thereof.
[0213] The exemplary materials shown in Table 1G (Example #: G1-G6) are Li a P b O c N d A material of a composition of , wherein 1.5≤a≤4.0, 0.5≤b≤2.0, 1.0≤c≤4.0, and 0.01≤d≤2.0, which is designed and prepared such that the ratio of a:b:c:d is approximately the same as M Li :M P :M Nt The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. In one example, the solid electrolyte material is a lithium phosphorus oxynitride (LiPON) type having an amorphous structure, for example, Li 2.88 P 1.0 O 3.73 N 0.14 , Li 1.9 Si 0.28 P 1.0 O 1.1 N 1.0 , with a value greater than 10 -5 -10 -6 S / cm, or greater than 6×10 -6 , or greater than 6×10 -5 S / cm, or greater than 9×10 -5 S / cm ionic conductivity.
[0214] Table 1G
[0215]
[0216] The exemplary materials shown in Table 2A (Example #: H1-H6) are Li a P b S c D1 d …DN n Xv A sulfide material of the composition, wherein 3≤a≤16, 0.5≤b≤4.5, 3≤c≤16, 0≤d≤1.5, 0≤n≤1.5, 0≤v≤4, and wherein D 1 , D2, …, D N At least one of them is a metal, N ≥ 0, and X is a halogen, which is designed and prepared so that the ratio of a:b:c:d:...:n is approximately the same as M Li :M P :M S :M D1 :…:M DN The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. In one example, the solid electrolyte material of the sulfide material is an amorphous structure. In another example, the solid electrolyte material of the sulfide material is a cubic structure. The solid electrolyte material of the sulfide material includes Li 7 P 3 S 11 , Li 3 P 1 S 4 , Li 6 P 1 S 5 Cl, Li 6 P 1 S 5 Br 1 , Li 6 P 1 S 5 l. Li 6 P 1 S 5 F 1 , Li 7 P 2 S 8 I 1 , Li 7 P 2 S 8 Br 1 , Li 7 P 2 S 8 Cl 1 , Li 7 P 2 S 8 F 1 , Li 15 P 4 S 16 Cl 3 , Li 14.8 Mg 0.1 P 4 S 16 Cl 3 , Li9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 Ge 1 P 2 S 12 , Li 10 Si 1 P 2 S 12 , Li 10 Sn 1 P 2 S 12 , Li 10 Si 0.3 Sn 0.7 P 2 S 12 , Li 10 Al 0.3 Sn 0.7 P 2 S 12 , Li 11 Al 1 P 2 S 12 , with, for example, greater than 10 -3 -10 -9 S / cm, preferably greater than 8×10 -5 S / cm, preferably greater than 4×10 -3 S / cm, preferably greater than 5×10 -3 S / cm, preferably greater than 6×10 -3 S / m, preferably greater than 7×10 -3 S / cm, preferably greater than 8×10 -3 S / cm, preferably greater than 9×10 -3 S / cm ionic conductivity.
[0217] Table 2A
[0218]
[0219] The exemplary material compositions in Table 2B (Example #: I1-I6) include Li a P b S c A sulfide material of a composition of , wherein 3≤a≤16, 0.5≤b≤4.5, and 3≤c≤16, which is designed and prepared such that the ratio of a:b:c is approximately the same as M Li :M P :M SThe ratio is the same. The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. Examples I1-I6 described in Table 2B are carried out to prepare a solid electrolyte material at an annealing temperature exceeding 700°C; for example, 700°C to 1000°C; 900°C to 1200°C; such as 1050°C; such as 1080°C; such as 1100°C; such as 1200°C; such as 1150°C; such as 950°C; such as 900°C; such as 850°C; such as 800°C; such as 750°C.
[0220] Table 2B
[0221]
[0222] In one example, the solid electrolyte material of the sulfide material is an orthorhombic structure or a triclinic structure and includes Li 3 PS 4 , Li 7 P 3 S 11 , for example, ionic conductivity greater than 10 -3 S / cm, preferably greater than 8×10 -4 , preferably greater than 9×10 -4 S / cm, preferably greater than 2×10 -3 , preferably greater than 4×10 -3 S / cm, preferably greater than 5×10 -3 S / cm, preferably greater than 6×10 -3 S / cm, preferably greater than 7×10 -3 S / cm, preferably greater than 8×10 -3 S / cm, preferably greater than 9×10 -3 S / cm.
[0223] The exemplary materials shown in Table 2C (Example #: J1-J6) are Li a P b S c D1 d …DN n O v A sulfide material of a composition of 5≤a≤16, 0.5≤b≤4.5, 3≤c≤16, 0≤d≤1.5, 0≤n≤1.5, 0≤v≤4, designed and prepared so that the ratio of a:b:c:...:n is approximately the same as M Li :M P :M S :M D1 :…:M DNThe annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. The solid electrolyte material includes Li 10 SiP 2 S 11.3 O 0.7 , Li 9.42 Si 1.02 P 2.1 S 9.96 O 2.04 .
[0224] Table 2C
[0225]
[0226] The exemplary material compositions in Table 2D (Example #: K1-K6) are Li a X b P c S d A sulfide material of a composition of wherein 9≤a≤12, 0.5≤b≤1.5, 1.5≤c≤3.0, and 11≤d≤15, and wherein X is a metal, which is designed and prepared such that the ratio of a:b:c:d is approximately the same as M Li :M X :M P :M S The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. The solid electrolyte materials of sulfide materials include Li 10 G 2 S 12 , Li 10 SiP 2 S 12 , which exhibit different structures and ionic conductivities, for example, ionic conductivities greater than 10 -3 -10 -8 S / cm, preferably greater than 5×10 -7 S / cm, preferably greater than 8×10 -5 S / cm, preferably greater than 9×10 -5 S / cm, preferably greater than 5×10 -4 , preferably greater than 8×10 -4 S / cm, preferably greater than 2×10 -3 , preferably greater than 4×10 -3 S / cm, preferably greater than 5×10 - 3 S / cm, preferably greater than 6×10 -3 S / cm, preferably greater than 7×10 -3 S / cm, preferably greater than 8×10 -3, preferably greater than 9×10 -3 S / cm.
[0227] Table 2D
[0228]
[0229]
[0230] Tables 3-5 are the test results of the solid electrolyte material lithium oxide garnet (Examples #1-#3) measured. The solid electrolyte material lithium oxide garnet was annealed at 950°C for 8 hours and the chemical composition was Li a La b Zr c Al d O v , which is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M Zr盐 :M Al盐 The ratio of Li:La:Zr:Al is the same as that of the prepared M. Li盐 :M La盐 :M Zr盐 :M Al盐 The molar ratio is within the expected range; for example, the ratio of the prepared Al-doped LLZO is 6.2≤M Li盐 ≤7.2:2.8≤M La盐 ≤3.5:1.0≤M Zr盐 ≤2.2:0≤M Al盐 ≤0.8; such as 6.4≤M Li盐 ≤6.9:2.4≤M La盐 ≤3.0:1.3≤M Zr盐 ≤2.0:0≤M Al盐 ≤0.5; such as 6.5≤M Li盐 ≤6.9:2.5≤M La盐 ≤2.95:1.5≤M Zr盐 ≤2.0:0.1≤M Al盐 ≤0.25; such as 6.8≤M Li盐 ≤7.2:2.6≤M La盐 ≤3.2:1.7≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.3; such as 6.9≤M Li盐 ≤7.1:2.8≤MLa盐 ≤2.9:1.8≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.28; such as 6.4≤M Li盐 ≤7.2:2.6≤M La盐 ≤2.98:1.9≤M Zr盐 ≤2.0:0.2≤M Al盐 ≤0.29.
[0231] Table 3: Exemplary compositions of measured Al-doped LLZO materials
[0232]
[0233]
[0234] Table 4: Exemplary compositions of measured Al-doped LLZO materials
[0235]
[0236] In one example, the composition of the Al-doped LLZO material tested is Li 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35 , as shown in Table 3; and its XRD results show a cubic structure. In another example, the composition of the tested Al-doped LLZO material is Li 6.54 La 2.82 Zr 2.0 Al 0.24 O 12.08 , as shown in Table 4; and its XRD results show a cubic structure. In another example, the composition of the tested Al-doped LLZO material is Li 6.74 La 2.96 Zr 2.0 Al 0.25 O 12.45, as shown in Table 5; and its XRD results show a cubic structure. After annealing, the content of each metal in the obtained Al-doped LLZO material was analyzed by an inductively coupled plasma ("ICP") analyzer, which was 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2. 95:1.5≤c≤2.0:0.1≤d≤0.25; such as 6.8≤a≤7.2:2.6≤b≤3.2:1.7≤c≤2.1:0.2≤d≤0.3; such as 6.9≤a≤7.1:2.8≤b≤2.9:1.8≤c≤2.1:0.2≤d≤0.28; such as 6.4≤a≤7.2:2.6≤b≤2.98:1.9≤c≤2.0:0.2≤d≤0.26.
[0237] Table 5: Exemplary compositions of measured Al-doped LLZO materials
[0238]
[0239]
[0240] Tables 6-8 illustrate the test results of the measured solid electrolyte materials (Examples #4-#6), which were annealed at 1150°C for 15 hours and had a chemical composition of Li a La b Zr c Al d O v , which is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M Zr盐 :M Al盐 The ratio of Li:La:Zr:Al is the same as that of the prepared M. Li盐 :M La盐 :M Zr盐 :M Al盐 The molar ratio of the preparation is within the expected range; for example, 6.2≤M Li盐 ≤7.2:2.8≤M La盐 ≤3.5:1.0≤M Zr盐 ≤2.2:0≤M Al盐 ≤0.8; such as 6.4≤M Li盐≤6.9:2.4≤M La盐 ≤3.0:1.3≤M Zr盐 ≤2.0:0≤M Al盐 ≤0.5; such as 6.5≤M Li盐 ≤6.9:2.5≤M La盐 ≤2.95:1.5≤M Zr盐 ≤2.0:0.1≤M Al盐 ≤0.25; such as 6.8≤M Li盐 ≤7.2:2.6≤M La盐 ≤3.2:1.7≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.3; such as 6.9≤M Li盐 ≤7.1:2.8≤M La盐 ≤2.9:1.8≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.28; such as 6.4≤M Li盐 ≤7.2:2.6≤M La盐 ≤2.98:1.9≤M Zr盐 ≤2.0:0.2≤M Al盐 ≤0.29.
[0241] Table 6: Exemplary compositions of measured Al-doped LLZO materials
[0242]
[0243] Table 7: Exemplary compositions of measured LLZO materials
[0244]
[0245]
[0246] After annealing, the content of each metal in the obtained Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer, which is 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2. 95: 1.5≤c≤2.0: 0.1≤d≤0.25; such as 6.8≤a≤7.2: 2.6≤b≤3.2: 1.7≤c≤2.1: 0.2≤d≤0.3; such as 6.9≤a≤7.1: 2.8≤b≤2.9: 1.8≤c≤2.1: 0.2≤d≤0.28; such as 6.4≤a≤7.2: 2.6≤b≤2.98: 1.9≤c≤2.0: 0.2≤d≤0.26. In one example, the composition of the Al-doped LLZO material tested is Li 6.32 La 3.2 Zr 2.0 Al 0.46 O 12.9 , as shown in Table 6; and its XRD results show a cubic structure. In another example, the composition of the tested Al-doped LLZO material is Li 6.49 La 3.28 Zr 2.0 Al 0.31 O 12.7 , as shown in Table 7; and its X-ray diffraction results show a cubic structure. In another example, the composition of the tested Al-doped LLZO material is Li 6.27 La 3.22 Zr 2.0 Al 0.3 O 12.39 , as shown in Table 8; and its XRD results show a cubic structure.
[0247] Table 8: Exemplary compositions of measured LLZO materials
[0248]
[0249] Table 9 shows the test results of the solid electrolyte material (Example #7) measured, which was annealed at 1050°C for 8 hours and had a chemical composition of Li a La b Zr c Al d O v , which is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M Zr盐:M Al盐 The ratio of Li:La:Zr:Al is the same as that of the prepared M. Li盐 :M La盐 :M Zr盐 :M Al盐 The molar ratio of the preparation is within the expected range; for example, 6.2≤M Li盐 ≤7.2:2.8≤M La盐 ≤3.5:1.0≤M Zr盐 ≤2.2:0≤M Al盐 ≤0.8; such as 6.4≤M Li盐 ≤6.9:2.4≤M La盐 ≤3.0:1.3≤M Zr盐 ≤2.0:0≤M Al盐 ≤0.5; such as 6.5≤M Li盐 ≤6.9:2.5≤M La盐 ≤2.95:1.5≤M Zr盐 ≤2.0:0.1≤M Al盐 ≤0.25; such as 6.8≤M Li盐 ≤7.2:2.6≤M La盐 ≤3.2:1.7≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.3; such as 6.9≤M Li盐 ≤7.1:2.8≤M La盐 ≤2.9:1.8≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.28; such as 6.4≤M Li盐 ≤7.2:2.6≤M La盐 ≤2.98:1.9≤M Zr盐 ≤2.0:0.2≤M Al盐 ≤0.29.
[0250] After annealing, the content of each metal in the obtained Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer, which is 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2. 95: 1.5≤c≤2.0: 0.1≤d≤0.25; such as 6.8≤a≤7.2: 2.6≤b≤3.2: 1.7≤c≤2.1: 0.2≤d≤0.3; such as 6.9≤a≤7.1: 2.8≤b≤2.9: 1.8≤c≤2.1: 0.2≤d≤0.28; such as 6.4≤a≤7.2: 2.6≤b≤2.98: 1.9≤c≤2.0: 0.2≤d≤0.26. In one example, the composition of the Al-doped LLZO material tested is Li 6.4 La 2.86 Zr 2.0 Al 0.24 O 11.98 , as shown in Table 9; and its XRD results show a cubic structure.
[0251] Table 9: Exemplary compositions of measured Al-doped LLZO materials
[0252]
[0253] Tables 10-11 illustrate the test results of the solid electrolyte materials (Examples #8-9) measured, which were annealed at 850°C for 8 hours and had a chemical composition of Li a La b Zr c Al d O v , which is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M Zr盐 :M Al盐 The proportions are the same, where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, and 2.0≤v≤12.
[0254] In one example, one observation is that the measured Li:La:Zr:Al ratio of the Al-doped LLZO material composition after annealing is higher than that of the prepared M Li盐 :M La盐 :M Zr盐 :M Al盐 The molar ratio of the preparation is within the expected range; for example, 6.2≤M Li盐 ≤7.2:2.8≤MLa盐 ≤3.5:1.0≤M Zr盐 ≤2.2:0≤M Al盐 ≤0.8; such as 6.4≤M Li盐 ≤6.9:2.4≤M La盐 ≤3.0:1.3≤M Zr盐 ≤2.0:0≤M Al盐 ≤0.5; such as 6.5≤M Li盐 ≤6.9:2.5≤M La盐 ≤2.95:1.5≤M Zr盐 ≤2.0:0.1≤M Al盐 ≤0.25; such as 6.8≤M Li盐 ≤7.2:2.6≤M La盐 ≤3.2:1.7≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.3; such as 6.9≤M Li盐 ≤7.1:2.8≤M La盐 ≤2.9:1.8≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.28; such as 6.4≤M Li盐 ≤7.2:2.6≤M La盐 ≤2.98:1.9≤M Zr盐 ≤2.0:0.2≤M Al盐 ≤0.29.
[0255] After annealing, the content of each metal in the obtained Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer, which is 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2. 95:1.5≤c≤2.0:0.1≤d≤0.25; such as 6.8≤a≤7.2:2.6≤b≤3.2:1.7≤c≤2.1:0.2≤d≤0.3; such as 6.9≤a≤7.1:2.8≤b≤2.9:1.8≤c≤2.1:0.2≤d≤0.28; such as 6.4≤a≤7.2:2.6≤b≤2.98:1.9≤c≤2.0:0.2≤d≤0.26.
[0256] Table 10: Exemplary compositions of measured Al-doped LLZO materials
[0257]
[0258] Table 11: Exemplary compositions of measured Al-doped LLZO materials
[0259]
[0260]
[0261] In one example, the composition of the Al-doped LLZO material tested was Li 6.43 La 2.93 Zr 2.0 Al 0.24 O 12.08. , as shown in Table 10; and its XRD results show a cubic structure. In another example, the composition of the tested Al-doped LLZO material is Li 6.57 La 2.99 Zr 2.0 Al 0.22 O 12.22 , as shown in Table 11; and the XRD results show a cubic structure.
[0262] Tables 12-13 illustrate the test results of the solid electrolyte materials (Examples #10-11) measured, which were annealed at 900°C for 8 hours and had a chemical composition of Li a La b Zr c Al d O v , which is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M Zr盐 :M Al盐 The proportions are the same, where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, and 2.0≤v≤12.
[0263] Table 12: Exemplary compositions of measured Al-doped LLZO materials
[0264]
[0265] Table 13: Exemplary compositions of measured Al-doped LLZO materials
[0266]
[0267]
[0268] In one example, one observation is that the measured Li:La:Zr:Al ratio of the Al-doped LLZO material composition after annealing is higher than that of the prepared M Li盐:M La盐 :M Zr盐 :M Al盐 The molar ratio of the preparation is within the expected range; for example, 6.2≤M Li盐 ≤7.2:2.8≤M La盐 ≤3.5:1.0≤M Zr盐 ≤2.2:0≤M Al盐 ≤0.8; such as 6.4≤M Li盐 ≤6.9:2.4≤M La盐 ≤3.0:1.3≤M Zr盐 ≤2.0:0≤M Al盐 ≤0.5; such as 6.5≤M Li盐 ≤6.9:2.5≤M La盐 ≤2.95:1.5≤M Zr盐 ≤2.0:0.1≤M Al盐 ≤0.25; such as 6.8≤M Li盐 ≤7.2:2.6≤M La盐 ≤3.2:1.7≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.3; such as 6.9≤M Li盐 ≤7.1:2.8≤M La盐 ≤2.9:1.8≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.28; such as 6.4≤M Li盐 ≤7.2:2.6≤M La盐 ≤2.98:1.9≤M Zr盐 ≤2.0:0.2≤M Al盐 ≤0.29.
[0269] After annealing, the content of each metal in the obtained Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer, which is 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2. 95:1.5≤c≤2.0:0.1≤d≤0.25; such as 6.8≤a≤7.2:2.6≤b≤3.2:1.7≤c≤2.1:0.2≤d≤0.3; such as 6.9≤a≤7.1:2.8≤b≤2.9:1.8≤c≤2.1:0.2≤d≤0.28; such as 6.4≤a≤7.2:2.6≤b≤2.98:1.9≤c≤2.0:0.2≤d≤0.26.
[0270] In one example, the composition of the Al-doped LLZO material tested was Li 6.25 La 3.01 Zr 2.0 Al 0.22 O 11.92 , as shown in Table 12; and its XRD results show a cubic structure. In another example, the composition of the tested Al-doped LLZO material is Li 6.49 La 3.02 Zr 2.0 Al 0.23 O 12.2 , as shown in Table 13; and its XRD results show a cubic structure.
[0271] Table 14 shows the test results of the measured solid electrolyte materials (Examples #B1-B3) annealed at 1100°C for 6 hours and having a chemical composition of Li a La b Zr c Al d O v , which is designed and prepared so that the ratio of a:b:c:d is approximately the same as M Li盐 :M La盐 :M Zr盐 :M Al盐 The proportions are the same, where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, and 2.0≤v≤12.
[0272] In one example, one observation is that the measured Li:La:Zr:Al ratio of the Al-doped LLZO material composition after annealing is higher than that of the prepared M Li盐 :M La盐 :M Zr盐 :M Al盐 The molar ratio of the preparation is within the expected range; for example, 6.2≤M Li盐 ≤7.2:2.8≤M La盐 ≤3.5:1.0≤M Zr盐 ≤2.2:0≤M Al盐 ≤0.8; such as 6.4≤M Li盐 ≤6.9:2.4≤M La盐 ≤3.0:1.3≤M Zr盐 ≤2.0:0≤M Al盐 ≤0.5; such as 6.5≤M Li盐 ≤6.9:2.5≤M La盐 ≤2.95:1.5≤M Zr盐 ≤2.0:0.1≤M Al盐 ≤0.25; such as 6.8≤MLi盐 ≤7.2:2.6≤M La盐 ≤3.2:1.7≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.3; such as 6.9≤M Li盐 ≤7.1:2.8≤M La盐 ≤2.9:1.8≤M Zr盐 ≤2.1:0.2≤M Al盐 ≤0.28; such as 6.4≤M Li盐 ≤7.2:2.6≤M La盐 ≤2.98:1.9≤M Zr盐 ≤2.0:0.2≤M Al盐 ≤0.29.
[0273] After annealing, the content of each metal in the obtained Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer, which is 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2. 95:1.5≤c≤2.0:0.1≤d≤0.25; such as 6.8≤a≤7.2:2.6≤b≤3.2:1.7≤c≤2.1:0.2≤d≤0.3; such as 6.9≤a≤7.1:2.8≤b≤2.9:1.8≤c≤2.1:0.2≤d≤0.28; such as 6.4≤a≤7.2:2.6≤b≤2.98:1.9≤c≤2.0:0.2≤d≤0.26.
[0274] Table 14: Exemplary compositions of measured Al-doped LLZO materials
[0275]
[0276] After the second annealing process for sintering the solid electrolyte material into pellets, the content of Al-doped LLZO is 6.2≤a≤7.2:2.8≤b≤3.5:1.0≤c≤2.2:0≤d≤0.8; such as 6.4≤a≤6.9:2.4≤b≤3.0:1.3≤c≤2.0:0≤d≤0.5; such as 6.5≤a≤6.9:2.5≤b≤2.95:1.5≤c≤ 2.0: 0.1≤d≤0.25; such as 6.8≤a≤7.2: 2.6≤b≤3.2: 1.7≤c≤2.1: 0.2≤d≤0.3; such as 6.9≤a≤7.1: 2.8≤b≤2.9: 1.8≤c≤2.1: 0.2≤d≤0.28; such as 6.4≤a≤7.2: 2.6≤b≤2.98: 1.9≤c≤2.0: 0.2≤d≤0.26. An observation can be found as follows: compared with the first annealing process for manufacturing the solid electrolyte material, the lithium content increases (by about 3% to 6%) after the second annealing process (e.g., sintering the solid electrolyte material).
[0277] Table 15 illustrates the tap density (TD), average particle size D, and average particle size of the solid electrolyte material after the annealing process of the exemplary solid electrolytes (Examples #20-25). 50 , D 10 , D 90 , D 1 , D 99 In order to obtain an ideal lithium solid electrolyte material with high discharge capacity, excellent cycle performance and high capacity energy density, the morphology and tap density of the material must be precisely controlled during the preparation process. In one embodiment, the Li a La b Zr c D1 d D2 e …DN n O v , where 6.2≤a≤7.2, 2.8≤b≤3.5, 1.0≤c≤2.0, 2.0≤v≤12, and where D 1 , D 2 ,…,D N At least one of them is a metal, N≥0, 0≤d≤0.8, 0≤e≤0.8, and 0≤n≤0.8. The annealing temperature and annealing time can be controlled to be 700 to 1200° C. for 7 to 20 hours.
[0278] Table 15: Measurement of tap density (TD) & average particle size & SPAN value of exemplary solid electrolyte materials
[0279]
[0280]
[0281] It was found that the tap density ("TD") of the obtained solid electrolyte was greater than 0.8 g / ml, preferably greater than 0.9 g / ml, preferably greater than 1.0 g / ml, preferably greater than 1.09 g / ml, preferably greater than 1.15 g / ml, preferably greater than 1.2 g / ml, preferably greater than 1.3 g / ml, preferably greater than 1.4 g / ml, preferably greater than 1.5 g / ml, preferably greater than 1.6 g / ml, preferably greater than 1.7 g / ml, preferably greater than 1.8 g / ml, preferably greater than 1.9 g / ml, preferably greater than 2.0 g / ml, which can be attributed to the uniform distribution of particles with good packing properties.
[0282] For example, the tap density ("TD") obtained from the solid electrolyte material annealed at 850°C for a period of time (e.g., 6 to 12 hours) is greater than 1.0 g / ml, preferably greater than 1.1 g / ml, preferably greater than 1.15 g / ml. In another example, the tap density ("TD") obtained from the solid electrolyte material annealed at 900°C for a period of time (e.g., 6 to 12 hours) is greater than 1.1 g / ml, preferably greater than 1.15 g / ml, preferably greater than 1.18 g / ml, preferably greater than 1.2 g / ml.
[0283] For example, the tap density ("TD") obtained from a solid electrolyte material annealed at 1050°C for a period of time (e.g., 6 to 12 hours) is shown to be greater than 1.2 g / ml, preferably greater than 1.3 g / ml, preferably greater than 1.35 g / ml, preferably greater than 1.4 g / ml, and preferably greater than 1.45 g / ml, preferably greater than 1.5 g / ml, preferably greater than 1.55 g / ml.
[0284] Another observation is that the SPAN values (D 90 -D 10 ) / D 50Less than 1.7, preferably less than 1.6, preferably less than 1.5, preferably less than 1.4, preferably less than 1.3, preferably less than 1.2, preferably less than 1.1, preferably less than 1.0, preferably less than 0.9, preferably less than 0.8. In one aspect, the SPAN value of the solid electrolyte material is 0.8 < SPAN ≤ 1.7; 0.8 < SPAN ≤ 1.4; such as 0.8 < SPAN ≤ 1.6; 0.8 < SPAN ≤ 1.5. In another aspect, the SPAN value of the solid electrolyte material is 0.9 ≤ SPAN ≤ 1.65. In yet another aspect, the SPAN value of the solid electrolyte material is 1.1 ≤ SPAN ≤ 1.65; such as 1.2 ≤ SPAN ≤ 1.65; such as 1.3 ≤ SPAN ≤ 1.65; such as 1.4 ≤ SPAN ≤ 1.65; such as 1.5 ≤ SPAN ≤ 1.65; such as 1.1 ≤ SPAN ≤ 1.3.
[0285] In another aspect, the SPAN value of the solid electrolyte material does not change significantly with the process of different annealing temperatures. In addition, the D of the solid electrolyte material 90 can be controlled and obtained to be 20 μm to 40 μm; such as 25 μm to 40 μm; such as 25 μm to 38 μm; such as 28 μm to 38 μm; such as 30 μm to 38 μm; such as 31 μm to 38 μm; such as 25 μm to 36 μm; such as 25 μm to 33 μm; such as 25 μm to 31 μm; such as 26 μm to 31 μm.
[0286] In addition, control the D of the solid electrolyte material 50 and obtain it to be 10 μm to 18 μm, less than 18 μm, such as 10 μm to 15 μm, such as 10 μm to 14 μm, such as 11 μm to 17 μm, such as 11 μm to 16 μm; such as 12 μm to 17 μm; such as 12 μm to 16 μm; such as 13 μm to 16 μm; such as 14 μm to 16 μm; such as 11 μm to 15 μm; such as 10 μm to 14 μm; such as 10 μm to 13 μm.
[0287] Still further, the D of the solid electrolyte material 10 is 3 μm to 10 μm; such as 3 μm to 9 μm; such as 3 μm to 8 μm; such as 3 μm to 7 μm; such as 3 μm to 6 μm; such as 4 μm to 10 μm; such as 4 mm to 9 μm; such as 4 μm to 8 μm; such as 4 μm to 7 μm; such as 4 μm to 6 μm; such as 5 μm to 9 μm; such as 5 μm to 8 μm. In addition, the D of the solid electrolyte material 1It is 0.1μm to 3μm; such as 0.1μm to 3μm; such as 0.15μm to 3μm; such as 0.2μm to 3μm; such as 0.3μm to 3μm; such as 0.4μm to 3μm; such as 0.5μm to 3μm; such as 0.3μm to 2μm; such as 0.3μm to 1μm; such as 0.2μm to 1μm; such as 0.2μm to 2μm; such as 0.25μm to 1μm.
[0288] In addition, the D 99 35μm to 60μm; such as 35μm to 58μm; such as 35μm to 55μm; such as 38μm to 59μm; such as 40μm to 56μm; such as 43μm to 54μm; such as 40μm to 53μm; such as 41μm to 58μm; such as 42μm to 59μm; such as 43μm to 52μm; such as 45μm to 60μm; such as 50μm to 60μm.
[0289] Example 20 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 21 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 22 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 23 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15.
[0290] Example 24 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 25 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 26 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 27 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15. Example 28 illustrates the measured tap density (TD), average particle size D 50 , D 10 , D 90 , D 1 , D 99 The results are shown in Table 15.
[0291] Fig. 9The X-ray diffraction ("XRD") patterns of aluminum-doped lithium lanthanum zirconium oxide materials ("LLZO") of Example #41, Example #42, Example #43, Example #44, Example #45, and Example #46 and a reference material showing a garnet-type cubic structure are shown. The XRD patterns of the solid electrolyte materials in Example #41, Example #42, Example #43, Example #44, Example #45, and Example #46 show a garnet-type cubic phase of the solid electrolyte material. The solid electrolyte material contains a high lithium ion (Li+) conductive phase, and its XRD pattern has peaks at all 2θ angles of the cubic structure of the reference material.
[0292] The XRD patterns of doped lithium lanthanum zirconium oxide fine powders synthesized at different temperatures are depicted in Fig.10 Example 41 shows the diffraction peaks of the doped lithium lanthanum zirconium oxide material powder synthesized at 850°C for 8 hours. As shown in Example 41, the XRD pattern of the lithium lanthanum zirconium oxide material synthesized at 800°C is similar to the XRD pattern of the reference sample in the form of commercially available cubic LLZO, and it is proved that the formation of garnet-type cubic phase LLZO is achieved at a temperature of 800°C using the present invention.
[0293] In addition, the results of Example 41 indicate that a cubic phase of Al-doped LLZO has been formed, and no diffraction peak characteristic of a tetragonal phase of LLZO is detected. It should be noted that the cubic phase of LLZO exhibits better ionic conductivity than the tetragonal phase of LLZO.
[0294] Example 42 shows the diffraction peaks of the doped LLZO powder synthesized at 850°C for 8 hours. As shown in Example 42, the XRD pattern of the doped LLZO synthesized at 900°C is similar to the XRD pattern of the reference sample in the form of a commercially available cubic doped LLZO, and proves that the formation of garnet-type cubic phase LLZO is achieved at a temperature of 900°C using the present invention. In Example 42, from Fig.10 The cubic structure observed in is consistent with the commercially available reference sample. In addition, the results of Example 42 indicate that a cubic garnet structure of doped LLZO has been formed, and no diffraction peak characteristic of a tetragonal structure is detected.
[0295] Example 43 shows the diffraction peaks of the doped LLZO powder synthesized at 950° C. for 8 hours. As shown in Example 43, the XRD pattern of the LLZO synthesized at 950° C. is similar to the XRD pattern of the reference sample in the form of a commercially available cubic phase LLZO, and proves that the formation of garnet-type cubic LLZO is achieved at a temperature of 950° C. using the present invention. In addition, the results of Example 43 indicate that the cubic phase LLZO has been formed and no diffraction peaks characteristic of the tetragonal phase LLZO are detected.
[0296] Example 44 shows the diffraction peaks of the doped LLZO powder synthesized at 1000° C. for 8 hours. As shown in Example 44, the XRD pattern of the doped LLZO synthesized at 1000° C. is similar to the XRD pattern of the reference sample in the form of commercially available cubic LLZO, and proves that the formation of garnet-type cubic phase LLZO is achieved at a temperature of 1000° C. using the present invention. In addition, the results of Example 44 indicate that the cubic phase LLZO has been formed, and no diffraction peaks characteristic of the tetragonal phase LLZO are detected.
[0297] Example 45 shows the diffraction peaks of the doped LLZO powder synthesized at 1050° C. for 8 hours. As shown in Example 45, the XRD pattern of the doped LLZO synthesized at 1050° C. is similar to the XRD pattern of the reference sample in the form of commercially available cubic LLZO, and proves that the formation of garnet-type cubic LLZO is achieved at 1050° C. using the present invention. In addition, the results of Example 45 indicate that cubic phase LLZO has been formed, and no diffraction peaks characteristic of tetragonal phase LLZO are detected.
[0298] Example 46 shows the diffraction peaks of the doped LLZO powder synthesized at 1100° C. for 8 hours. As shown in Example 46, the XRD pattern of the doped LLZO synthesized at 1100° C. is similar to the XRD pattern of the reference sample in the form of a commercially available cubic doped LLZO, and proves that the formation of garnet-type cubic doped LLZO is achieved at 1100° C. using the present invention. In addition, the results of Example 46 indicate that a cubic phase LLZO has been formed, and no diffraction peaks characteristic of a tetragonal phase LLZO are detected.
[0299] Fig.10 The XRD patterns of lithium lanthanum zirconium oxide materials (LLZO) doped with aluminum (Al) in Example #51, Example #52, Example #53, and Example #54 and a reference material showing a garnet-type cubic structure are shown. The XRD patterns of the solid electrolyte materials in Example #51, Example #52, and Example #53 all show garnet-type cubic solid electrolyte materials.
[0300] The XRD patterns of Al-doped LLZO fine powders synthesized at the same temperature of 900 °C for different hours (6 hours to 12 hours) are depicted in Fig.11In. Example 51 shows the diffraction peaks of LLZO powder synthesized at 900°C for 6 hours. As shown in Example 51, the XRD pattern of Al-doped LLZO synthesized at 900°C is similar to the XRD pattern of a reference sample in the form of commercially available cubic LLZO, and it is demonstrated that the formation of garnet-type cubic LLZO is achieved at a temperature of 900°C for 6 hours using the present invention. In addition, the results of Example 51 indicate that cubic phase LLZO has been formed, and no diffraction peaks characteristic of tetragonal phase LLZO are detected. Example 52 shows the diffraction peaks of LLZO powder synthesized at 900°C for 8 hours. As shown in Example 52, the XRD pattern of Al-doped LLZO synthesized at 900°C for 8 hours is similar to the XRD pattern of a reference sample in the form of commercially available cubic LLZO, and it is demonstrated that the formation of garnet-type cubic phase LLZO is achieved at 900°C for 8 hours using the present invention. Furthermore, the results of Example 52 indicated that a cubic phase of LLZO had been formed, and no diffraction peak characteristic of a tetragonal phase of LLZO was detected.
[0301] Example 53 shows the diffraction peaks of LLZO powder synthesized at 900°C for 10 hours. As shown in Example 53, the XRD pattern of Al-doped LLZO synthesized at 900°C for 10 hours is similar to the XRD pattern of the reference sample in the form of commercially available cubic LLZO, and proves that the formation of garnet-type cubic phase LLZO is achieved at 900°C for 10 hours using the present invention. In addition, the results of Example 53 indicate that cubic phase LLZO has been formed and no diffraction peaks characteristic of tetragonal phase LLZO are detected.
[0302] Example 54 shows the diffraction peaks of LLZO powder synthesized at 900°C for 12 hours. As shown in Example 54, the XRD pattern of Al-doped LLZO synthesized at 900°C for 12 hours is similar to the XRD pattern of the reference sample in the form of commercially available cubic LLZO, and proves that the formation of garnet-type cubic phase LLZO is achieved at 900°C for 12 hours using the present invention. In addition, the results of Example 54 indicate that cubic phase LLZO has been formed and no diffraction peaks characteristic of tetragonal phase LLZO are detected.
[0303] Fig.11 The XRD patterns of the aluminum (Al)-doped lithium lanthanum zirconium oxide material (LLZO) of Example #61 and a reference showing a garnet-type cubic phase solid electrolyte material are shown. The XRD pattern of the LLZO fine powder synthesized at 850°C for 8 hours is depicted in FIG. Fig.11Example 61 shows the diffraction peaks of the Al-doped LLZO powder synthesized at 850°C for 8 hours. As shown in Example 61, the XRD pattern of the LLZO synthesized at 850°C is similar to the XRD pattern of the academic (or literature) reference sample in the form of cubic phase LLZO, and proves that the formation of garnet-type cubic phase LLZO is achieved at a temperature of 850°C using the present invention. In addition, the results of Example 61 indicate that cubic phase LLZO has been formed and no diffraction peaks characteristic of tetragonal phase LLZO are detected.
[0304] Fig.12 The XRD patterns of the aluminum (Al)-doped lithium lanthanum zirconium oxide material (LLZO) of Example #62 and a reference showing a garnet-type cubic phase solid electrolyte material are shown. The XRD pattern of the LLZO fine powder synthesized at 900°C for 8 hours is depicted in FIG. Fig.12 Example 62 shows the diffraction peaks of the Al-doped LLZO powder synthesized at 900°C for 8 hours. As shown in Example 62, the XRD pattern of the LLZO synthesized at 900°C is similar to the XRD pattern of the academic (or literature) reference sample in the form of cubic phase LLZO, and proves that the formation of garnet-type cubic phase LLZO is achieved at 900°C using the present invention. In addition, the results of Example 62 indicate that cubic phase LLZO has been formed and no diffraction peaks characteristic of tetragonal phase LLZO are detected.
[0305] Fig.13 The XRD patterns of the lithium lanthanum zirconium oxide material (LLZO) of Example #71 and commercial samples of references #1 and #2 showing a garnet-type tetragonal phase as solid electrolyte materials are shown. The XRD pattern of the LLZO fine powder synthesized at 900°C for 8 hours is depicted in FIG. Fig.13 Example 71 shows the diffraction peaks of lithium lanthanum zirconium oxide material powder synthesized at 900°C for 8 hours. As shown in Example 71, the XRD pattern of LLZO synthesized at 900°C is similar to the XRD pattern of academic (or literature) reference samples in the form of cubic LLZO, and it is proved that the formation of garnet-type tetragonal phase LLZO is achieved at 900°C using the present invention.
[0306] Fig.14A , Fig. 14B and Fig. 14C is an exemplary SEM image of solid particles of the solid electrolyte material after the annealing process. Fig.14A , Fig. 14B and Fig. 14CSEM images of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) are shown after annealing at 850°C for 8 hours, 900°C for 8 hours, and 1050°C for 8 hours, respectively. It can be found that one observation is that the annealing temperature does not significantly affect the morphology and crystal structure of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al). In addition, Fig.14A , Fig. 14B and Fig. 14C The diagram shows that particles of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) appear to be estimated to be in the range of 1um to 100um; such as 10um to 20um; such as 10um to 90um; such as 10um to 50um; such as 10um to 40um; such as 10nm to 70um; such as 20nm to 80um; such as 20nm to 60um; such as 20nm to 50um; such as 30nm to 70um; such as 20nm to 50um; such as 40nm to 70um; such as 50nm to 70um; such as 10um to 30um; such as 15um to 40um; such as 20um to 40um; such as 30um to 60um.
[0307] exist Fig.14A In one example shown in FIG. 1 , a lithium lanthanum zirconium oxide material (LLZO) particle 1410 doped with aluminum (Al) has a linear morphology. Fig. 14B As another example shown in FIG. 1 , a lithium lanthanum zirconium oxide material (LLZO) particle 1420 doped with aluminum (Al) has an irregular cluster-like morphology. Fig. 14C In another example shown in , a lithium lanthanum zirconium oxide material (LLZO) particle 1430 doped with aluminum (Al) is morphologically spherical clusters, resulting in a spherical morphology. It can be found that one observation is that the linear morphology at a lower annealing temperature in 14A is destroyed at a higher annealing temperature and forms a cluster of linear morphology as shown in 14C, resulting in coupling of the linear morphology.
[0308] Fig.15A and Fig. 15B is an SEM image of an example of solid particles of the solid electrolyte material after the annealing process. Fig.15A and Fig. 15B It shows that after annealing at 1050 ° C for 8 hours, the chemical composition is Li 7 La 3 Zr 2 O 12 SEM image of lithium lanthanum zirconium oxide material (LLZO). In addition, Fig. 15B Shows the Fig.15A A closer look at Fig. 15BFigure 1 shows the LLZO material at high magnification, where the morphology of the LLZO material can be clearly seen. Fig. 15B In one example shown, a lithium lanthanum zirconium oxide material (LLZO) particle 1510 has a linear morphology. Fig.15A and Fig. 15B The diagram shows that the particles of lithium lanthanum zirconium oxide material (LLZO) appear to be estimated to be in the range of 1um to 100um; such as 10um to 20um; such as 10um to 90um; such as 10um to 50um; such as 10um to 40um; such as 10um to 70um; such as 20um to 80um; such as 20um to 60um; such as 20um to 50um; such as 30um to 70um; such as 20um to 50um; such as 40um to 70um; such as 50um to 70um; such as 10um to 30um; such as 15um to 40um; such as 20um to 40um; such as 30um to 60um.
[0309] Fig.16A and Fig. 16B is an SEM image of an example of solid particles of the solid electrolyte material after the annealing process. Fig.16A and Fig. 16B The SEM image of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) after annealing at 1050°C for 8 hours is shown. In addition, Fig. 16B Shows the Fig.16A A closer look at Fig. 16B LLZO particles are shown at high magnification, where the size and shape of the LLZO particles can be clearly seen. Fig.16A and Fig. 16B As shown in , individual LLZO particles consolidate to form a spherical network, which can enhance the ionic conductivity of the bulk material. The LLZO particles appear to have a spherical shape, and their size is estimated to be in the range of 1um to 100um; such as 10um to 20um; such as 10um to 90um; such as 10um to 50um; such as 10um to 40um; such as 10um to 70um; such as 20um to 80um; such as 20um to 60um; such as 20um to 50um; such as 30um to 70um; such as 20um to 50um; such as 40um to 70um; such as 50um to 70um; such as 10um to 30um; such as 15um to 40um; such as 20um to 40um; such as 30um to 60um. Fig.16A and Fig. 16B As shown in FIG. 1 , it can be found that one observation result is that the lithium lanthanum zirconium oxide (LLZO) material 1610 doped with aluminum (Al) is morphologically spherical clusters. Fig. 16BIn the diagram, a lithium lanthanum zirconium oxide (LLZO) material doped with aluminum (Al) 1620 is shown at a larger magnification, showing a main linear morphology. In addition, the linear lithium lanthanum zirconium oxide (LLZO) materials doped with aluminum (Al) are coupled to each other and form secondary clusters.
[0310] Figures 17A-17D is an SEM image of an example of solid particles of the solid electrolyte material after the annealing process. Fig.17A It is shown that after annealing at 950°C for 8 hours, the Li 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35 SEM image of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) with a composition of . Fig. 17B It is shown that after annealing at 950°C for 8 hours, the Li 6.74 La 2.96 Zr 2.0 Al 0.25 O 12.45 SEM image of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) with a composition of . Fig.17A and Fig. 17B In the embodiment, the Al-doped LLZO particles appear to have a spherical shape, and their sizes are estimated to be in the range of 1um to 100um; such as 10um to 20um; such as 10um to 90um; such as 10um to 50um; such as 10um to 40um; such as 10nm to 70um; such as 20nm to 80um; such as 20nm to 60um; such as 20nm to 50um; such as 30nm to 70um; such as 20nm to 50um; such as 40nm to 70um; such as 50nm to 70um; such as 10um to 30um; such as 15um to 40um; such as 20um to 40um; such as 30um to 60um. In addition, it can be found that one observation result is that the lithium lanthanum zirconium oxide (LLZO) material 1710 doped with aluminum (Al) is morphologically spherical clusters, such as Fig.17A As shown in Fig. 17B In another example shown in , it can be found that another observation is that the lithium lanthanum zirconium oxide (LLZO) material 1720 doped with aluminum (Al) is morphologically spherical clusters.
[0311] Fig. 17C It is shown that after annealing at 850°C for 8 hours, the Li 6.57 La 2.99 Zr2.0 Al 0.22 O 12.22 The SEM image of the lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) of the composition. In addition, it can be found that one observation result is that the lithium lanthanum zirconium oxide (LLZO) material 1730 doped with aluminum (Al) is spherical clusters in morphology, such as Fig. 17C As shown in Fig. 17C In the figure, the Al-doped LLZO particles appear to have a spherical shape, and their sizes are estimated to be in the range of 1um to 100um; such as 10um to 20um; such as 10um to 90um; such as 10um to 50um; such as 10um to 40um; such as 10um to 70um; such as 20um to 80um; such as 20um to 60um; such as 20nm to 50um; such as 30um to 70um; such as 20um to 50um; such as 40um to 70um; such as 50um to 70um; such as 10um to 30um; such as 15um to 40um; such as 20um to 40um; such as 30um to 60um.
[0312] Fig.17D It is shown that after annealing at 900°C for 8 hours, the Li 6.49 La 3.02 Zr 2.0 Al 0.23 O 12.2 SEM image of lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) with a composition of . Fig.17D As shown in , the Al-doped LLZO particles appear to have a spherical shape, and their sizes are estimated to be in the range of 1um to 100um; such as 10um to 20um; such as 10um to 90um; such as 10um to 50um; such as 10um to 40um; such as 10um to 70um; such as 20um to 80um; such as 20um to 60um; such as 20um to 50um; such as 30um to 70um; such as 20um to 50um; such as 40um to 70um; such as 50um to 70um; such as 10um to 30um; such as 15um to 40um; such as 20um to 40um; such as 30um to 60um. Fig.17D In another example shown in , it can be found that another observation is that the lithium lanthanum zirconium oxide (LLZO) material 1740 doped with aluminum (Al) is morphologically spherical clusters.
[0313] Table 16 illustrates the test results of capacitance and coulombic efficiency (CE) of examples of battery cells made of solid electrolyte materials after annealing process (Examples #30-35). The annealing temperature and annealing time can be controlled to be 700 to 1200°C for 7 to 20 hours. In Table 16, the battery made of lithium lanthanum zirconium oxide material (LLZO) particles appears to have different charge / discharge capacity cycling performance at different current / weight (mA / g), where 1C rate is equal to 200mA / g. In one example, the charge capacity ranges from 210 (mAh / g) to 255 (mAh / g); such as 215 (mAh / g) to 255 (mAh / g); such as 225 (mAh / g) to 255 (mAh / g); such as 235 (mAh / g) to 255 (mAh / g); such as 245 (mAh / g) to 255 (mAh / g). In another example, the charge capacity is greater than 205 (mAh / g), preferably greater than 210 (mAh / g), preferably greater than 215 (mAh / g), preferably greater than 220 (mAh / g), preferably greater than 225 (mAh / g), preferably greater than 230 (mAh / g), preferably greater than 235 (mAh / g), preferably greater than 240 (mAh / g), preferably greater than 245 (mAh / g), preferably greater than 250 (mAh / g), preferably greater than 255 (mAh / g). In another example, the discharge capacity ranges from 210 (mAh / g) to 255 (mAh / g); such as 215 (mAh / g) to 255 (mAh / g); such as 225 (mAh / g) to 255 (mAh / g); such as 235 (mAh / g) to 255 (mAh / g); such as 245 (mAh / g) to 255 (mAh / g). In another example, the discharge capacity is greater than 205 (mAh / g), preferably greater than 210 (mAh / g), preferably greater than 215 (mAh / g), preferably greater than 220 (mAh / g), preferably greater than 225 (mAh / g), preferably greater than 230 (mAh / g), preferably greater than 235 (mAh / g), preferably greater than 240 (mAh / g), preferably greater than 245 (mAh / g), preferably greater than 250 (mAh / g), preferably greater than 255 (mAh / g). It is found that the coulombic efficiency (CE, %) of the obtained solid electrolyte is greater than 96%, preferably greater than 96.5%, preferably greater than 97%, preferably greater than 97.5%, preferably greater than 98%, preferably greater than 98.5%, preferably greater than 99%, preferably greater than 99.5%, preferably greater than 99.6%, preferably greater than 99.7%, preferably greater than 99.8%, preferably greater than 99.9%.
[0314] Table 16: Measured electrical properties of lithium-ion battery cells made from exemplary solid electrolyte materials annealed at 850°C
[0315] Current / weight, mA / g Charging capacity, mAh / g Discharge capacity, mAh / g Coulombic efficiency, % 25 230.2972 222.7164 96.708 50 218.6137 216.4293 99.001 75 209.7601 208.8956 99.588 100 202.7414 202.0882 99.678 200 169.2282 168.9559 99.839 300 149.7479 149.2897 99.694 25 231.1816 226.6669 98.047
[0316] While the foregoing is directed to embodiments of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, and the scope thereof is determined by the appended claims.
Claims
1. A method for preparing a solid electrolyte (SSE) material, include: The first flow of the first gas is caused to flow in a stoichiometric amount with a lithium-containing salt, one or more metals D 1 , D 2 ,…,D N mixing with a liquid mixture of one or more inorganic salts; forming a gas-liquid mixture and ejecting a mist of said liquid mixture into a motive ejection chamber at a high motive velocity, delivering a second stream of heated gas into the motive jet chamber, drying the gas-liquid mixture for a first reaction period of less than 20 minutes to perform one or more oxidation reactions in the presence of a second gas stream and form a gas-solid mixture, conveying the gas-solid mixture out of the motive jet chamber, separating the gas-solid phase mixture into one or more solid particles of SSE material, delivering the one or more solid particles into an annealing chamber, and The one or more solid particles of the SSE material are annealed for a second reaction period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas flow and obtain a crystalline product, wherein the crystalline product of the SSE material is in the form of spherical clusters under scanning electron microscopy (SEM) analysis.
2. The method according to claim 1, further comprising: include: The crystallized product of the SSE material is ground to obtain nano-sized particles.
3. The method of claim 1, wherein the powdered particles are annealed in a dynamic crystallization process in the presence of an oxygen flow. The method according to claim 1 , wherein the first reaction time is less than 3 minutes.
5. The method according to claim 1, wherein the ionic conductivity (σ) of the crystallized product of the SSE material is greater than 10 at 25°C. -4 S / cm.
6. The method of claim 1, wherein the tap density of the SSE material is greater than 1.0 g / ml.
7. The method of claim 1, wherein the tap density of the SSE material is greater than 1.4 g / ml after annealing the SSE material at more than 900°C for more than 8 hours.
8. The method of claim 1, wherein the crystallized product is a garnet-type ceramic material having a cubic structure as measured by X-ray diffraction (XRD) analysis.
9. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and wherein the crystallized product of the SSE material as measured by X-ray diffraction (XRD) analysis is a garnet-type ceramic material having a cubic structure.
10. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and an aluminum-containing salt, and wherein the crystallized product of the SSE material as measured by X-ray diffraction (XRD) analysis is a garnet-type ceramic material having a cubic structure.
11. The method of claim 1 , wherein the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and wherein the crystallized product of the SSE material as measured by X-ray diffraction (XRD) analysis is a garnet-type ceramic material having a tetragonal structure.
12. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a tantalum-containing salt, and wherein the crystallized product of the SSE material as measured by X-ray diffraction (XRD) analysis is a garnet-type ceramic material having a cubic structure.
13. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, a lanthanum-containing salt, a titanium-containing salt, and wherein the crystallized product of the SSE material is a perovskite-type ceramic material.
14. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, an aluminum-containing salt, a phosphorus-containing salt, and wherein the crystallized product of the SSE material measured by X-ray diffraction (XRD) analysis is a sodium superionic conductor (NASICON) type ceramic material having a hexagonal structure.
15. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, a germanium-containing salt, and wherein the SSE material is a ceramic material.
16. The method of claim 1, wherein the liquid mixture comprises a lithium-containing salt, a sulfur-containing salt, and wherein the SSE material is a sulfide material.
17. The method according to claim 1, wherein D 1 , D 2 ,…,D N Selected from the group consisting of La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br and combinations thereof.
18. Basic requirements 1 Prescribed method, including free choice of pottery materials 7 La 3 Zr 2 O 12 , Li 6.75 La 3 Zr 1.75 Ta 0.25 O 12 , Li 6.5 La 3 Zr 2 Al 0.25 O 12 , Li 6.5 La 3 Zr 2 Al 0.24 O 12 , Li 6.5 La 3 Zr 2 Al 0.22 O 12 , Li 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35 , Li 6.74 La 2.96 Zr 2.0 Al 0.25 O 12.45 , Li 6.27 La 3.22 Zr 2.0 Al 0.3 O 12.39 , Li 6.4 La 2.86 Zr 2.0 Al 0.24 O 11.98 , Li 6.43 La 2.93 Zr 2.0 Al 0.24 O 12.08 , Li 6.32 La 3.2 Zr 2.0 Al 0.46 O 12.9 , Li 6.57 La 2.99 Zr 2.0 Al 0.22 O 12.22 , Li 6.4 La 3 Zr 2 Al 0.2 O 12 , Li 6.54 The 2.82 Zr 2.0 Al 0.24 The 12.08 、Li 6.49 The 3.28 Zr 2.0 Al 0.31 The 12.7 、Li 6.28 The 3 Zr 2 Al 0.24 The 12 、Li 6.25 The 3.01 Zr 2.0 Al 0.22 The 11.92 、Li 6.49 The 3.02 Zr 2.0 Al 0.23 The 12.2 、Li 6.5 The 3 Zr 1.5 The 0.5 The 12 、Li 6.15 The 3 Zr 1.75 The 0.25 Al 0.2 The 12 、Li 6.25 The 3 Zr 2 Al 0.25 The 12 、Li 6.15 The 3 Zr 1.75 The 0.25 Ga 0.2 The 12 、Li 6.25 The 3 Zr 2 The 0.25 Ga 0.2 The 12 、Li 6.4 The 3 Zr 2 Ga 0.2 The 12 、Li 6.4 The 3 Zr 1.4 The 0.6 The 12 and its combination of composition.
19. The method according to claim 1, further comprising: include: sintering the crystallized product of the ceramic material at an annealing temperature above 900°C to further process the ceramic material, and Measures the ionic conductivity of ceramic materials.
20. A method for preparing a solid electrolyte material, include: The stoichiometric amount of lithium salt, lanthanum salt, zirconium salt and one or more metal D is formed. 1 , D 2 ,…,D N a liquid mixture of one or more inorganic salts to mix with the first gas stream to form a gas-liquid mixture; spraying a mist of the liquid mixture into a power spray chamber; drying the gas-liquid mixture for a first reaction time period of less than 20 minutes to carry out one or more oxidation reactions in the presence of a second stream of heated gas and form a gas-solid mixture; conveying the gas-solid mixture out of the motive jet chamber; separating the gas-solid mixture into one or more solid particles of SSE material; delivering the one or more solid particles into an annealing chamber, and Annealing one or more solid particles of the SSE material for a second reaction period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas stream to obtain a crystalline product; wherein the final crystalline product of the SSE material has an ionic conductivity (σ) greater than 10 measured at 25° C. -4 S / cm, chemical composition is Li a La b Zr c D1 d D2 e …DN n O v Ceramic material, wherein 6.2≤a≤7.2, 2.8≤b≤3.5, 1.2≤c≤2.2, 2.0≤v≤12, and wherein D 1 , D 2 ,…,D N At least one of them is a metal, N≥0, 0≤d≤0.8, 0≤e≤0.8 and 0≤n≤0.
8.
21. The method of claim 20, wherein the SPAN value (D 90 -D 10 ) / D 50 0.8 <SPAN≤1.0。 22. The method of claim 20, wherein the SPAN value (D 90 -D 10 ) / D 50 0.8 <SPAN≤1.7。 23. The method of claim 20, wherein after annealing, the D 50 10μm to 18μm.
24. The method of claim 20, wherein after annealing, the D 90 20μm to 40μm, D 10 3μm to 10μm, D 99 is 35μm to 60μm, and D 1 0.1μm to 3μm.
25. A method for preparing a solid electrolyte material, include: The first flow of the first gas is caused to flow in a stoichiometric amount with a lithium-containing salt, one or more metals D 1 , D 2 ,…,D N a liquid mixture of one or more inorganic salts, forming a gas-liquid mixture and ejecting a mist of the liquid mixture into a kinetic ejection chamber at a high kinetic velocity, delivering a second stream of heated gas into the motive jet chamber, drying the gas-liquid mixture for a first reaction period of less than 20 minutes to perform one or more oxidation reactions in the presence of a second gas stream and form a gas-solid mixture, conveying the gas-solid mixture out of the motive jet chamber, separating the gas-solid mixture into one or more solid particles of SSE material, delivering the one or more solid particles into an annealing chamber, annealing the one or more solid particles of the SSE material for a second reaction period of more than 2 hours to perform a dynamic crystallization process in the presence of a third gas stream and obtain a crystalline product, and The crystallized product of the ceramic material is ground to obtain nano-sized particles, and the crystallized product of the SSE material is in the form of spherical clusters under scanning electron microscope (SEM) analysis.
Citation Information
Cited By
Solid electrolyte with surface ion transmission mechanism and application of solid electrolyte