Carbon-doped 2H-phase molybdenum disulfide and preparation method thereof
By calcining molybdenum trioxide and vulcanizing agent in a carbon disulfide and argon atmosphere, and then vulcanizing with sulfur powder, the doping and layering process of molybdenum disulfide is successfully simplified, and the problem of poor product consistency is solved, and efficient carbon doping is achieved The preparation of hetero 2H phase molybdenum disulfide improves ion transport efficiency and conductivity.
Patent Information
- Application Number
- CN202411403520.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the doping and layer expansion process steps of molybdenum disulfide are complicated, and the product consistency is poor, making it difficult to achieve large-scale preparation.
Molybdenum trioxide and a sulfurizing agent are mixed and calcined in an atmosphere of carbon disulfide and argon to obtain a carbon-doped molybdenum sulfur oxide composite material, and then sulfur powder is sulfidized to obtain carbon-doped 2H-phase molybdenum disulfide, which is achieved through preliminary vulcanization and subsequent vulcanization A block structure with large layer spacing.
The preparation process is simplified, product consistency is improved, and faster ion transport efficiency and conductivity are obtained, which is suitable for large-scale production.
Smart Images

Figure CN119018936A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of synthetic material preparation, and in particular to carbon-doped 2H-phase molybdenum disulfide and a preparation method thereof. Background Art
[0002] MoS2 has a graphite-like 2D layered structure with a large interlayer spacing. The layers are connected by van der Waals forces to ensure stable ion embedding. It can also be intercalated and exfoliated. It is polycrystalline and its crystal structure and electronic properties can be regulated, which makes MoS2 have more physical and chemical properties and applications. In the MoS2 phase structure, the 2H structure is stable, but the conductivity of the semiconductor phase is poor. Currently, the modification of MoS2 is mainly doping and layer expansion. However, in the related methods, there are problems such as cumbersome experimental steps and poor consistency of the obtained products, making it difficult to achieve large-scale preparation. Summary of the invention
[0003] The main purpose of the present invention is to provide a carbon-doped 2H phase molybdenum disulfide and a preparation method thereof, so as to solve the technical problems that the process steps of doping and expanding the molybdenum disulfide are complicated and the product consistency is poor.
[0004] To achieve the above object, the present invention provides a method for preparing carbon-doped 2H phase molybdenum disulfide, comprising the following steps: Molybdenum trioxide and a sulfurizing agent are mixed and ground, and calcined in a carbon disulfide and argon atmosphere to obtain a carbon-doped molybdenum oxysulfide composite material, wherein the carbon-doped molybdenum oxysulfide composite material is marked as MoOS-C; The MoOS-C is sulfurized with sulfur powder to obtain carbon-doped 2H phase molybdenum disulfide.
[0005] In some embodiments of the present invention, the type of the vulcanizing agent includes thiocyanuric acid.
[0006] In some embodiments of the present invention, the mass ratio of the molybdenum trioxide to the sulfurizing agent is in the range of 1:3 to 1:9.
[0007] In some embodiments of the present invention, in the calcination step, the calcination temperature ranges from 500°C to 700°C.
[0008] In some embodiments of the present invention, in the calcination step, the calcination time is 1.5h~3h.
[0009] In some embodiments of the present invention, in the calcination step, the calcination heating rate is (3-8)°C / min.
[0010] In some embodiments of the present invention, the mass ratio of the sulfur powder to MoOS-C is 1:8-1:12.
[0011] In some embodiments of the present invention, in the vulcanization step, the vulcanization temperature is 500° C. to 700° C.; and / or the vulcanization time is 3 h to 5 h.
[0012] In some embodiments of the present invention, in the vulcanization step, the vulcanization heating rate is (3-8)°C / min.
[0013] A second aspect of the present invention provides carbon-doped 2H-phase molybdenum disulfide prepared by the method for preparing carbon-doped 2H-phase molybdenum disulfide as described above.
[0014] The present invention also provides a battery negative electrode, which comprises the carbon-doped 2H-phase molybdenum disulfide of the present invention.
[0015] The present invention also provides a battery, wherein the battery negative electrode comprises the battery negative electrode as described above.
[0016] In some embodiments of the present invention, the battery comprises a lithium-ion battery.
[0017] The beneficial effects that can be achieved by the present invention are: The present invention uses a sulfurizing agent to sulfurize molybdenum trioxide in a carbon disulfide atmosphere to obtain a carbon-doped molybdenum oxysulfide composite material, and then uses sulfur powder to sulfurize to obtain carbon-doped 2H phase molybdenum disulfide. Preliminary sulfurization and carbon doping are first performed, and then subsequent sulfurization is performed with sulfur powder. It is easy to obtain carbon-doped 2H phase molybdenum disulfide with a large interlayer spacing and a dense bulk structure, thereby obtaining faster ion transmission efficiency, better electrical conductivity and structural stability. In addition, the synthesis method is simple and efficient, the obtained product has good consistency, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0019] Figure 1 The figure is a schematic diagram of a process for preparing carbon-doped 2H-phase molybdenum disulfide according to an embodiment of the present invention.
[0020] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0021] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0024] The present invention provides a method for preparing carbon-doped 2H phase molybdenum disulfide, referring to Figure 1 , including the following steps: S10: mixing molybdenum trioxide and a sulfurizing agent, grinding them, and calcining them in a carbon disulfide and argon atmosphere to obtain a carbon-doped molybdenum oxysulfide composite material, and the carbon-doped molybdenum oxysulfide composite material is recorded as MoOS-C; S20: Sulfurization of MoOS-C with sulfur powder to obtain carbon-doped 2H phase molybdenum disulfide.
[0025] In step S10, molybdenum trioxide and a sulfurizing agent are calcined in a carbon disulfide and argon atmosphere to obtain a carbon-doped molybdenum oxysulfide composite material MoOS-C. In step S20, MoOS-C is sulfurized with sulfur powder to obtain carbon-doped 2H-phase molybdenum disulfide. The obtained carbon-doped 2H-phase molybdenum disulfide has a wider interlayer spacing, can obtain better conductivity and faster ion transfer efficiency, and in addition, the carbon-doped 2H-phase molybdenum disulfide also has a dense bulk structure, which can obtain higher structural stability.
[0026] In some embodiments, the type of the vulcanizing agent in step S10 includes thiocyanuric acid.
[0027] In some embodiments, the mass ratio of molybdenum trioxide to the sulfurizing agent ranges from 1:3 to 1:9, and can be any ratio in the range of 1:3 to 1:9, such as 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, etc., under the above ratio range conditions.
[0028] In some embodiments, in the calcination step, the calcination temperature ranges from 500°C to 700°C; and / or the calcination time is 1.5h to 3h, which can be any value in the range of 1.5h to 3h, such as 1.5h, 2h, 2.5h, 3h, etc. Within the above calcination temperature range, it is beneficial to promote the sulfurization and carbon doping of molybdenum trioxide to obtain a carbon-doped molybdenum oxysulfide composite material MoOS-C.
[0029] In some embodiments, in the calcination step, the calcination heating rate is (3~8)℃ / min, which can be any value in the range of (3~8)℃ / min, such as 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, etc.
[0030] In some embodiments, the mass ratio of sulfur powder to MoOS-C is 1:8-1:12, and can be any ratio in the range of 1:8-1:12, such as 1:8, 1:9, 1:10, 1:11, 1:12, etc.
[0031] In some embodiments, in the vulcanization step, the vulcanization temperature is 500°C to 700°C, and can be any value in the range of 500°C to 700°C, such as 500°C, 550°C, 600°C, 650°C, 700°C, etc.
[0032] In some embodiments, in the vulcanization step, the vulcanization time is 3 h to 5 h, and can be any value within the range of 3 h to 5 h, such as 3 h, 3.5 h, 4 h, 4.5 h, 5 h, etc.
[0033] In some embodiments, in the vulcanization step, the vulcanization heating rate is (3~8)℃ / min, which can be any value in the range of (3~8)℃ / min, such as 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, etc.
[0034] In some embodiments, the calcination in step S10 and the sulfidation in step S20 are both performed in a furnace.
[0035] In the present invention, the molybdenum trioxide in step S10 can be purchased commercially, or prepared by the following steps: grinding ammonium molybdate tetrahydrate into powder, putting it into a porcelain boat, and calcining it in an F muffle furnace at 550° C. to 600° C. for 2 h to 3 h to obtain molybdenum trioxide.
[0036] The present invention also provides a battery negative electrode, which includes the carbon-doped 2H-phase molybdenum disulfide of the present invention. The battery negative electrode of the present invention at least has all the beneficial effects of the carbon-doped 2H-phase molybdenum disulfide.
[0037] The present invention also provides a battery, wherein the negative electrode of the battery comprises the negative electrode of the battery as described above and has at least all the beneficial effects of carbon-doped 2H phase molybdenum disulfide.
[0038] Carbon-doped 2H phase molybdenum disulfide has a large interlayer spacing and a dense bulk structure. When applied to batteries, it can help the batteries achieve faster ion transfer efficiency, better conductivity and stability, which is beneficial to improving the battery's first coulombic efficiency, first charging capacity, and residual capacity after 100 cycles.
[0039] In some embodiments of the present invention, the battery comprises a lithium-ion battery.
[0040] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0041] Example 1 The preparation method of carbon-doped 2H phase molybdenum disulfide in this embodiment is as follows: S10: 0.5 g of molybdenum trioxide and 1.5 g of sulfurizing agent trithiocyanate were mixed and ground into powder, placed in a porcelain boat, and placed in an F muffle furnace and heated to 600 °C at a heating rate of 5 °C / min for calcination for 2 h to obtain a carbon-doped molybdenum oxysulfide composite material, marked as MoOS-C.
[0042] S20: Take 0.3 g of sulfur powder and mix it with 3 g of MoOS-C in step S10, put it in a porcelain boat, put it into an F muffle furnace and heat it to 600° C. at a heating rate of 5° C. / min for calcination and sulfurization to obtain carbon-doped 2H phase molybdenum disulfide.
[0043] Example 2 Example 2 Carbon-doped 2H-phase molybdenum disulfide was prepared by referring to the preparation method of Example 1, except that in step S10 of Example 2, the mass ratio of molybdenum trioxide to the vulcanizing agent trithiocyanate was 1:6.
[0044] Example 3 Example 3 Carbon-doped 2H phase molybdenum disulfide was prepared by referring to the preparation method of Example 1, except that in step S10 of Example 3, the mass ratio of molybdenum trioxide to the vulcanizing agent trithiocyanate was 1:9.
[0045] Example 4 Example 3 Carbon-doped 2H phase molybdenum disulfide was prepared by referring to the preparation method of Example 1, except that in step S10 of Example 4, the temperature was raised to 500° C. at a heating rate of 5° C. / min for calcination.
[0046] Example 5 Example 5 Carbon-doped 2H phase molybdenum disulfide was prepared by referring to the preparation method of Example 1, except that in step S20 of Example 5, the temperature was raised to 700° C. at a heating rate of 5° C. / min for calcination and sulfurization.
[0047] Comparative Example 1 Comparative Example 1: 0.3 g of sulfur powder and 0.5 g of molybdenum trioxide were mixed and ground into powder, placed in a porcelain boat, and placed in an F muffle furnace and heated to 600° C. at a heating rate of 5° C. / min for calcination and sulfurization to obtain a product.
[0048] Application Testing The products of Examples 1 to 5 and Comparative Example 1 were used as active materials for the negative electrode of a lithium-ion battery, mixed with a conductive agent (Super-P) and a binder polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1, and N-methylpyrrolidone (NMP) was used as a solvent. After grinding, the mixture was evenly coated on a copper foil and dried in a vacuum oven at 80°C for 12 h. The electrode sheet was cut into discs with a diameter of about 1.2 cm. A metal lithium sheet was used as a counter electrode. 1.0 M LiPF6-EC / DMC / EMC (1:1:1 vol%) was used as the electrolyte. The cells were assembled into button batteries in an inert argon atmosphere glove box.
[0049] The test operating voltage window is 0.01-3.0 V, and the current density is 0.5 A / g. Table 1 is a performance comparison of Examples 1-5 and Comparative Example 1.
[0050] Table 1
[0051] It can be seen from Table 1 that the carbon-doped 2H phase molybdenum disulfide prepared in Examples 1 to 5 is used as the active material of the battery negative electrode. The carbon-doped 2H phase molybdenum disulfide has a large interlayer spacing and a dense bulk structure, and can obtain faster ion transmission efficiency, better conductivity function and structural stability. The corresponding prepared batteries obtain better first coulomb efficiency, first charge capacity and cycle performance, which are all better than those of Comparative Example 1.
[0052] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing carbon-doped 2H phase molybdenum disulfide, characterized in that: The following steps are involved: Molybdenum trioxide and a sulfurizing agent are mixed and ground, and calcined in a carbon disulfide and argon atmosphere to obtain a carbon-doped molybdenum oxysulfide composite material, wherein the carbon-doped molybdenum oxysulfide composite material is marked as MoOS-C; The MoOS-C is sulfurized with sulfur powder to obtain carbon-doped 2H phase molybdenum disulfide.
2. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: The vulcanizing agent includes thiocyanuric acid.
3. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: The mass ratio of the molybdenum trioxide to the sulfurizing agent is in the range of (1:3) to (1:9).
4. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: In the calcination step, the calcination temperature ranges from 500°C to 700°C.
5. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: In the calcination step, the calcination time is 1.5h~3h.
6. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: In the calcination step, the calcination heating rate is (3-8)°C / min.
7. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: The mass ratio of the sulfur powder to MoOS-C is (1:8) to (1:12).
8. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: In the vulcanization step, the vulcanization temperature is 500° C. to 700° C.; and / or the vulcanization time is 3 h to 5 h.
9. The method for preparing carbon-doped 2H phase molybdenum disulfide according to claim 1, characterized in that: In the vulcanization step, the vulcanization heating rate is (3-8)°C / min.
10. Carbon-doped 2H-phase molybdenum disulfide prepared by the method for preparing carbon-doped 2H-phase molybdenum disulfide according to any one of claims 1 to 9.