Enhanced mineral powder grinding aid and preparation method thereof
By optimizing the component design and proportion of ore powder aids, the problems of unstable effects and high costs in the existing technology are solved, and the grinding efficiency and hydration activity of ore powder are significantly improved, meeting the needs of green building materials. .
Patent Information
- Application Number
- CN202411064126.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ore powder aids have problems such as unstable effects, narrow application scope and high cost in improving grinding efficiency and hydration activity, which are difficult to meet the needs of green building materials.
By optimizing the component design and ratio of the abrasive agent, the polyether monomer is prepared by reacting alcohol heads with epoxy monomers, the defect inducer is prepared by reacting amine heads with cyclic monomers, and the dispersion correction components are used to form 50% concentration of enhanced ore powder aid, adjust the grafting ratio of ethylene oxide and propylene oxide to improve particle fineness and hydration strength.
It significantly improves the fineness and particle size distribution of ore powder particles, enhances hydration activity, reduces grinding energy consumption, improves the mechanical properties and durability of concrete, and expands the scope of application of grinding aids.
Smart Images

Figure BDA0004978877410000051 
Figure BDA0004978877410000061 
Figure BDA0004978877410000071
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to a mineral powder grinding aid and a preparation method thereof. Background Art
[0002] In the cement and concrete industry, mineral powder is an important industrial by-product and is widely used due to its excellent hydraulic properties and environmental protection characteristics. However, the special glass structure of mineral powder leads to low grinding efficiency, high energy consumption, and increased production costs. In recent years, with the in-depth promotion of the concept of green manufacturing, the development of efficient and environmentally friendly mineral powder grinding aids has become a research hotspot in the industry. Ideal grinding aids can not only significantly improve the grinding efficiency of mineral powder and reduce energy consumption, but also enhance the hydration activity of mineral powder and improve the mechanical properties and durability of concrete.
[0003] There are many types of mineral powder grinding aids on the current market, mainly including organic grinding aids, inorganic grinding aids and their composite systems. Organic grinding aids such as lignin sulfonates, polycarboxylates, etc. have good dispersibility and lubrication, can effectively improve the fluidity of mineral powder particles, and reduce energy consumption during the grinding process. Inorganic grinding aids such as silicates, sulfates, etc., promote the activation of mineral powder and increase its hydration rate through chemical reactions with the surface of mineral powder. However, the existing grinding aid system still has certain limitations, such as unstable grinding effect, narrow scope of application, high cost and other problems. It is urgent to develop new, efficient, broad-spectrum and economical mineral powder grinding aids to meet the growing demand for green building materials.
[0004] CN105154007A discloses a method for preparing and using a mineral powder grinding aid mother liquor, comprising the following steps: preparing an amine oxide derivative and a quaternary ammonium salt derivative, and uniformly mixing them with a certain mass fraction of glycerol, molasses, and water. The design concept of the grinding aid is consistent with that of the alcoholamine grinding aid, both of which provide electron pairs for adsorption through N, and the hydrophobic group ensures particle dispersion. Due to the lack of groups that provide a crushing effect in the structure, the optimization effect of the particle fineness and gradation is limited.
[0005] CN117753538A provides a special grinding aid for mineral powder and a preparation method thereof, comprising a modified crystal nucleus early strength agent, a polymerized polyol, a styrene-maleic anhydride copolymer and water, wherein the early strength agent is compounded by an propylene alcohol polyether polyol and a polycarboxylic acid water reducer, and can provide a good dispersion effect; the styrene-maleic anhydride copolymer has sufficient carboxyl groups and benzene rings in its structure, which respectively play the role of adsorption and crushing, and thus has a good mineral powder grinding aid effect.
[0006] The present invention aims to address the deficiencies of the prior art and propose a new type of mineral powder grinding aid. By optimizing the component design and ratio of the grinding aid, the fineness and particle size distribution of the mineral powder particles can be significantly optimized while taking into account the hydration strength, thereby providing strong technical support for the sustainable development of the cement and concrete industries. Summary of the invention
[0007] The present invention provides an enhanced mineral powder grinding aid and a preparation method thereof. Aiming at the low activity and poor grindability of mineral powder, the technical scheme of the present invention is as follows:
[0008] (1) Preparation of dispersant
[0009] Step 1: Add 19.11-31.48 parts of alcohol head and 1.0-2.2 parts of catalyst into the autoclave, replace with nitrogen several times, start to evacuate to a gauge pressure of -0.1MPa, then heat to 120-130°C and start dehydration for 1-2h, then cool to 115°C and start to continuously and uniformly introduce 193.21-195.50 parts of cyclic monomers, control the pressure to be less than 0.4MPa, keep warm at 110-120°C for 1.5-2.5h to react to negative pressure, cool and discharge to obtain a polyether monomer;
[0010] Step 2: Add the prepared polyether monomer to the reaction kettle, heat it to 55-65°C in a water bath and keep it warm; prepare 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water to make liquid A; prepare 89.16-97.32 parts of ether substance, 3.2-7.9 parts of reducing agent and water to make liquid B; drip liquid A and liquid B at the same time, wherein liquid A is dripped for 2-2.5 hours and liquid B is dripped for 1.5-2 hours; keep the temperature for 1 hour after the dripping of liquid A, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a dispersant mother liquor with a concentration of 30%. The several parts of polyether monomer prepared in step 1 are adjusted in a certain proportion according to the required amount in step 2, so as to control the concentration of the dispersant mother liquor obtained by the reaction to be always controlled at 30%, which reduces the workload for subsequent compounding and other work.
[0011] (2) Preparation of defect-inducing agents
[0012] Step 1: Add 128.61-207.73 parts of amine heads into a high-pressure reactor, raise the temperature to 120°C while evacuating, and the pressure in the reactor is 0.2-0.3MPa. The material in the reactor is sucked out from the reactor and then sprayed into the reactor from the top. At the same time, add cyclic monomers. After a period of circulation, cool to 90-100°C.
[0013] Step 2: Add 1.0-2.2 parts of catalyst and replace with nitrogen to start vacuuming to a gauge pressure of -0.1MPa, then raise the temperature to 120°C. Start to introduce the remaining cyclic monomer into the reactor, introduce 92.28-171.39 parts of cyclic monomer into the reactor, control the pressure to be less than 0.4MPa, keep circulating spray for 2.0-2.5h after all the cyclic monomers are introduced into the reactor, keep warm for 1h after the reaction is completed, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a defect inducing agent mother liquor with a concentration of 30%.
[0014] (3) Preparation of dispersion correction components
[0015] 129.31-208.33 parts of carboxyl heads and 1.0-2.2 parts of catalysts are added to a high-pressure reactor. After nitrogen replacement for several times, vacuum is started to be drawn to a gauge pressure of -0.1 MPa, and then the temperature is raised to 130-140°C and maintained for 60 minutes, and then the temperature is raised to 140°C and maintained at this temperature. The reaction pressure is maintained at 0.3 MPa by controlling the introduction rate of cyclic monomers. When the total amount of cyclic monomers introduced is 91.66-170.70 parts, the material is stopped, and a aging reaction is carried out at 140°C until the pressure no longer decreases, and a vacuum treatment is carried out at a pressure of -0.09 MPa for 30 minutes, and then the temperature is reduced to 40°C for discharging, and 5.9-9.4 parts of a neutralizer are added at one time and then water is added to 1000 parts to obtain a mother liquor with a concentration of 30%.
[0016] (4) Preparation of production-enhancing mineral powder grinding aids
[0017] The prepared dispersant mother solution, defect inducing agent mother solution, dispersion correction component mother solution and polymeric polyol are compounded in a certain proportion and water is added to 1000 parts to obtain the enhanced mineral powder grinding aid mother solution with a concentration of 50%.
[0018] Preferably, the alcohol head is 3-methyl-2-butene-1-ol.
[0019] Preferably, the catalyst is one of sodium hydroxide, potassium hydroxide and sodium methoxide, and sodium methoxide is most preferred.
[0020] Preferably, the cyclic monomer is ethylene oxide.
[0021] Preferably, the initiator is one of ammonium persulfate, diisopropyl peroxydicarbonate, and dihexyl peroxydicarbonate, and dihexyl peroxydicarbonate is most preferred; the chain transfer agent is one of thioglycolic acid, mercaptoethanol, and mercaptopropionic acid, and mercaptoethanol is most preferred; the ether substance is diethylene glycol monoallyl ether or poly 1,2-propylene glycol, and diethylene glycol monoallyl ether is most preferred.
[0022] Preferably, the amine head is N-ethylmethyl propylene amine; the reducing agent is sodium hypophosphite; the neutralizing agent is potassium carbonate; and the carboxyl head in the dispersion correction component is tiglic acid.
[0023] Preferably, the alcohol-ether molar ratio is 2.1-3:1, most preferably 2.2:1.
[0024] Preferably, the polymeric polyol is composed of several of ethylene glycol, glycerol, trimerpropylene glycol and triethanolamine.
[0025] Preferably, the mass ratio of the dispersant, the defect inducer, the correction component and the polymeric polyol is 3:1:1:3.
[0026] The inventive concept of the present invention is as follows:
[0027] The present invention is mainly based on the functional design of polymers based on the reaction of hydroxyl groups of alcohol heads with epoxy monomers. Hydroxyl groups and epoxy groups are etherified to synthesize polymers with molecular weights of about 8,000 to 10,000. Ethylene oxide and propylene oxide are selected as epoxy materials. The number of methyl groups is adjusted by adjusting the grafting ratio of ethylene oxide and propylene oxide. Studies have found that methyl groups have a certain effect of improving the particle size and particle fineness, and the number of methyl groups is adjusted according to the ratio of the two epoxides.
[0028] N-ethylmethyl propylene amine is reacted with epoxide to prepare a low molecular weight substance with a molecular weight of about 100 to 300, which is a defect inducing agent. The terminal amine group in the molecular structure has the same effect as that of alcohol amine, that is, the amine group can give electron pairs to form an adsorption layer on the surface of solid particles, so that the surface charge of the particles is increased, and its solvated part is effectively diffused into the dispersion medium, which increases the depth of the solid particles being wetted by the solvent, so that the solid particles are separated by the electrostatic repulsion, and the agglomeration of the solid particles is effectively prevented. Tigris acid is reacted with epoxide to prepare a low molecular weight substance with a molecular weight of about 100 to 300, which is a dispersion correction component. It has a carbonyl group and an ether bond, and can form a hydrogen bond with a polymerized polyol. The hydrogen bond is a weak intermolecular force, so the dispersion correction component has physical adsorption properties and can be well desorbed, and is a non-directional adsorbent. Since Tigris acid has a methyl group, it can play a dispersing role. The combined adsorption and dispersing properties can play a dispersing performance correction function.
[0029] Defect inducing agents and dispersion correction components are both small molecules, which can avoid the occurrence of undesirable phenomena such as competitive adsorption with dispersants, which ultimately lead to the failure of grinding aid performance. Small molecules are adsorbed before dispersants, providing defects and synergistic dispersion for small single particles and cracks, while dispersant macromolecules disperse multiple particles. The synergistic effect of the three can effectively exert a significant grinding enhancement effect.
[0030] The beneficial effects of the present invention are as follows:
[0031] 1. The grinding aid provided by the present invention can adjust the number of methyl groups by adjusting the grafting ratio of ethylene oxide and propylene oxide, and its action range is wider and the grinding aid effect is better.
[0032] 2. The grinding aid provided by the present invention can give out electron pairs through the amino group, forming an adsorption layer on the surface of solid particles, thereby increasing the surface charge of the particles. The solvated part thereof effectively diffuses into the dispersion medium, increasing the depth of the solid particles being wetted by the solvent, and keeping the solid particles away from each other due to the electrostatic repulsion, thereby effectively preventing the agglomeration of the solid particles.
[0033] 3. The grinding aid provided by the present invention uses a dispersion correction component, which is a small molecule substance and has a carbonyl group and an ether bond, and can form a hydrogen bond. The hydrogen bond is a weak intermolecular force, so the dispersion correction component has physical adsorption performance and can be well desorbed and is a non-directional adsorbent. And because tiglic acid has a methyl group, it can play a dispersing role, and the combined adsorption performance and dispersing effect can play a dispersing performance correction function. DETAILED DESCRIPTION
[0034] The applicant will further explain the technical scheme and beneficial effects of the present invention in detail in conjunction with specific embodiments, but it should be understood that the following embodiments should not be construed as limiting the scope of protection claimed in the claims of the present application to any extent. A slag grinding aid with a mass fraction of 0.03% is added to a sample of 96% slag and 4% gypsum totaling 5 kg. The specific steps are: the grinding aids prepared in Examples 1-6 in Table 1 are added at a total mass of 0.03% and put into a ball mill. The grinding time is 80 minutes. After the grinding is completed, a series of tests are performed on the particles to evaluate their grinding aid performance.
[0035] Activity index determination: According to GB / T 18046-2008 "Granulated blast furnace ore powder for cement, mortar and concrete", the compressive strength of the test examples and the commercially available sample (Hongxin HX-ZQY grinding aid) at the corresponding age is measured, and the ratio of the two is the activity index; fineness test: FSY-150 cement fineness negative pressure sieve analyzer is used to measure the 45μm sieve residue of the ore powder after grinding of each example and comparative example; specific surface area test: According to GB / T8074-2008 "Method for determination of specific surface area of cement", FBT-9 cement Blair fully automatic specific surface area measuring instrument is used for determination; particle size distribution: Mastersizer3000 laser particle size analyzer is used for determination. After detection, the experimental results are shown in Tables 3 and 4.
[0036] Table 1 Preparation raw material composition of enhanced grinding aid
[0037]
[0038]
[0039]
[0040] Table 2 Preparation process of enhanced grinding aid
[0041]
[0042]
[0043] Table 3 Test results of mineral powder grinding aid performance
[0044]
[0045] Table 4 Particle size distribution test results
[0046]
[0047]
[0048] As shown in Table 3, compared with commercially available grinding aids, at a lower dosage, the mineral powder grinding aids prepared in Examples 1 and 6 have a more significant improvement effect on the particle specific surface and fineness, and the reduction in particle fineness has a positive effect on hydration activity, making the low-activity rubber material contact area with water larger, promoting the hydration reaction process, so the 3d and 28d strengths are significantly improved. Combined with the particle size distribution data in Table 4, the enhanced mineral powder grinding aid provided by the present invention has a significant increase in the volume fraction of 0-3μm particles, and a slight increase in the volume fraction of 3-32μm particles. 0-32μm particles are considered to be the main part of the strength, so the grinding aid provided by the present invention can reduce the mineral powder fineness and improve its hydration activity, thereby exerting a significant enhancement effect.
[0049] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an enhanced mineral powder grinding aid, characterized in that: The parts are all parts by mass, comprising the following steps: (1) Preparation of dispersant Step 1: Add 19.11-31.48 parts of alcohol head and 1.0-2.2 parts of catalyst into the autoclave, replace with nitrogen several times, start to evacuate to a gauge pressure of -0.1MPa, then heat to 120-130°C and start dehydration for 1-2h, then cool to 115°C and start to continuously and uniformly introduce 193.21-195.50 parts of cyclic monomers, control the pressure to be less than 0.4MPa, keep warm at 110-120°C for 1.5-2.5h to react to negative pressure, cool and discharge to obtain a polyether monomer; Step 2: Add the prepared polyether monomer into a reaction kettle, heat it to 55-65°C in a water bath and then keep it warm; prepare liquid A by adding 5.6-8.6 parts of an initiator, 1.2-4.8 parts of a chain transfer agent and water; prepare liquid B by adding 89.16-97.32 parts of an ether substance, 3.2-7.9 parts of a reducing agent and water; add liquid A and liquid B dropwise at the same time, wherein liquid A is added dropwise for 2-2.5 hours and liquid B is added dropwise for 1.5-2 hours; after liquid A is added dropwise, keep it warm for 1 hour, add 5.9-9.4 parts of a neutralizer at one time and add water to 1000 parts to obtain a dispersant mother solution with a concentration of 30wt%; (2) Preparation of defect-inducing agents Step 1: Add 128.61-207.73 parts of amine heads into a high-pressure reactor, raise the temperature to 120°C while evacuating, and the pressure in the reactor is 0.2-0.3MPa. The material in the reactor is sucked out from the reactor and then sprayed into the reactor from the top. At the same time, add the cyclic monomer. After a period of circulation, cool to 90-100°C. Step 2: Add 1.0 to 2.2 parts of catalyst and replace with nitrogen to start vacuuming to a gauge pressure of -0.1 MPa, then heat to 120°C, start introducing the remaining cyclic monomer into the reactor, introduce 92.28 to 171.39 parts of cyclic monomer into the reactor, control the pressure to be less than 0.4 MPa, maintain circulating spraying for 2.0 to 2.5 hours after all the cyclic monomers are introduced into the reactor, keep warm for 1 hour after the reaction is completed, add 5.9 to 9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a defect inducing agent mother liquor with a concentration of 30wt%; (3) Preparation of dispersion correction components Add 129.31-208.33 parts of carboxyl head and 1.0-2.2 parts of catalyst into a high-pressure reactor, and start to evacuate to a gauge pressure of -0.1MPa after nitrogen replacement for several times, then heat to 130-140°C and keep for 60 minutes, then heat to 140°C and maintain this temperature, keep the reaction pressure at 0.3MPa by controlling the introduction rate of cyclic monomers, stop feeding when the total amount of cyclic monomers introduced is 91.66-170.70 parts, carry out aging reaction at 140°C until the pressure no longer decreases, and carry out vacuum treatment at a pressure of -0.09MPa for 30 minutes, then reduce the temperature to 40°C and discharge, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a mother liquor with a concentration of 30wt%; (4) Preparation of mineral powder grinding aid The prepared dispersant mother liquor, defect inducing agent mother liquor, dispersing correction component mother liquor and polymeric polyol are compounded in a certain proportion, and water is added to 1000 parts to obtain the enhanced mineral powder grinding aid mother liquor with a concentration of 50wt%. The enhanced mineral powder grinding aid mother liquor is diluted at 1:29 to obtain the enhanced mineral powder grinding aid working solution.
2. The method according to claim 1, characterized in that: The alcohol head is 3-methyl-2-butene-1-ol.
3. The method according to claim 1, characterized in that: The catalyst is one of sodium hydroxide, potassium hydroxide and sodium methoxide.
4. The method according to claim 1, characterized in that: The cyclic monomer is ethylene oxide.
5. The method according to claim 1, characterized in that: The initiator is one of ammonium persulfate, diisopropyl peroxydicarbonate and dihexyl peroxydicarbonate; the chain transfer agent is one of thioglycolic acid, mercaptoethanol and mercaptopropionic acid; and the ether substance is diethylene glycol monoallyl ether or poly 1,2-propylene glycol.
6. The method according to claim 1, characterized in that The amine head is N-ethylmethyl propylene amine; the reducing agent is sodium hypophosphite; the neutralizing agent is potassium carbonate; and the carboxyl head in the dispersion correction component is tiglic acid.
7. The method according to claim 1, characterized in that The alcohol-ether molar ratio is 2.1-3:
1.
8. The method according to claim 1, characterized in that: The molar ratio of the dispersant, the defect inducing agent, the dispersion correction component and the polymeric polyol is 3:1:1:
3.
9. The method according to claim 1, characterized in that: The polymeric polyol is composed of several of ethylene glycol, glycerol, trimeryl glycol and triethanolamine.
10. An enhanced mineral powder grinding aid, characterized in that: The method is prepared by any one of claims 1 to 9.