Grouting material for filling flowing water in tunnel karst cave and preparation method of grouting material
By using the combination of modified basalt fibers and bentonite in the grouting materials, the problem of insufficient anti-moving water dispersion ability of existing grouting materials in karst areas is solved, and efficient anti-seepage plugging and filling in water-moving environments is achieved. Effect.
Patent Information
- Application Number
- CN202310607165.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing grouting materials have insufficient anti-driving water dispersion capacity during tunnel construction in karst areas, are prone to loss, cannot effectively fill and seal, and have poor fiber dispersion.
Modified basalt fibers and bentonite are used to adopt 10-15 parts by mass of bentonite, 35-45 parts by mass of silicate cement, 1-4 parts by mass of modified basalt fibers and 0.5-1 part by mass of lignin water reducing agent. The synergistic effect of the mixture is to form a grouting material with superior underwater stability, dilution resistance and high strength. The modified basalt fibers are modified by silane coupling agent in anhydrous ethanol solution to improve the fiber dispersion and anti-shrinking properties.
It has achieved the improvement of the durability and anti-shrinking performance of grouting materials in a water-moving environment, can effectively prevent seepage and leak plugging, meet the filling needs of karst formation cracks and pores, and improve the mechanical properties and dispersion resistance of grouting materials.
Smart Images

Figure CN119019129A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of geotechnical engineering grouting, and in particular relates to a grouting material for dynamic water filling of a tunnel karst cave and a preparation method thereof. Background Art
[0002] Currently, shield tunnels have been widely used in the development of underground infrastructure. Shield tunnel construction in karst areas is a common challenge, especially under groundwater flow conditions. When constructing tunnels in karst areas, adverse geological hazards such as shield sinking, water and mud inrush, tunnel face instability, ground collapse, and soil liquefaction may occur, so preventive measures must be taken to prevent significant casualties and serious economic losses.
[0003] At present, among a large number of water inrush control technologies, grouting is the most widely used water blocking and reinforcement measure. The grouting material widely used in tunnel cave grouting projects is clay cement solidified slurry, which has the characteristics of low economic cost, strong underwater anti-dispersion ability and low environmental pollution. However, the consolidated body of clay cement solidified slurry still has the problems of insufficient strength and poor toughness. Therefore, in the field of geotechnical engineering, it is urgent to develop a new grouting material with anti-dynamic water dispersion to solve the problem of insufficient strength of clay grouting materials.
[0004] As a green and environmentally friendly mineral fiber, basalt fiber is made from natural basalt ore, and its main components are silicon dioxide, aluminum oxide and iron oxide. It is a typical silicate mineral fiber, which has natural compatibility with cement composite materials, and has good mechanical properties, high temperature resistance and acid and alkali resistance, and can be used for grouting materials.
[0005] However, the basalt commonly used at present is basalt powder or clustered basalt fiber with a smaller particle size. Basalt powder cannot cope with the micro-cracks generated by the stone body, and the tensile strength, anti-scouring performance and water resistance of the grouting material formed are still poor. Especially in the case of groundwater surge in karst formation cracks, pores or large channels, the grouting material is easy to lose and cannot achieve the filling and plugging effect. In addition, directly adding clustered basalt fibers has the disadvantage of poor fiber dispersion. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides a grouting material for dynamic water filling of a tunnel cave and a preparation method thereof.
[0007] In one aspect of the present invention, there is provided a grouting material for dynamic water filling of a tunnel cave, the grouting material comprising:
[0008] 10-15 parts by mass of bentonite;
[0009] 35-45 parts by mass of Portland cement;
[0010] 1-4 parts by mass of modified basalt fiber;
[0011] 0.5-1 parts by mass of lignin water reducer;
[0012] 40-55 parts by mass of water.
[0013] Optionally, the modified basalt fiber has a diameter ranging from 13 to 17 μm and a length ranging from 3 to 12 mm; and / or,
[0014] The modified basalt fiber has a tensile strength of not less than 1050 MPa, an elongation at break of 3-5%, and an elastic modulus of 75 GPa.
[0015] Optionally, the modified basalt fiber is formed by modifying basalt fiber with a silane coupling agent in an anhydrous ethanol solution.
[0016] Optionally, the silane coupling agent is γ-aminopropyltriethoxysilane.
[0017] Optionally, the bentonite is calcium-based bentonite, and the montmorillonite content is greater than 70%.
[0018] Optionally, the calcium-based bentonite has a fineness that satisfies a 200-mesh sieve residue of less than 4%, and a particle size range of 0.1-10 μm.
[0019] Another aspect of the present invention provides a method for preparing the grouting material for dynamic water filling of tunnel caves as described above, the method comprising:
[0020] obtaining modified basalt fiber;
[0021] Stirring the modified basalt fiber, bentonite and water to obtain a first slurry, and subjecting the first slurry to a static treatment;
[0022] Stirring silicate cement, lignin water reducer and water to obtain a second slurry;
[0023] The first slurry after the static treatment is mixed with the second slurry, and stirred into a paste to obtain a grouting material.
[0024] Optionally, the step of obtaining the modified basalt fiber comprises:
[0025] The basalt fiber is placed in a mixed solution of a silane coupling agent and 95v% anhydrous ethanol, stirred and dispersed for 2h under heating conditions, and then washed and dried to obtain the modified basalt fiber.
[0026] Optionally, the modified basalt fiber, bentonite and water are stirred to obtain a first slurry, comprising:
[0027] The bentonite and modified basalt fiber are placed in a mixer with a rotation speed of not less than 125 r / min and dry-mixed for 100s to 130s, and water is added and ultrasonically stirred for 170s to 190s to obtain a first slurry.
[0028] Optionally, the stirring to a paste comprises:
[0029] Stir at 125 r / min for 2 to 4 min, then stir at 65 r / min until it becomes a paste.
[0030] The present invention proposes a grouting material for dynamic water filling of tunnel karst caves and a preparation method thereof, wherein the grouting material comprises: 10-15 parts by mass of bentonite; 35-45 parts by mass of silicate cement; 1-4 parts by mass of modified basalt fiber; 0.5-1 parts by mass of lignin water reducer; and 40-55 parts by mass of water. Based on the synergistic effect of modified basalt fiber and bentonite, the present invention forms a grouting material with advantages such as superior underwater stability, anti-dilution, and high underwater strength, and has good durability in a dynamic water environment, is not easy to lose, and can be used in anti-seepage and plugging grouting construction in dynamic water areas such as karst stratum cracks, pores or large channels where groundwater surges. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a flowchart of a method for preparing grouting materials for dynamic water filling of tunnel caves according to an embodiment of the present invention;
[0032] Figure 2 This is a physical picture of the grouting material slurry of Example 4 of the present invention;
[0033] Figure 3 This is a physical picture of the grouting material slurry of Example 5 of the present invention;
[0034] Figure 4 This is a physical picture of the grouting material slurry of Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.
[0036] In one aspect of the present invention, a grouting material for dynamic water filling of tunnel caves is provided, comprising: 10-15 parts by mass of bentonite; 35-45 parts by mass of silicate cement; 1-4 parts by mass of modified basalt fiber; 0.5-1 parts by mass of lignin water reducer; and 40-55 parts by mass of water.
[0037] In this embodiment, a grouting material with the advantages of excellent underwater stability, anti-dilution, high underwater strength, etc. is formed based on the above components. It has good durability in a dynamic water environment and is not easy to lose. It can be used in the anti-seepage and leakage grouting construction of dynamic water areas such as karst formation cracks, pores or large channels where groundwater suddenly surges.
[0038] Among them, in this embodiment, the use of basalt fiber can inhibit the generation and expansion of microcracks in the stone body, while improving the toughness, compressive strength, tensile strength and water resistance of the stone body; secondly, based on the use of modified basalt fiber, its dispersibility is also effectively improved, and it is not easy to cross and clump in the slurry, so that it is interconnected to form a network structure, thereby improving the anti-scouring performance of the grouting material, and it is not easy to lose in a dynamic water environment.
[0039] Secondly, in this embodiment, the water absorption and expansion properties of bentonite are also utilized to stably control the fluidity and setting time of the grouting material. At the same time, it also works synergistically with the modified basalt fiber to improve the dispersibility of the modified basalt fiber and further enhance the scour resistance of the slurry, thereby making the solidification performance of the slurry stone body more stable and controllable.
[0040] Further, in this embodiment, the modified basalt fiber has a diameter ranging from 13 to 17 μm and a length ranging from 3 to 12 mm (eg, 3 mm, 6 mm, 12 mm in length).
[0041] It should be understood that, considering the pumpability of grouting and the comprehensive performance of grouting materials, it is necessary to control the content and length of modified basalt, etc., and within the above preferred content, preferred diameter and preferred length preferred range, it is most conducive to improving the mechanical properties and anti-scouring properties of grouting materials, etc. When the content is too high or the diameter is too long, the basalt fiber will block the grouting pipe. In addition, the basalt fiber of the above preferred length also has a bridging effect, which enhances the anti-dispersion and mechanical strength of the grouting material through the bridging effect.
[0042] Furthermore, in the present embodiment, the tensile strength of the modified basalt fiber is not less than 1050MPa, the elongation at break is 3-5%, and the elastic modulus is 75GPa. By adopting the modified basalt fiber in the above-mentioned preferred diameter and length range, the modified basalt fiber has the advantages of high tensile strength and high breaking strength. When it is applied to the grouting material, only a small amount (for example, 1-4 mass) of modified basalt fiber is required to effectively improve the toughness of the solidified body of the grouting material, provide load after cracks are generated in the solidified body, and effectively improve the scouring resistance of the slurry under dynamic water conditions.
[0043] Furthermore, in this embodiment, the modified basalt fiber is formed by modifying the basalt fiber with a silane coupling agent in an anhydrous ethanol solution. In other words, the basalt fiber needs to be modified to improve its dispersibility and make the surface of the basalt fiber rougher to improve the bonding with the matrix.
[0044] It should be noted that the silane coupling agent is γ-aminopropyltriethoxysilane (KH570). Based on this modifier, the dispersibility of basalt fiber can be effectively improved. In addition, the modified basalt fiber also has a synergistic effect with bentonite, that is, during the preparation process, the bentonite also has a certain dispersing effect on the basalt fiber to a certain extent. Thus, in this embodiment, only this kind of modifier is used to achieve the modification effect of basalt fiber and effectively improve its dispersibility.
[0045] Furthermore, the bentonite is calcium-based bentonite, and the montmorillonite content is greater than 70%. The fineness of the calcium-based bentonite satisfies that the residue on a 200-mesh sieve is less than 4%, the particle size mainly ranges from 0.1 to 10 μm, and the pulping rate is greater than 14 μm. 3 / t.
[0046] In this embodiment, bentonite slurry is used as the base slurry of the grouting material. The water absorption and expansion properties of bentonite are utilized to stably control the fluidity and setting time of the slurry, while improving the anti-dispersion property of the slurry, so that the curing performance of the slurry stone body is more stable and controllable.
[0047] Furthermore, the water absorption of calcium bentonite is relatively small, with a maximum of no more than 200%, and there is enough free radical water to react with cement, that is, calcium bentonite still has fluidity during the hydration process, and the paste formed by mixing hydrated calcium bentonite with cement has certain fluidity and pourability. In addition, calcium bentonite absorbs water quickly and reaches saturation in less than 2 hours, which can improve the efficiency of on-site slurry preparation.
[0048] In this embodiment, the grouting material includes modified basalt fiber, and the bentonite is calcium bentonite, and the content of the bentonite is only 10-15 parts by mass to ensure the fluidity and coagulation stability of the slurry.
[0049] Furthermore, the cement is ordinary Portland cement having a specific surface area of not less than 358 m 2 / kg. The initial setting time is 172min, the final setting time is 224min, and the compressive strength after 3d and 28d is 5.5MPa and 27.2MPa respectively. When the specific surface area of cement is within the above preferred range, the degree of hydration of cement is high, which can improve the early strength of the grouting material; when the initial setting time and the final setting time are the above preferred time, the controllability of the grouting material can be improved for easy operation and use; and when the compressive strength is the above preferred value, the mechanical strength of the solidified body of the grouting material can be improved.
[0050] Furthermore, in this embodiment, a lignin water reducer is added as an admixture to adjust the processability of the grouting material, making the slurry easy to process, and can also reduce the water consumption of the grouting material, reduce the water-cement ratio, and improve the cohesion of the slurry.
[0051] It should be noted that the increase in cement content can greatly improve the compressive strength of the grouting material, but under dynamic water conditions, the cement slurry has a weak dilution resistance and is easily eroded by water. Therefore, in this embodiment, by increasing the content of bentonite, its water absorption can be used to improve the dilution resistance of the grouting material, but on the other hand, when the content of bentonite is too high, it is not conducive to the growth of mechanical strength. Based on this, modified basalt fiber is also introduced as a reinforcing material. The randomly dispersed modified basalt fiber can improve the water erosion resistance of the grouting material through a mesh structure. In this way, after the grouting material is cured, the fiber can also improve the mechanical strength of the grouting material through a bridging effect.
[0052] The present invention forms silicate cement as the main component through the synergistic effect of calcium-based bentonite and modified basalt fiber. Only a small amount of modified basalt and bentonite is needed to improve the mechanical properties of the grouting material and meet the requirements of filling and plugging under dynamic water conditions.
[0053] like Figure 1 As shown, another aspect of the present invention provides a method S100 for preparing the grouting material for dynamic water filling of tunnel caves as described above, comprising steps S110 to S140:
[0054] S110. Obtain modified basalt fiber.
[0055] Specifically, the basalt fiber is placed in a mixed solution of a silane coupling agent and 95v% anhydrous ethanol (for example, γ-aminopropyltriethoxysilane, KH-570), and is placed in a mixer with a rotation speed of not less than 125r / min for stirring and dispersion. The water bath temperature is 80°C. After stirring for 2h, the basalt fiber is taken out and immersed in water for cleaning, and then the surface moisture is dried to obtain dispersed modified basalt fiber.
[0056] In this embodiment, the basalt fiber has the best modification effect when treated in an anhydrous ethanol solution under the condition of 80° C. water bath heating, and has good dispersibility. The surface of the basalt fiber is rougher and has the best adhesion to the matrix.
[0057] S120, stirring the modified basalt fiber, bentonite and water to obtain a first slurry, and allowing the first slurry to stand.
[0058] Specifically, 1-4 parts by mass of modified basalt fiber and 10-15 parts by mass of bentonite are placed in a mixer with a rotation speed of not less than 125 r / min and dry-mixed for 100s to 130s (e.g., 120s). Then, 50% of the water in the above-mentioned parts by mass is added and ultrasonically stirred for 170s to 190s (e.g., 180s) to obtain a first slurry, and the first slurry is allowed to stand for 12 hours to hydrate the bentonite.
[0059] In this embodiment, the dispersion of basalt fibers is improved by dry mixing and ultrasonic stirring, so that they are interconnected to form a network structure, thereby improving the anti-scouring ability of the slurry and preventing it from being lost in water. In addition, based on the synergistic effect of calcium-based bentonite and modified basalt fibers, only a small amount of both is required to improve the slurry retention rate and mechanical properties.
[0060] S130, stirring silicate cement, lignin water reducer and water to obtain a second slurry.
[0061] Specifically, 35-45 parts by mass of Portland cement, 0.5-1 parts by mass of lignin water reducer and the balance of water are stirred for 60 seconds to prepare the second slurry.
[0062] S140, mixing the first slurry after the static treatment with the second slurry, stirring until it is in a paste state, and obtaining a grouting material.
[0063] Specifically, the first slurry after the static treatment was mixed with the second slurry, stirred at a high speed of 125 r / min for 3 minutes, and then slowly stirred at a speed of 65 r / min until the mixed slurry was in a paste state.
[0064] In this embodiment, the two slurries can be better mixed by staged stirring, that is, firstly high-speed stirring is used to quickly mix the first slurry and the second slurry, and then slow stirring is used to fully mix the modified basalt fiber in the slurry, thereby improving the tensile strength and water erosion resistance.
[0065] The preparation method of the invention is simple and easy to operate. The prepared grouting material is non-toxic and harmless and can be used to block sudden surges of groundwater in cracks, pores or large channels in karst strata, and has a strong value for promotion and use.
[0066] It should be noted that, in order to illustrate the performance of the grouting material prepared by the present invention, its fluidity, slurry setting time, mechanical properties, and slurry retention rate were tested and analyzed, and the testing process was carried out in accordance with various standards.
[0067] The fluidity test is carried out in accordance with the relevant test methods in GB / T 2419-2005 "Method for Determination of Fluidity of Cement Mortar"; the slurry setting time is measured in accordance with the relevant test methods in GB / T 1346 "Test Method for Water Consumption, Setting Time and Stability of Cement Standard Consistency". The compressive strength and splitting tensile strength tests are carried out in accordance with GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".
[0068] Among them, the test parameter slurry retention rate refers to the ratio of the mass of slurry retained in the water tank under dynamic water conditions to the original mass of slurry, which is used to evaluate the anti-dispersion of slurry under dynamic water conditions. Fluidity refers to injecting the prepared slurry into a truncated cone circular mold, scraping the surface with a scraper, lifting the truncated cone circular mold in the vertical direction, and immediately starting the jumping table to complete a cycle of 25 jumps within 25 seconds at a frequency of once per second. Use a 30mm range caliper to measure the expansion diameter of the bottom surface of the slurry in two directions perpendicular to each other, and calculate the average value, which is the fluidity of the slurry.
[0069] The grouting material and its performance for dynamic water filling of tunnel caves will be further described below in conjunction with several specific embodiments:
[0070] Example 1
[0071] The grouting material of this example includes the following components: 10 parts of calcium-based bentonite, 45 parts of ordinary Portland cement, 50 parts of water, 0.5 parts of lignin water reducer, and 1 part of modified basalt fiber (3 mm in length). For its preparation process, please refer to the previous record.
[0072] According to Table 1, the fluidity of the grouting material prepared in this embodiment is 205 mm, the initial setting time is 60 min, the final setting time is 225 min, the slurry retention rate is 95.4%, the compressive strength after 7 days is 1.16 MPa, the compressive strength after 28 days is 3.25 MPa, and the tensile strength after 28 days is 0.24 MPa.
[0073] Example 2
[0074] The grouting material of this example includes the following components: 15 parts of calcium-based bentonite, 45 parts of ordinary Portland cement, 50 parts of water, 0.5 parts of lignin water reducer, and 1 part of modified basalt fiber (3 mm in length). For the preparation process, please refer to the previous description.
[0075] According to Table 1, the fluidity of the grouting material prepared in this embodiment is 197 mm, the initial setting time is 45 min, the final setting time is 200 min, the slurry retention rate is 94.3%, the compressive strength after 7 days is 1.14 MPa, the compressive strength after 28 days is 3.42 MPa, and the tensile strength after 28 days is 0.27 MPa.
[0076] Compared with Example 1, it can be seen that the content of bentonite increases, and the fluidity, setting time and slurry retention rate of the grouting material decrease.
[0077] Example 3
[0078] The grouting material of this example includes the following components: 15 parts of calcium-based bentonite, 45 parts of ordinary Portland cement, 50 parts of water, 0.5 parts of lignin water reducer, and 2 parts of modified basalt fiber (3 mm in length). For its preparation process, please refer to the previous record.
[0079] According to Table 1, the fluidity of the grouting material prepared in this embodiment is 189 mm, the initial setting time is 55 min, the final setting time is 205 min, the slurry retention rate is 95.7%, the compressive strength after 7 days is 1.21 MPa, the compressive strength after 28 days is 3.61 MPa, and the tensile strength after 28 days is 0.31 MPa.
[0080] Compared with Example 2, it can be seen that as the content of modified basalt fiber increases, the setting time, slurry retention rate, compressive strength and tensile strength of the slurry all increase, which shows that the modified basalt fiber has a great influence on the controllability, scour resistance and mechanical properties of the slurry.
[0081] Example 4
[0082] The grouting material of this example includes the following components: 15 parts of calcium-based bentonite, 45 parts of ordinary Portland cement, 50 parts of water, 0.5 parts of lignin water reducer, and 3 parts of modified basalt fiber (3 mm in length). For the preparation process, please refer to the previous record.
[0083] According to Table 1, the fluidity of the grouting material prepared in this embodiment is 185 mm, the initial setting time is 50 min, the final setting time is 210 min, the slurry retention rate is 95.8%, the compressive strength after 7 days is 1.18 MPa, the compressive strength after 28 days is 3.53 MPa, and the tensile strength after 28 days is 0.33 MPa.
[0084] Compared with Example 3, it can be seen that as the content of modified basalt fiber increases, the final setting time, slurry retention rate, and tensile strength of the slurry all increase, and the compressive strength decreases, which indicates that increasing the content of modified basalt fiber will further improve the scour resistance of the slurry.
[0085] Furthermore, this embodiment also provides a physical picture of the grouting material used in the on-site grouting application, such as Figure 2 As shown in Figure 2, the fluidity and uniformity of the slurry during the grouting process are similar to Figure 4 This shows that the modified basalt fiber has little effect on the fluidity of the slurry. Compared with comparative example 1, its fluidity is reduced, but it still meets the requirements of on-site grouting (fluidity not less than 180mm). The grouting volume is 0.5m every 30 minutes. 3 , the grouting pressure is 0.3MPa. Secondly, the 28d drilling coring rate is greater than 80%, the consolidation strength is not less than 0.25MPa, and the water permeability is not greater than 10Lu, which shows that the modified basalt fiber can effectively improve the consolidation strength of the grouting material and reduce the water permeability, achieve effective plugging in a dynamic water environment, and meet the on-site grouting conditions.
[0086] Example 5
[0087] The grouting material of this example includes the following components: 15 parts of calcium-based bentonite, 45 parts of ordinary Portland cement, 50 parts of water, 0.5 parts of lignin water reducer, and 2 parts of modified basalt fiber (length 12 mm). Please refer to the previous record for its preparation process.
[0088] According to Table 1, the fluidity of the grouting material prepared in this embodiment is 182 mm, the initial setting time is 55 min, the final setting time is 215 min, the slurry retention rate is 92.3%, the compressive strength after 7 days is 1.12 MPa, the compressive strength after 28 days is 3.21 MPa, and the tensile strength after 28 days is 0.31 MPa.
[0089] Compared with Example 3, it can be seen that as the length of the modified basalt fiber increases, the slurry retention rate, compressive strength and tensile strength of the slurry decrease. This shows that when the length of the modified basalt fiber is too long, the scour resistance and mechanical properties of the slurry will decrease.
[0090] Furthermore, the prepared grouting material is also used in on-site grouting applications, such as Figure 3 As shown, the fluidity of the slurry is average, compared with Figure 4 The slurry in the grout has poor uniformity. When the fiber length is long, it has a greater impact on the fluidity of the slurry, and its fluidity decreases, but it can still meet the requirements of on-site grouting (fluidity is not less than 180mm).
[0091] Comparative Example 1
[0092] The grouting material of this example includes the following components: 15 parts of calcium-based bentonite, 45 parts of ordinary Portland cement, 50 parts of water, and 0.5 parts of lignin water reducer. Please refer to the above description for its preparation process.
[0093] According to Table 1, the fluidity of the grouting material prepared in this comparative example is 213 mm, the initial setting time is 45 min, the final setting time is 195 min, the slurry retention rate is 82.3%, the compressive strength after 7 days is 1.07 MPa, the compressive strength after 28 days is 2.96 MPa, and the tensile strength after 28 days is 0.21 MPa.
[0094] Furthermore, the prepared grouting material is also used in on-site grouting applications, such as Figure 4 As shown, it can be seen that the slurry has good uniformity and high fluidity. It can be seen from Table 1 that the fluidity of the grouting material is greater than 200 mm, which meets the requirements of on-site grouting (fluidity is not less than 180 mm). This shows that in the grouting material without the addition of modified basalt fiber, it has good fluidity and can be fully diffused. However, the setting time, slurry retention rate, compressive strength and tensile strength of the grouting material are all poor, and cannot meet the filling requirements under dynamic water conditions.
[0095] Table 1 Results of relevant test parameters of grouting materials of Examples 1-5 and Comparative Example 1
[0096]
[0097] In summary, combined with Comparative Example 1-Examples 1-5, it can be seen that, on the one hand, the fluidity of the grouting material with the addition of modified basalt fiber has decreased, but it still meets the requirements of on-site grouting (fluidity not less than 180 mm). For example, the fluidity of the slurry in Example 1 is also above 200 mm. In addition, according to Figure 2 and Figure 4It can be seen that although the fluidity of the slurry in Example 4 has decreased, its uniformity and fluidity are similar to those of Comparative Example 1, and its slurry meets the requirements of sufficient diffusion and can be filled in every part of the cave; in addition, even if the fluidity of the slurry in Example 5 is relatively poor, it still meets the requirements of on-site grouting, and under this premise, it also has higher compressive energy reading, tensile strength, longer setting time, etc. In summary, the grouting material added with modified basalt fiber has a better filling effect. On the other hand, the setting time and slurry retention rate of the grouting material with the addition of modified basalt fiber are improved, which shows that the grouting material with the addition of modified basalt fiber has high controllability and greatly improves the mechanical properties and slurry retention rate while meeting the grouting requirements, especially in a dynamic water tank environment with a water flow rate of 1.2m / s. The slurry retention rate of the grouting material after flushing is significantly improved, up to 95.8%, which shows that the grouting material provided by the present invention has very good anti-scouring performance under dynamic water conditions, and can effectively prevent the slurry from being washed away by the water flow after injection and unable to stay in the cave to coagulate, that is, the grouting material with the addition of modified basalt fiber has an ideal filling effect, can meet the grouting needs of special working conditions, and achieve efficient grouting and water blocking. On the other hand, the grouting material with modified basalt fiber has good compressive strength and tensile strength. The 28-day compressive strength and tensile strength of the slurry stone body are enhanced by 7.09-21.96%, and the splitting tensile strength is 14.28-57.14%. The mechanical properties are superior and reliable.
[0098] The present invention provides a grouting material for dynamic water filling of tunnel caves and a preparation method thereof, which has the following beneficial effects:
[0099] First, the present invention adds an appropriate amount of modified basalt fiber and calcium-based bentonite to the traditional cement curing slurry, thereby forming a modified basalt fiber bentonite cement curing slurry with excellent underwater stability, anti-dilution, high underwater strength, and good durability in a dynamic water environment, which can be widely used in anti-seepage and leak-proof grouting construction in dynamic water areas;
[0100] Second, the present invention improves the anti-dispersion performance of the slurry by adding modified basalt fibers. At the same time, during the hardening stage, the fibers inhibit the generation and expansion of microcracks in the stone body, thereby improving the toughness, compressive strength, tensile strength and water resistance of the stone body.
[0101] Third, the present invention uses calcium-based bentonite slurry as the base slurry of the grouting material, and utilizes the water absorption and expansion of calcium-based bentonite to stably control the fluidity and setting time of the slurry, while improving the anti-dispersion property of the slurry, so that the curing performance of the slurry stone body is more stable and controllable;
[0102] Fourthly, the preparation method of the present invention is simple and easy to operate. The prepared grouting material is non-toxic and harmless and can be used to block the sudden surge of groundwater in cracks, pores or large channels in karst strata, and has a strong value for promotion and use;
[0103] Fifth, based on the fact that the modified basalt fiber has high toughness and strength and is not easy to cross-clump during slurry stirring, the present invention improves the dispersibility of the basalt fiber by dry mixing and ultrasonic stirring, so that the basalt fiber is interconnected to form a network structure, thereby improving the slurry's anti-scouring ability and is not easy to lose in water.
[0104] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A grouting material for dynamic water filling of tunnel caves, characterized in that: The grouting material comprises: 10-15 parts by mass of bentonite; 35-45 parts by mass of Portland cement; 1-4 parts by mass of modified basalt fiber; 0.5-1 parts by mass of lignin water reducer; 40-55 parts by mass of water.
2. The grouting material according to claim 1, characterized in that: The modified basalt fiber has a diameter range of 13-17 μm and a length range of 3-12 mm; and / or, The modified basalt fiber has a tensile strength of not less than 1050 MPa, an elongation at break of 3-5%, and an elastic modulus of 75 GPa.
3. The grouting material according to claim 2, characterized in that: The modified basalt fiber is formed by modifying the basalt fiber with a silane coupling agent in an anhydrous ethanol solution.
4. The grouting material according to claim 3, characterized in that: The silane coupling agent is γ-aminopropyltriethoxysilane.
5. The grouting material according to claim 1, characterized in that: The bentonite is calcium-based bentonite, and the montmorillonite content is greater than 70%.
6. The grouting material according to claim 5, characterized in that: The fineness of the calcium-based bentonite satisfies that the residue on a 200-mesh sieve is less than 4%, and the particle size ranges from 0.1 to 10 μm.
7. A method for preparing a grouting material for dynamic water filling of a tunnel cave as claimed in any one of claims 1 to 6, characterized in that: The method comprises: obtaining modified basalt fiber; Stirring the modified basalt fiber, bentonite and water to obtain a first slurry, and subjecting the first slurry to a static treatment; Stirring silicate cement, lignin water reducer and water to obtain a second slurry; The first slurry after the static treatment is mixed with the second slurry, and stirred into a paste to obtain a grouting material.
8. The method according to claim 7, characterized in that The method of obtaining the modified basalt fiber comprises: The basalt fiber is placed in a mixed solution of a silane coupling agent and 95v% anhydrous ethanol, stirred and dispersed for 2h under heating conditions, and then washed and dried to obtain the modified basalt fiber.
9. The method according to claim 7, characterized in that: The modified basalt fiber, bentonite and water are stirred to obtain a first slurry, comprising: The bentonite and modified basalt fiber are placed in a mixer with a rotation speed of not less than 125 r / min and dry-mixed for 100s to 130s, and water is added and ultrasonically stirred for 170s to 190s to obtain a first slurry.
10. The method according to claim 7, characterized in that The stirring to a paste state comprises: Stir at 125 r / min for 2 to 4 min, then stir at 65 r / min until it becomes a paste.