Superparaelectric-phase perovskite ceramic material with A and B site components and preparation method and application of superparaelectric-phase perovskite ceramic material

CN119019166AActive Publication Date: 2024-11-26GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411113857.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

然而,畴翻转能垒的损失限制了储能性能的进一步提高

Benefits of technology

[0043] 1. The present invention adopts a traditional solid-phase reaction method to prepare perovskite ceramic materials, using three equivalent metals ACO in equimolar proportions. 3 to replace the corresponding A position, and combine the two BOs in a molar ratio of (9-7):(1-3) 2 Replaced at the B position, the control of multiple components at the A and B positions is achieved. By adjusting the temperature to be close to or lower than the ambient temperature, a superparaelectric phase was successfully constructed for better application in the field of energy storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019166A_ABST
    Figure CN119019166A_ABST
Patent Text Reader

Abstract

The invention discloses a superparaelectric-phase perovskite type ceramic material with A and B site components and a preparation method and application thereof.The chemical formula of the superparaelectric-phase perovskite type ceramic material with the A and B site components is (Ba1 / 3Sr1 / 3Ca1 / 3) (SnxTi1-x) O3, and x is larger than or equal to 0.1 and smaller than or equal to 0.3. The superparaelectric-phase perovskite type ceramic material with the A and B site components can be used for preparing relaxor ferroelectric materials, has good energy storage performance and can be used for preparing the relaxor ferroelectric materials. And the method meets the current lead-free requirement, is environment-friendly, is simple in process flow and stable in performance, and is beneficial to large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of dielectric energy storage of perovskite oxide materials, and in particular relates to a superparaelectric perovskite ceramic material with A and B components, and a preparation method and application thereof. Background Art

[0002] Dielectric capacitors have a very high power density (10 8 W / kg), excellent charge and discharge speed (μs to ns), ultra-long service life, high thermal stability (-50℃~250℃) and mechanical strength, etc., have broad application prospects in power electronics, new energy vehicles and aerospace. However, compared with electrochemical energy storage technology, dielectric capacitors usually exhibit relatively low energy density, which limits their application in integration and miniaturization. In addition, the effective energy storage density (W rec ) and high energy storage efficiency (η) as effective parameters for evaluating energy storage performance, which largely depends on the large polarization difference ΔP (= maximum polarization P max -Remanent polarization P r ) and high breakdown strength (E b ). Therefore, the development and application of efficient energy storage materials have attracted more and more attention.

[0003] At the same time, as one of the key research structures of energy storage materials, perovskite oxide (ABO3) has excellent adjustability and large structural tolerance, which provides rich possibilities for regulating the energy storage performance of perovskite structure ceramic materials. This makes it possible to induce relaxation behavior through composition design, thereby obtaining excellent energy storage performance.

[0004] As a potential candidate for energy storage dielectric material system, relaxor ferroelectrics have unique nanodomain structure and diffuse phase transition characteristics. Typical relaxor ferroelectrics have three key characteristic temperatures: Burns temperature (T B ), the temperature corresponding to the maximum dielectric constant (T m ) and freezing temperature (T f ), each of which corresponds to different ferroelectric properties and microstructures. At present, the research on relaxor ferroelectrics mainly focuses on T f ~T m However, the loss of domain reversal energy barrier limits the further improvement of energy storage performance. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a superparaelectric perovskite ceramic material with A and B components and a preparation method and application thereof. The chemical formula of the superparaelectric perovskite ceramic material with A and B components provided by the present invention is

[0006] —(Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn x Ti 1-x )O3, wherein 0.1≤x≤0.3, and its perovskite structure belongs to the cubic system, and the space group is Pm3m. The A and B position component superparaelectric phase perovskite type ceramic materials of the present invention can be used to prepare relaxor ferroelectric materials, have good energy storage performance, and can be used as energy storage ceramic materials. The energy storage ceramic material of the present invention meets the current lead-free requirements, is environmentally friendly, has a simple process flow and stable performance, and is conducive to large-scale production.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] One of the technical solutions of the present invention:

[0009] A superparaelectric perovskite ceramic material with A and B components, the general structural formula is ABO3, wherein the A component is composed of three elements, Ba, Sr and Ca, and the B component is composed of two elements, Ti and Sn;

[0010] The three elements at the A position occupy the A position in an equimolar ratio, and the molar ratio of the two elements Ti and Sn at the B position is (1 to 3) (7 to 9).

[0011] Preferably, in the superparaelectric perovskite ceramic material of the A and B components, the two metal elements at the B position are Sn 4+ :Ti 4+ =1∶9, Sn 4+ :Ti 4+ =1∶4, Sn 4+ :Ti 4+ =3:7 three molar ratios occupy the B position.

[0012] Preferably, the chemical formula of the superparaelectric perovskite ceramic material of the A and B components is (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn x Ti 1-x )O3, wherein 0.1≤x≤0.3, more preferably x=0.1, 0.2 or 0.3;

[0013] The perovskite structure of the superparaelectric perovskite ceramic material of the A and B components belongs to the cubic crystal system, and the space group is .

[0014] The second technical solution of the present invention:

[0015] The present invention also provides a method for preparing the superparaelectric perovskite ceramic material of the A and B components, comprising the following steps:

[0016] (1) According to the stoichiometric ratio of the superparaelectric perovskite ceramic materials of the A and B components, the raw materials BaCO3, SrCO3, CaCO3, TiO2 and SnO2 are weighed and added into a ball mill, the grinding balls are zirconium oxide balls, anhydrous ethanol is added as the ball milling medium, and the ball mill is placed in a planetary ball mill, and dried after ball milling;

[0017] (2) pre-calcining the dried material in step (1) at 1000° C. to 1100° C. for 4 to 6 hours in an air atmosphere to obtain a pre-calcined powder;

[0018] (3) adding the pre-sintered powder into a ball mill, using zirconium oxide balls as the grinding balls, adding anhydrous ethanol as the ball milling medium, placing the ball mill into a planetary ball mill, and drying after ball milling;

[0019] (4) adding a polyvinyl alcohol solution to the pre-calcined powder dried in step (3) to granulate the granules, sieving the granules, dry-pressing them into cylindrical green bodies, and then debinding the cylindrical green bodies;

[0020] (5) The cylindrical green body after debinding is sintered at a temperature of 1400° C. to 1500° C. for 4 to 6 hours in an air atmosphere to obtain the superparaelectric perovskite ceramic material of the A and B components.

[0021] Preferably, in the preparation method of the superparaelectric phase perovskite ceramic material of the A and B components, in step (1), the mass ratio of the mixed material, the grinding ball and the ball milling medium is 1:2:2, wherein the mass of the mixed material refers to the total mass of the raw materials BaCO3, SrCO3, CaCO3, TiO2 and SnO2. Among them, zirconium oxide as a grinding ball material can reduce pollution and improve grinding efficiency, anhydrous ethanol as a ball milling medium can ensure chemical stability, and the appropriate mass ratio of the mixed material, the grinding ball and the ball milling medium ensures sufficient grinding and uniform mixing, thereby forming a uniform ceramic structure in the subsequent sintering process. The ball milling is performed at a speed of 300 to 360 r / min for 6 hours, and the ball milled material is dried at 120°C for 2 to 3 hours. Among them, a reasonable ball milling time ensures sufficient grinding and mixing of the material, and the appropriate speed control does not cause overheating, while avoiding excessive grinding to affect the particle size of the material, thereby affecting the energy storage ceramic performance.

[0022] Preferably, the purity of the raw materials BaCO3, SrCO3, CaCO3, TiO2 and SnO2 is above 99.9%, and the above raw materials are dried at 100-120°C for 12-24 hours before mixing.

[0023] Preferably, in the preparation method of the superparaelectric perovskite ceramic material of the A and B components, in step (2), the heating rate from room temperature to 1000°C to 1100°C is 3 to 5°C / min, preferably to 1100°C. Among them, the reasonable pre-firing temperature and time during pre-firing are helpful to remove organic matter, moisture and volatile substances in the material, which may generate gas during high-temperature sintering, resulting in holes or cracks inside the ceramic, affecting the mechanical strength and electrical properties of the material. At the same time, a suitable heating rate can avoid thermal stress and cracks, thereby facilitating the acquisition of a uniform, crack-free pre-firing sample.

[0024] Preferably, in the preparation method of the superparaelectric perovskite ceramic material of the A and B components, in step (3), the ball milling is performed at a rotation speed of 300 to 360 r / min for 6 hours, and the ball-milled material is dried at 120° C. for 2 to 3 hours.

[0025] Preferably, in the method for preparing the superparaelectric perovskite ceramic material of the A and B components, in step (4), the mass concentration of the polyvinyl alcohol solution is 5%;

[0026] The sieving is through a 60-120 mesh sieve;

[0027] The uniaxial pressure during dry pressing is 5-8 MPa, and the holding time is 1-2 minutes; the mold used for dry pressing is a cylindrical mold with a diameter of 8-10 mm;

[0028] The debinding process is performed at 550°C for 6 to 8 hours with a heating rate of 1.5 to 2°C / min. During the debinding process, a too fast heating rate may lead to stress concentration inside the green body, resulting in cracks or deformation, and reduce the electrical properties of the energy storage ceramic; while a too slow heating rate may lead to uneven material structure and excessive moisture absorption during the process, increasing the difficulty of the subsequent sintering process.

[0029] Preferably, in the preparation method of the superparaelectric perovskite ceramic material of the A and B components, in step (5), the rate at which the cylindrical green body after debinding is heated to 1400°C to 1500°C in an air atmosphere is 3 to 5°C / min. Among them, the calcination temperature and time will affect the grain size, phase purity and uniformity of the material, and affect the electrical properties, thermal stability and mechanical strength of the material. The appropriate heating rate promotes the uniform growth of grains and the formation of the microstructure of the material, and improves the density of the effective material, thereby obtaining a higher breakdown field strength.

[0030] The superparaelectric state occurs at T B >T>T m Temperature range, by adjusting the temperature to be close to or lower than the ambient temperature (T amb), which can significantly improve the energy storage performance and dielectric temperature stability. <T B The small-sized domains and short-range disordered polar nanodomains (PNRs) in relaxor ferroelectrics enhance the local structural disorder. In superparaelectric relaxor ferroelectrics, lower hysteresis losses help maintain a high polarization state, while the reduction in hysteresis losses and high dynamic PNRs together promote the formation of an elongated PE curve, which is crucial for improving energy storage performance. Based on this, the present invention constructs a superparaelectric phase through carefully designed components, providing a new idea for improving the performance of energy storage ceramics. The synergistic effect of multiple elements leads to chemical and structural disorder, thereby reducing the size of the nanodomains, which is essential for enhancing the breakdown field strength (E b ) and improve temperature stability plays a vital role. Therefore, the present invention constructs a superparaelectric phase through component design, which helps to improve energy storage density and efficiency, thereby better meeting the needs of practical applications.

[0031] The third technical solution of the present invention:

[0032] The present invention also provides a relaxor ferroelectric material based on superparaelectric phase perovskite type ceramic materials of A and B components, wherein the superparaelectric phase perovskite type ceramic materials of A and B components are the above-mentioned superparaelectric phase perovskite type ceramic materials of A and B components.

[0033] The relaxor ferroelectric material based on the superparaelectric phase perovskite-type ceramic material of the A and B components of the present invention has high energy storage density and high energy storage efficiency, and its energy storage performance is greatly improved compared with existing energy storage materials.

[0034] The fourth technical solution of the present invention:

[0035] The present invention also provides a method for preparing the relaxor ferroelectric material based on the superparaelectric phase perovskite type ceramic material of the A and B components, wherein silver electrodes are plated on the upper and lower surfaces of the superparaelectric phase perovskite type ceramic material of the A and B components, and the relaxor ferroelectric material based on the superparaelectric phase perovskite type ceramic material of the A and B components is obtained after calcination and cooling.

[0036] Preferably, in the preparation method of the relaxor ferroelectric material based on the superparaelectric perovskite ceramic material of the A and B components, the thickness of the superparaelectric perovskite ceramic material of the A and B components is 0.10-0.15 mm, and the surface of the superparaelectric perovskite ceramic material of the A and B components is ground smooth before the silver electrode is plated;

[0037] The calcination temperature is 650° C. and the heat preservation time is 30 minutes.

[0038] The fifth technical solution of the present invention:

[0039] The present invention also provides the application of the superparaelectric phase perovskite ceramic material of the A and B components or the relaxor ferroelectric material based on the superparaelectric phase perovskite ceramic material of the A and B components in the field of dielectric energy storage, which is particularly suitable for application scenarios requiring fast charging and discharging and high energy density.

[0040] The chemical reaction involved in the present invention is as follows:

[0041] 3ACO3+xB′O2+(1-x)B″O2→(A′A″A″′)(xB′)[(1-x)B″]O3+3CO2+O2

[0042] Compared with the prior art, the present invention has the following advantages and technical effects:

[0043] 1. The present invention adopts the traditional solid phase reaction method to prepare the perovskite ceramic material, uses three equivalent metals ACO3 to replace the corresponding A position in an equimolar ratio, and replaces two BO2 at the B position in a molar ratio of (9-7): (1-3), thereby realizing the regulation of multiple components at the A and B positions. By adjusting the temperature to be close to or lower than the ambient temperature, the superparaelectric phase is successfully constructed for better application in the field of energy storage.

[0044] 2. The component design of the present invention works synergistically with the superparaelectric relaxor ferroelectric, resulting in the formation of small-sized domains and short-range disordered polar nano-microregions (PNRs) in the material, thereby enhancing the disorder of the local structure. The lower hysteresis loss maintains the high polarizability of the material. At the same time, the reduction of hysteresis loss and high dynamic PNRs also promote the formation of a slender PE curve. These factors have a great impact on improving the breakdown field strength (E b ) and temperature stability play a vital role.

[0045] 3. The superparaelectric phase energy storage ceramics of the present invention show significant performance advantages over existing high-entropy energy storage ceramics. The energy storage mechanism of superparaelectric phase energy storage ceramic materials is based on the polarization principle of dielectric materials. It efficiently stores energy by forming a double electric layer on the electrode surface, which is in sharp contrast to the complex solid solution structure composed of multiple elements and the high entropy effect produced by high-entropy energy storage ceramics. The material composition of superparaelectric energy storage ceramics is simple, and the preparation process is mature and standardized, which not only ensures its high dielectric properties and low dielectric loss, but also significantly reduces the production cost. Relatively speaking, the preparation process of high-entropy energy storage ceramics is more complicated, involving precise control of multiple elements, which not only increases the cost but also makes it difficult to ensure the purity of the sample. In terms of performance, superparaelectric energy storage ceramics excel in energy storage density, charge and discharge rate, and temperature stability, and are particularly suitable for application scenarios that require fast charging and discharging and high energy density. Moreover, in terms of energy storage efficiency and response speed, superparaelectric energy storage ceramics are significantly superior to high-entropy energy storage ceramics.

[0046] 4. The superparaelectric perovskite ceramic material prepared by the present invention can be used as an energy storage material, meets the current lead-free requirements, is environmentally friendly, has a simple process flow, and has stable performance. Compared with the original material (pure BaTiO3 material without superparaelectric design of A and B components), its comprehensive energy storage performance has been greatly improved, which is conducive to large-scale production and can be widely used in pulse power electronic systems such as radar and communication. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0048] Figure 1 (Ba prepared in Example 1 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )XRD spectrum of O3 oxide ceramic material.

[0049] Figure 2 (Ba prepared in Example 1 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )SEM morphology results of O3 oxide ceramic materials.

[0050] Figure 3 (Ba prepared in Example 1 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )Hysteresis loop (PE curve) of O3 relaxor ferroelectric ceramic material at 10 Hz frequency.

[0051] Figure 4 (Ba prepared in Example 2 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )XRD spectrum of O3 oxide ceramic material.

[0052] Figure 5 (Ba prepared in Example 2 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )PE curve of O3 relaxor ferroelectric ceramic material at 10Hz frequency.

[0053] Figure 6 (Ba prepared in Example 3 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )XRD spectrum of O3 oxide ceramic material.

[0054] Figure 7 (Ba prepared in Example 3 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )PE curve of O3 relaxor ferroelectric ceramic material at 10Hz frequency.

[0055] Figure 8 (Ba prepared in Comparative Example 1 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )XRD spectrum of O3 oxide material.

[0056] Fig. 9 For the comparative example 2 prepared (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Zr 0.2 Ti 0.8 )XRD spectrum of O3 oxide material.

[0057] Fig.10 For the comparative example 3 prepared (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.6 Ti 0.4 )XRD spectrum of O3 oxide material. DETAILED DESCRIPTION

[0058] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0059] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0060] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0061] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0062] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0063] Unless otherwise specified, the room temperature in the present invention is 25±2°C.

[0064] All raw materials used in the embodiments of the present invention are commercially available.

[0065] In the embodiments of the present invention, the purity of the raw materials BaCO3, SrCO3, CaCO3, TiO2 and SnO2 is above 99.9%, and the above raw materials are dried at 100-120°C for 12-24 hours before mixing.

[0066] The technical solution of the present invention is further illustrated by the following embodiments.

[0067] Example 1

[0068] A, B component superparaelectric phase perovskite ceramic materials (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 ) Preparation of O3:

[0069] (1) BaCO3, SrCO3, CaCO3, TiO2 and SnO2 raw materials with a purity of more than 99.9% are dried at 110°C for 12 hours before mixing, and are accurately weighed according to the stoichiometric ratio and then mixed (accurate to 0.0001g) to obtain a mixed material, wherein the molar ratio of the metal elements of BaCO3, SrCO3 and CaCO3 is 1:1:1, and the molar ratio of the metal elements of SnO2 and TiO2 is 1:9; the mixed material is added to a ball mill and wet-milled, the grinding balls are zirconium oxide balls, anhydrous ethanol is added as a ball milling medium, the mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2, and the mixed material is fully ball milled at a speed of 320r / min for 6 hours, and the ball-milled material is placed in a 120°C oven for drying for 3 hours;

[0070] (2) pre-calcining the dried material in step (1) at a temperature of 5° C. / min from room temperature to 1050° C. in an air atmosphere for 5 hours to obtain a pre-calcined powder;

[0071] (3) adding the calcined powder obtained in step (2) into a ball mill and performing wet ball milling. The grinding balls are zirconium oxide balls and anhydrous ethanol is added as the ball milling medium. The mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2. The mixed material is fully ball milled at a speed of 320 r / min for 6 hours. The ball milled material is placed in a 120° C. oven and dried for 3 hours;

[0072] (4) adding a polyvinyl alcohol solution having a binder mass concentration of 5% to the pre-burned powder dried in step (3) and granulating the pre-burned powder, wherein the amount of polyvinyl alcohol added is 3% of the total mass of the pre-burned powder, passing through an 80-mesh sieve, and dry-pressing the pre-burned powder into a cylindrical green body with a diameter of 8 mm using a powder tablet press at a pressure of 6 MPa. The pressure holding time is 1 minute, and then the cylindrical green body is debinded at 550° C. for 7 hours at a heating rate of 2° C. / min;

[0073] (5) The cylindrical green body after debinding was heated to 1400°C at 4°C / min in air atmosphere and sintered at this temperature for 5 hours to obtain (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )O3 oxide ceramic material.

[0074] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 ) XRD spectrum of O3 oxide ceramic material is shown in Figure 1 , showing that it has been synthesized (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn0.1 Ti 0.9 )O3 phase.

[0075] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 ) The SEM morphology of O3 oxide ceramic materials is shown in Figure 2 , it can be seen that the ceramic has a good crystallization condition.

[0076] The (Ba prepared in this embodiment 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )O3 oxide ceramic material preparation (Ba 1 / 3Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )O3 relaxor ferroelectric ceramic material, the specific method is:

[0077] will (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 The upper and lower surfaces of the O3 oxide ceramic material were ground smooth to a thickness of 0.10 mm, and then silver-plated electrodes were sintered at 650°C for 30 minutes and cooled to obtain (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )O3 relaxor ferroelectric ceramic material.

[0078] Figure 3 The (Ba prepared in this example 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )O3 relaxor ferroelectric ceramic material hysteresis loop (PE curve) at 10Hz frequency, and its available energy storage density (W) under 540kV / cm electric field is calculated. rec ) reaches 5.05J / cm 3 , the energy storage efficiency (η) reaches 82.56%.

[0079] Example 2

[0080] A, B component superparaelectric phase perovskite ceramic materials (Ba 1 / 3 Sr1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 ) Preparation of O3:

[0081] (1) BaCO3, SrCO3, CaCO3, TiO2 and SnO2 raw materials with a purity of more than 99.9% are dried at 110°C for 12 hours before mixing, and are accurately weighed according to the stoichiometric ratio and then mixed (accurate to 0.0001g) to obtain a mixed material, wherein the molar ratio of the metal elements of BaCO3, SrCO3 and CaCO3 is 1:1:1, and the molar ratio of the metal elements of SnO2 and TiO2 is 1:4; the mixed material is added to a ball mill and wet-milled, the grinding balls are zirconium oxide balls, anhydrous ethanol is added as a ball milling medium, the mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2, and the mixed material is fully ball milled at a speed of 300r / min for 6 hours, and the ball-milled material is placed in a 120°C oven for drying for 2 hours;

[0082] (2) pre-calcining the dried material in step (1) in an air atmosphere at a temperature of 5°C / min from room temperature to 1100°C for 4 hours to obtain a pre-calcined powder;

[0083] (3) adding the calcined powder obtained in step (2) into a ball mill and performing wet ball milling, wherein the grinding balls are zirconium oxide balls and anhydrous ethanol is added as the ball milling medium, and the mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2, and the mixture is fully ball milled at a speed of 300 r / min for 6 hours, and the ball milled material is placed in a 120° C. oven and dried for 2 hours;

[0084] (4) adding a polyvinyl alcohol solution having a binder mass concentration of 5% to the pre-burned powder dried in step (3) and granulating the pre-burned powder, wherein the amount of polyvinyl alcohol added is 3% of the total mass of the pre-burned powder, passing through a 60-mesh sieve, and dry-pressing the pre-burned powder into a cylindrical green body with a diameter of 8 mm using a powder tablet press at a pressure of 8 MPa. The pressure holding time is 1 minute, and then the cylindrical green body is debinded at 550° C. for 8 hours at a heating rate of 2° C. / min;

[0085] (5) The cylindrical green body after debinding was heated to 1450°C at a rate of 3°C / min in an air atmosphere and sintered at this temperature for 6 hours to obtain (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )O3 oxide ceramic material.

[0086] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti0.8 ) XRD spectrum of O3 oxide ceramic material is shown in Figure 4 , showing that it has been synthesized (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )O3 phase.

[0087] The (Ba prepared in this embodiment 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )O3 oxide ceramic material preparation (Ba 1 / 3Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )O3 relaxor ferroelectric ceramic material, the specific method is:

[0088] will (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 The upper and lower surfaces of the O3 oxide ceramic material were ground smooth to a thickness of 0.10 mm, and then silver-plated electrodes were sintered at 650°C for 30 minutes and cooled to obtain (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )O3 relaxor ferroelectric ceramic material.

[0089] Figure 5 For this embodiment (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.2 Ti 0.8 )PE curve of O3 relaxor ferroelectric ceramic material at 10Hz frequency. The available energy storage density (W) under 390kV / cm electric field is calculated. rec ) reaches 4.88J / cm 3 , the energy storage efficiency (η) reaches 92.92%.

[0090] Example 3

[0091] A, B component superparaelectric phase perovskite ceramic materials (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 ) Preparation of O3:

[0092] (1) BaCO3, SrCO3, CaCO3, TiO2 and SnO2 raw materials with a purity of more than 99.9% are dried at 110°C for 12 hours before mixing, and are accurately weighed according to the stoichiometric ratio and then mixed (accurate to 0.0001g) to obtain a mixed material, wherein the molar ratio of the metal elements of BaCO3, SrCO3 and CaCO3 is 1:1:1, and the molar ratio of the metal elements of SnO2 and TiO2 is 3:7; the mixed material is added to a ball mill and wet-milled, the grinding balls are zirconium oxide balls, anhydrous ethanol is added as a ball milling medium, the mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2, and the mixed material is fully ball milled at a speed of 360r / min for 6 hours, and the ball-milled material is placed in a 120°C oven for drying for 2 hours;

[0093] (2) pre-calcining the material dried in step (1) in an air atmosphere at a temperature of 3°C / min from room temperature to 1000°C for 6 hours to obtain a pre-calcined powder;

[0094] (3) adding the calcined powder obtained in step (2) into a ball mill and performing wet ball milling. The grinding balls are zirconium oxide balls and anhydrous ethanol is added as the ball milling medium. The mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2. The mixed material is fully ball milled at a speed of 360 r / min for 6 hours. The ball milled material is placed in a 120° C. oven and dried for 3 hours;

[0095] (4) adding a polyvinyl alcohol solution having a binder mass concentration of 5% to the pre-burned powder dried in step (3) and granulating the pre-burned powder, wherein the amount of polyvinyl alcohol added is 3% of the total mass of the pre-burned powder, passing through a 120-mesh sieve, and dry-pressing the pre-burned powder into a cylindrical green body with a diameter of 10 mm using a powder tablet press at a pressure of 5 MPa. The pressure holding time is 2 minutes, and then the cylindrical green body is debinded at 550° C. for 6 hours at a heating rate of 1.5° C. / min;

[0096] (5) The cylindrical green body after debinding was heated to 1500°C at a rate of 5°C / min in air atmosphere and sintered at this temperature for 4 hours to obtain (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )O3 oxide ceramic material.

[0097] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 ) XRD spectrum of O3 oxide ceramic material is shown in Figure 6 , showing that it has been synthesized (Ba 1 / 3 Sr1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )O3 phase.

[0098] The (Ba prepared in this embodiment 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )O3 oxide ceramic material preparation (Ba 1 / 3Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )O3 relaxor ferroelectric ceramic material, the specific method is:

[0099] will (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )O3 oxide ceramic material upper and lower surfaces are ground smooth, ground to a thickness of 0.15mm, then silver-plated electrodes are plated, sintered at 650℃ for 30 minutes, and cooled to obtain (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )O3 relaxor ferroelectric ceramic material.

[0100] Figure 7 For this embodiment (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.3 Ti 0.7 )PE curve of O3 relaxor ferroelectric ceramic material at 10Hz frequency, and its available energy storage density (W) under 250kV / cm electric field is calculated. rec ) reaches 2.80J / cm 3 , the energy storage efficiency (η) reaches 93.39%.

[0101] Comparative Example 1

[0102] Compared with Example 1, the only difference is the pre-firing temperature, that is, the pre-firing temperature in step (2) is 900°C.

[0103] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 ) XRD spectrum of O3 oxide ceramic material is shown in Figure 8, showing that single phase (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.1 Ti 0.9 )O3.

[0104] Comparative Example 2

[0105] Compared with Example 2, the only difference is that SnO2 is replaced by ZrO2.

[0106] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Zr 0.2 Ti 0.8 ) XRD spectrum of O3 oxide ceramic material is shown in Fig. 9 , indicating that single phase (Ba) cannot be obtained by sintering at 1450℃ 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Zr 0.2 Ti 0.8 )O3.

[0107] Comparative Example 3

[0108] Compared with Example 3, the only difference is that the molar ratio of the metal elements of TiO2 and SnO2 is different, specifically: the molar ratio of the metal elements of BaCO3, SrCO3, and CaCO3 is 1:1:1, and the molar ratio of the metal elements of SnO2 and TiO2 is 3:2.

[0109] The (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.6 Ti 0.4 ) XRD spectrum of O3 oxide ceramic material is shown in Fig.10 , indicating that there is an impurity phase under 1500℃ sintering conditions, and a single phase cannot be obtained (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn 0.6 Ti 0.4 )O3.

[0110] By observing the data of Comparative Examples 1, 2 and 3, it is found that the presence of the second phase will become a concentrated area of ​​the electric field, thereby reducing the breakdown field strength. At the same time, the second phase will introduce other dielectric loss mechanisms, resulting in increased dielectric loss and thus reducing the energy storage efficiency and energy storage density of the material. Therefore, the relaxor ferroelectric ceramic material prepared in the above comparative example will significantly reduce the comprehensive energy storage performance, and the practical application value is not great.

[0111] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A superparaelectric perovskite ceramic material with A and B components, characterized in that: The general structural formula is ABO3, where the A position is composed of three elements: Ba, Sr and Ca, and the B position is composed of two elements: Ti and Sn; The three elements at the A position occupy the A position in an equimolar ratio, and the molar ratio of the two elements Ti and Sn at the B position is (9-7):(1-3).

2. The superparaelectric perovskite ceramic material of A and B components according to claim 1, characterized in that: The chemical formula of the superparaelectric perovskite ceramic material of the A and B components is (Ba 1 / 3 Sr 1 / 3 Ca 1 / 3 )(Sn x Ti 1-x )O3, where 0.1≤x≤0.3; The perovskite structure of the superparaelectric perovskite ceramic material of the A and B components belongs to the cubic crystal system, and the space group is— Pm3m.

3. A method for preparing the superparaelectric perovskite ceramic material of A and B components according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) According to the stoichiometric ratio of the superparaelectric perovskite ceramic materials of the A and B components, the raw materials BaCO3, SrCO3, CaCO3, TiO2 and SnO2 are weighed and added into a ball mill, the grinding balls are zirconium oxide balls, anhydrous ethanol is added as the ball milling medium, and the ball mill is placed in a planetary ball mill, and dried after ball milling; (2) pre-calcining the dried material in step (1) at 1000° C. to 1100° C. for 4 to 6 hours in an air atmosphere to obtain a pre-calcined powder; (3) adding the pre-sintered powder into a ball mill, using zirconium oxide balls as the grinding balls, adding anhydrous ethanol as the ball milling medium, placing the ball mill into a planetary ball mill, and drying after ball milling; (4) adding a polyvinyl alcohol solution to the pre-burned powder dried in step (3) to granulate, sieving the granules, dry-pressing them into cylindrical green bodies, and then debinding the cylindrical green bodies; (5) The cylindrical green body after debinding is sintered at a temperature of 1400° C. to 1500° C. for 4 to 6 hours in an air atmosphere to obtain the superparaelectric perovskite ceramic material of the A and B components.

4. The method for preparing the superparaelectric perovskite ceramic material of A and B components according to claim 3, characterized in that: In step (1), the mass ratio of the mixed material, the grinding balls and the ball milling medium is 1:2:2; The ball milling is performed at a rotation speed of 300-360 r / min for 6 hours, and the ball-milled material is dried at 120° C. for 2-3 hours.

5. The method for preparing the superparaelectric perovskite ceramic material of A and B components according to claim 3, characterized in that: In step (3), the ball milling is performed at a rotation speed of 300 to 360 r / min for 6 hours, and the ball-milled material is dried at 120° C. for 2 to 3 hours.

6. The method for preparing the superparaelectric perovskite ceramic material of A and B components according to claim 3, characterized in that: In step (4), the mass concentration of the polyvinyl alcohol solution is 5%; The sieving is through a 60-120 mesh sieve; The uniaxial pressure during dry pressing is 5-8 MPa, and the holding time is 1-2 minutes; The debinding is carried out at 550° C. for 6 to 8 hours, with a heating rate of 1.5 to 2° C. / min.

7. A relaxor ferroelectric material based on superparaelectric perovskite ceramic materials of A and B components, characterized in that: The superparaelectric perovskite ceramic material of the A and B components is the superparaelectric perovskite ceramic material of the A and B components as claimed in any one of claims 1 to 2.

8. A method for preparing a relaxor ferroelectric material based on superparaelectric perovskite ceramic materials of A and B components as claimed in claim 7, characterized in that: Silver electrodes are plated on the upper and lower surfaces of the A and B component superparaelectric phase perovskite type ceramic materials, and after calcination and cooling, the relaxor ferroelectric material based on the A and B component superparaelectric phase perovskite type ceramic materials is obtained.

9. The method for preparing a relaxor ferroelectric material based on superparaelectric phase perovskite ceramic materials of A and B components according to claim 8, characterized in that: The thickness of the superparaelectric perovskite ceramic material of the A and B components is 0.10 to 0.15 mm, and the surface of the superparaelectric perovskite ceramic material of the A and B components is ground smooth before the silver electrode is plated; The calcination temperature is 650° C. and the heat preservation time is 30 minutes.

10. Application of the superparaelectric phase perovskite ceramic material of A and B components as described in any one of claims 1 to 2 or the relaxor ferroelectric material based on the superparaelectric phase perovskite ceramic material of A and B components as described in claim 7 in the field of dielectric energy storage.

Citation Information

Patent Citations

  • Sn-doped high-entropy perovskite oxide ceramic material with high power density, and preparation method thereof

    CN111039672A

  • A-bit and B-bit common high-entropy perovskite type high-entropy ceramic material as well as preparation method and application of A-bit and B-bit common high-entropy perovskite type high-entropy ceramic material

    CN117049875A

  • Sodium bismuth titanate-based multilayer ceramic capacitor with high energy storage performance and wide practical temperature range and preparation method of sodium bismuth titanate-based multilayer ceramic capacitor

    CN117936269A

  • Dielectric ceramic

    EP0270099A2

  • Composite oxide ceramic, manufacturing method therefor and antenna

    JP2018020941A