Surface modified steel fiber toughened bauxite castable and preparation method thereof
By modifying the surface of the steel fiber and adding modified steel fibers to the bauxite castable, the problems of easy oxidation and low bonding strength in the prior art are solved, and the fracture toughness, flexural strength and Thermal shock stability.
Patent Information
- Application Number
- CN202411135461.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing bauxite castables are easily oxidized under high temperature conditions, resulting in a decrease in material strength and the bonding strength between the fiber and the castable matrix is low, affecting the mechanical properties of the material.
By modifying the surface of the steel fiber, the hydrophilic groups are loaded and silica is coated to enhance the oxidation resistance of the fibers, and the modified steel fibers are added to the bauxite castable, and the interface is enhanced through the mulle petrochemical reaction Binding strength.
The fracture toughness, flexural strength and thermal shock stability of steel fiber toughened bauxite castable are significantly improved, the bonding force between the fiber and the matrix is enhanced, and the performance of the material at high temperatures is improved.
Abstract
Description
Technical field:
[0001] The invention belongs to the technical field of refractory materials, and particularly relates to a surface-modified steel fiber toughened bauxite castable and a preparation method thereof. Background technology:
[0002] Bauxite castables are widely used as refractory linings in alloy and steel smelting industries due to their good mechanical strength, refractoriness and corrosion resistance. However, with the continuous progress and development of the metallurgical industry, smelting conditions have gradually become harsh and higher requirements have been placed on smelting equipment. Among them, refractory linings are an important component of smelting equipment, and the quality of their performance has a significant impact on the service performance of smelting equipment. In order to improve the thermal shock stability, flexural strength and fracture toughness of bauxite castables, reinforcing and toughening materials such as carbon fibers and steel fibers are usually added to the castable matrix. However, due to the cross-sectional effect, the bonding strength between the fiber and the castable matrix is low, which seriously affects the reinforcement effect of the fiber material. Therefore, optimizing the fiber-matrix bonding interface to improve the mechanical properties of the castable has become an urgent problem to be solved.
[0003] The patent "Corundum Silicon Carbide Steel Fiber Castable Material" with publication number CN110066181B discloses a corundum silicon carbide steel fiber castable material prepared from raw materials such as dense corundum, white corundum, silicon carbide, silicon oxide powder, aluminum oxide powder, modified silica sol, composite additives, chromium oxide, magnesium oxide, cement, etc. This method improves the thermal shock stability and flexural strength of the corundum silicon carbide castable material to a certain extent. However, its main defects are: (1) The interface effect between the steel fiber and the castable matrix still exists, affecting the mechanical properties of the material. (2) The steel fiber is easily oxidized under high temperature oxidizing atmosphere conditions, resulting in a decrease in material strength.
[0004] The patent "Aluminum dihydrogen phosphate combined with steel fiber reinforced refractory castable and preparation method" with publication number CN109734462A discloses an aluminum dihydrogen phosphate combined with steel fiber reinforced refractory castable prepared from high-aluminum raw materials, kyanite, silicon powder, α-Al2O3 powder, ρ-Al2O3 powder, magnesium aluminum spinel, heat-resistant steel fiber and aluminum dihydrogen phosphate-based composite binder. This method uses a high-bonding strength aluminum dihydrogen phosphate-based composite binder to improve the bonding strength between steel fibers and the castable matrix corundum silicon carbide castable to a certain extent. However, its main defects are: (1) The interface effect between steel fibers and the castable matrix is not completely improved, and there are still problems such as low bonding strength. (2) Under high temperature conditions, the steel fibers in the castable are easily oxidized to generate impurities such as iron oxide, which affect the high-temperature performance of the material.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention:
[0006] The object of the present invention is to provide a surface modified steel fiber toughened bauxite castable and a preparation method thereof, thereby overcoming the defects in the above-mentioned prior art.
[0007] To achieve the above-mentioned purpose, the present invention provides a surface-modified steel fiber toughened bauxite castable, whose mass components are: 60-80 parts of 85 bauxite clinker, 3-9 parts of activated alumina powder, 2-6 parts of silica powder, 2-4 parts of pure calcium aluminate cement, 1-3 parts of surface-modified heat-resistant steel fiber and 0.05-0.15 parts of water reducer; wherein 85 bauxite clinker, activated alumina powder, silica powder and pure calcium aluminate cement are used as raw materials, and surface-modified heat-resistant steel fiber and water reducer are used as additives.
[0008] Preferably, in the technical solution, the particle gradation of 85 bauxite clinker is: particle size is 5-8mm, 3-5mm, 1-3mm, 0-1mm, 200 mesh and 325 mesh.
[0009] Preferably, in the technical solution, the diameter of the surface modified heat-resistant steel fiber is ≥0.2 mm and the length is ≥5 mm.
[0010] A method for preparing a surface-modified steel fiber toughened bauxite castable, comprising the steps of: (1) mixing 10-25 parts by weight of a silane coupling agent, 5-10 parts by weight of anhydrous ethanol and 60-80 parts by weight of deionized water, immersing the steel fiber in the mixed solution for 5-10 minutes, and treating the steel fiber with ultrasound;
[0011] (2) taking out the steel fiber and drying it at 80° C. for 2-3 hours, then immersing it in silica sol under vacuum for 20-30 minutes, then taking it out and drying it at 100° C. for 6-8 hours to obtain a surface-modified heat-resistant steel fiber;
[0012] (3) 60-80 parts by weight of 85 bauxite clinker, 3-9 parts by weight of activated alumina powder, 2-6 parts by weight of silica powder, and 2-4 parts by weight of pure calcium aluminate cement are used as raw materials, 1-3 parts by weight of surface-modified heat-resistant steel fiber and 0.05-0.15 parts by weight of water reducer are used as additives, the raw materials and additives are poured into a mixer and stirred, and the mixture is stirred evenly to obtain a surface-modified steel fiber toughened bauxite castable.
[0013] Preferably, in the technical solution, in step (2), the pH of the silica sol is greater than 9, and the SiO2 concentration is greater than or equal to 10 wt%.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] The steel fiber is pretreated by surface modification technology, and the hydrophilic groups are loaded on the fiber surface to achieve the coating of the steel fiber by silica sol. On this basis, the steel fiber reinforced toughened bauxite castable is prepared by adding the surface modified steel fiber to the bauxite castable. Since the surface of the prepared steel fiber is covered with a layer of silica, the contact between oxygen and the steel fiber matrix is hindered, and the oxidation resistance of the steel fiber at high temperature is effectively improved. In addition, under high temperature conditions, the silica layer on the surface of the steel fiber and the alumina in the castable matrix can undergo secondary mullite and generate a large number of mullite whiskers at the bonding interface, which improves the interface effect between the steel fiber and the castable and increases the bonding strength. Therefore, by modifying the surface of the steel fiber and adding it to the castable, it plays an important role in the interfacial debonding effect and fiber pull-out effect of the reinforcing fiber in the matrix.
[0016] Compared with conventional steel fiber toughened bauxite castables, the surface modified steel fiber toughened bauxite castables prepared by the present invention have a specific fracture energy increased by 23-52% after heat treatment at 110°C×24h and 1400°C×3h, a room temperature / high temperature flexural strength increased by 30-50%, and a thermal shock water cooling number increased by 15-30%. Therefore, the fracture toughness, flexural strength and thermal shock stability of the steel fiber toughened bauxite castables are significantly improved by modifying the steel fiber surface. Specific implementation method:
[0017] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0018] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0019] Example 1
[0020] A surface-modified steel fiber toughened bauxite castable, the mass components of which are: 60-70 parts of 85 bauxite clinker, 6-9 parts of activated alumina powder, 4-6 parts of silica powder, 3-4 parts of pure calcium aluminate cement, 2-3 parts of surface-modified heat-resistant steel fiber and 0.10-0.15 parts of water reducer; wherein 85 bauxite clinker, activated alumina powder, silica powder, pure calcium aluminate cement are used as raw materials, and surface-modified heat-resistant steel fiber and water reducer are used as additives. The particle gradation of 85 bauxite clinker is: particle size is 5-8mm, 3-5mm, 1-3mm, 0-1mm, 200 mesh and 325 mesh. The diameter of the surface-modified heat-resistant steel fiber is ≥0.2mm, and the length is ≥5mm.
[0021] A method for preparing a surface-modified steel fiber toughened bauxite castable, comprising the steps of: (1) mixing 18-25 parts by weight of a silane coupling agent, 7-10 parts by weight of anhydrous ethanol and 70-80 parts by weight of deionized water, immersing the steel fiber in the mixed solution for 5-10 minutes, and treating the steel fiber with ultrasound;
[0022] (2) taking out the steel fiber and drying it at 80° C. for 2-3 hours, then immersing it in silica sol for 20-30 minutes under vacuum conditions, the pH of the silica sol being greater than 9, the SiO2 concentration being greater than or equal to 10 wt%, then taking it out and drying it at 100° C. for 6-8 hours to obtain a surface-modified heat-resistant steel fiber;
[0023] (3) 60-70 parts by weight of 85 bauxite clinker, 6-9 parts by weight of activated alumina powder, 4-6 parts by weight of silica powder, and 3-4 parts by weight of pure calcium aluminate cement are used as raw materials, 2-3 parts by weight of surface-modified heat-resistant steel fiber and 0.10-0.15 parts by weight of water reducer are used as additives, the raw materials and additives are poured into a mixer and stirred, and the surface-modified steel fiber toughened bauxite castable is obtained by stirring evenly.
[0024] Compared with conventional steel fiber toughened bauxite castables, the surface modified steel fiber toughened bauxite castable prepared in Example 1 has a specific fracture energy increased by 37-52% after heat treatment at 110°C×24h and 1400°C×3h, a room temperature / high temperature flexural strength increased by 40-50%, and a thermal shock water cooling number increased by 23-30%.
[0025] Example 2
[0026] A surface-modified steel fiber toughened bauxite castable, the mass components of which are: 70-80 parts of 85 bauxite clinker, 3-6 parts of activated alumina powder, 2-4 parts of silica powder, 2-3 parts of pure calcium aluminate cement, 1-2 parts of surface-modified heat-resistant steel fiber and 0.05-0.10 parts of water reducer; wherein 85 bauxite clinker, activated alumina powder, silica powder, pure calcium aluminate cement are used as raw materials, and surface-modified heat-resistant steel fiber and water reducer are used as additives. The particle gradation of 85 bauxite clinker is: particle size is 5-8mm, 3-5mm, 1-3mm, 0-1mm, 200 mesh and 325 mesh. The diameter of the surface-modified heat-resistant steel fiber is ≥0.2mm, and the length is ≥5mm.
[0027] A method for preparing a surface-modified steel fiber toughened bauxite castable, comprising the steps of: (1) mixing 10-18 parts by weight of a silane coupling agent, 5-7 parts by weight of anhydrous ethanol and 60-70 parts by weight of deionized water, immersing the steel fiber in the mixed solution for 5-10 minutes, and treating the steel fiber with ultrasound;
[0028] (2) taking out the steel fiber and drying it at 80° C. for 2-3 hours, then immersing it in silica sol for 20-30 minutes under vacuum conditions, the pH of the silica sol being greater than 9, the SiO2 concentration being greater than or equal to 10 wt%, then taking it out and drying it at 100° C. for 6-8 hours to obtain a surface-modified heat-resistant steel fiber;
[0029] (3) 70-80 parts by weight of 85 bauxite clinker, 3-6 parts by weight of activated alumina powder, 2-4 parts by weight of silica powder, and 2-3 parts by weight of pure calcium aluminate cement are used as raw materials, 1-2 parts by weight of surface-modified heat-resistant steel fiber and 0.05-0.10 parts by weight of water reducer are used as additives, the raw materials and additives are poured into a mixer and stirred, and the surface-modified steel fiber toughened bauxite castable is obtained by stirring evenly.
[0030] Compared with conventional steel fiber toughened bauxite castables, the surface modified steel fiber toughened bauxite castable prepared in Example 2 has a 23-37% increase in specific fracture energy after heat treatment at 110°C×24h and 1400°C×3h, a 30-40% increase in room temperature / high temperature flexural strength, and a 15-23% increase in the number of thermal shock water cooling times.
[0031] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A surface modified steel fiber toughened bauxite castable, characterized in that: The mass components thereof are 60-80 parts of 85 bauxite clinker, 3-9 parts of activated alumina powder, 2-6 parts of silica powder, 2-4 parts of pure calcium aluminate cement, 1-3 parts of surface modified heat-resistant steel fiber and 0.05-0.15 parts of water reducing agent; Among them, 85 bauxite clinker, activated alumina powder, silica powder, and pure calcium aluminate cement are used as raw materials, and surface modified heat-resistant steel fiber and water reducing agent are used as additives.
2. The surface modified steel fiber toughened bauxite castable according to claim 1, characterized in that: The particle size distribution of 85 bauxite clinker is: particle size 5-8mm, 3-5mm, 1-3mm, 0-1mm, 200 mesh and 325 mesh.
3. The surface modified steel fiber toughened bauxite castable according to claim 1, characterized in that: The diameter of the surface modified heat-resistant steel fiber is ≥0.2mm and the length is ≥5mm.
4. A method for preparing a surface-modified steel fiber toughened bauxite castable according to any one of claims 1 to 3, comprising the steps of: (1) mixing 10-25 parts by weight of a silane coupling agent, 5-10 parts by weight of anhydrous ethanol and 60-80 parts by weight of deionized water, immersing the steel fiber in the mixed solution for 5-10 minutes, and treating the mixture by ultrasound; (2) taking out the steel fiber and drying it at 80° C. for 2-3 hours, then immersing it in silica sol under vacuum for 20-30 minutes, then taking it out and drying it at 100° C. for 6-8 hours to obtain a surface-modified heat-resistant steel fiber; (3) 60-80 parts by weight of 85 bauxite clinker, 3-9 parts by weight of activated alumina powder, 2-6 parts by weight of silica powder, and 2-4 parts by weight of pure calcium aluminate cement are used as raw materials, 1-3 parts by weight of surface-modified heat-resistant steel fiber and 0.05-0.15 parts by weight of water reducer are used as additives, the raw materials and additives are poured into a mixer and stirred, and the mixture is stirred evenly to obtain a surface-modified steel fiber toughened bauxite castable.
5. The method for preparing the surface modified steel fiber toughened bauxite castable according to claim 4, characterized in that: In step (2), the pH of the silica sol is greater than 9, and the SiO2 concentration is greater than or equal to 10 wt%.
Citation Information
Patent Citations
Aluminum dihydrogen phosphate and steel fiber reinforced refractory castable and preparation method
CN109734462A
Corundum silicon carbide steel fiber castable
CN110066181B
High-strength steel fibre castable
CN101734934A
Composite bonding wear-resistant castable refractory
CN102491768A
Alumina-based refractory castable for molten steel treatment spray gun
CN114380582A
Cited By
A surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method
CN123062282A