Formaldehyde-free quick-dry two-component polyurethane resin and preparation method thereof
Through the technology of formaldehyde-free quick-drying two-component polyurethane resin, combined with epoxy end capping and thiol end capping, the problems of low production efficiency and formaldehyde release of existing polyurethane adhesives are solved, and high peeling is achieved The dual advantages of strength and environmental protection.
Patent Information
- Application Number
- CN202411119167.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The existing soft two-component polyurethane adhesives have low production efficiency and formaldehyde release problems in the field of clothing leather. The isocyanate curing agent reacts quickly but needs to be matured 24 hours. The melamine curing agent has low strength and contains formaldehyde, which is harmful. Human health.
Using formaldehyde-free quick-drying two-component polyurethane resin, the epoxy-capped polyurethane prepolymer is combined with the thiol-capped polyurethane prepolymer, forming a spatial network structure at 150-170°C to enhance the bonding strength, and The product is free of formaldehyde emission through specific formulas and processes.
It has achieved the improvement of high peel strength and production efficiency, while meeting environmental protection indicators, avoiding formaldehyde release, simplifying the production process, and facilitating industrial manufacturing.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polyurethane adhesives, and in particular to a formaldehyde-free quick-drying two-component polyurethane resin and a preparation method thereof. Background Art
[0002] Polyurethane adhesives are a class of compounds containing a carbamate group (-NHCOO-) structure. They have excellent adhesion, weather resistance, wear resistance, oil resistance, chemical resistance, and adjustable hardness. They are widely used in various fields such as textiles, furniture, electronic equipment, food packaging, and automobiles.
[0003] Soft two-component polyurethane adhesives are widely used in the field of garment leather, all of which are made by combining polyurethane resin and curing agent. There are two types of bridging agents used, one is isocyanate-terminated and the other is melamine-terminated. There is a big difference in the performance and usage of these two types of curing agents.
[0004] Isocyanate curing agents have high strength after curing, but there are two main problems. First, isocyanate reacts quickly with active hydrogen at room temperature and reacts with moisture in the air and active hydrogen in polyurethane. Therefore, the prepared materials must be used up as soon as possible, otherwise the viscosity of the prepared materials will gradually increase until particles and cross-linked structures are produced, and finally completely cured into a three-dimensional structure; second, the reaction between isocyanate and active hydrogen is a gradual reaction, and the reaction continues after the finished product is off the line, so it needs to be placed for more than 24 hours to ensure that the isocyanate is completely reacted. This reduces production efficiency and requires a special aging room to place it, resulting in a waste of resources.
[0005] Melamine curing agents can react instantly with hydroxyl groups in polyurethane resins at 130-150°C, and have high production efficiency. However, the melamine curing agent technology also has two disadvantages: first, the final product strength is not high, and the final peel strength is significantly lower than that of isocyanate curing agent products; second, melamine curing agents contain formaldehyde, which is seriously harmful to the human body. Due to the instability of the production line, formaldehyde in synthetic leather is often not completely dried and remains, causing harm to the health of users. Summary of the invention
[0006] In order to solve the technical difficulties existing in the above-mentioned existing soft two-component polyurethane adhesives, the inventors provide a formaldehyde-free quick-drying two-component polyurethane resin and a preparation method thereof, which can not only ensure the product peeling strength and production efficiency, but also ensure that the product releases no formaldehyde during use and meets environmental protection indicators.
[0007] The present application provides a formaldehyde-free quick-drying two-component polyurethane resin, which is achieved through the following technical solutions: A formaldehyde-free quick-drying two-component polyurethane resin is prepared from component A and component B, wherein component A is an epoxy-terminated polyurethane prepolymer; component B is a thiol-terminated polyurethane prepolymer; the ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is (0.95-1.20):1; The component A comprises diisocyanate, polydiol, chain extender, catalyst, functional additive and epoxy resin; The molar amount of active hydroxyl groups in the polyglycol and chain extender in component A is equal to 0.90-0.97 times the molar amount of -NCO in the diisocyanate; the sum of the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A and the molar amount of epoxy groups in the epoxy resin is greater than the molar amount of -NCO in the diisocyanate; The epoxy resin in component A includes at least one of E51, E44, E20, and E12; The chain extender in the A component is at least one of a diol or a triol having a molecular weight of 61-500 g / mol; The B component includes diisocyanate, polydiol, catalyst, functional additive and dithiol; The molar amount of active hydroxyl groups in the polyglycol in the B component is equal to 0.30-0.95 times the molar amount of -NCO in the diisocyanate; the sum of the molar amount of neutral hydroxyl groups in the polyglycol in the A component and the molar amount of sulfide groups in the dithiol is greater than the molar amount of -NCO in the diisocyanate; the dithiol in the B component includes at least one of ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, and 1,6-hexanedithiol; The diisocyanate in the A component and the B component is at least one of 4,4-diphenylmethane diisocyanate, MDI-50, toluene diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate and 1,6-hexyl diisocyanate; The polyglycol in the A component and the B component is at least one of a polyester diol, a polyether diol and a polycarbonate diol having a number average molecular weight of 1000-4000 g / mol; The catalyst in the components A and B is organic tin and / or organic bismuth; the functional additive in the components A and B is at least one of an antioxidant, an ultraviolet absorber, a stabilizer, an anti-hydrolysis agent, and a flame retardant.
[0008] Preferably, the ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is (1.06-1.12):1.
[0009] Preferably, the ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is 1.10:1.
[0010] The formaldehyde-free quick-drying two-component polyurethane resin in this application, when synthesizing component A, since epoxy resin contains hydroxyl groups, the hydroxyl groups will react with isocyanate and be connected to the molecular chain; after mixing with component B, at 150-170°C, the epoxy group will open the ring and react with the active hydrogen on the thiol to form a spatial network structure, improve the mechanical properties of the resin, and thus produce suitable bonding strength. The final product can not only meet environmental protection requirements, but also has the performance of quick drying and high peel strength, ensuring the production efficiency and production quality of the product.
[0011] Preferably, the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A is equal to 0.94-0.97 times the molar amount of -NCO in the diisocyanate; the molar amount of epoxy groups in the epoxy resin is 1.2-3.0 times the difference between the molar amount of -NCO in the diisocyanate and the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A.
[0012] Preferably, the molar amount of active hydroxyl groups in the polyglycol in the B component is equal to 0.70-0.92 times the molar amount of -NCO in the diisocyanate; the ratio of the molar amount of neutral hydroxyl groups in the polyglycol in the A component to the molar amount of sulfhydryl groups in the dithiol is (0.5-1.8):1.
[0013] Preferably, the ratio of the molar amount of neutral hydroxyl groups in the polyglycol in the A component to the molar amount of sulfhydryl groups in the dithiol is (1.4-1.8):1.
[0014] By adopting the above technical solution, the peel strength and production efficiency of the formaldehyde-free quick-drying two-component polyurethane resin can be improved, while ensuring that the formaldehyde-free quick-drying two-component polyurethane resin product does not release formaldehyde and meets environmental emission standards.
[0015] The present application provides a method for preparing a formaldehyde-free quick-drying two-component polyurethane resin, which is achieved by the following technical scheme: A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin, comprising the following steps: Preparation of component A: Evenly mix diisocyanate, catalyst, some functional additives and solvent, and heat to 40-60°C; gradually add polyglycol, chain extender and remaining functional additives under stirring, heat and stir to react until the viscosity of the reactant reaches 2.0×104~14.0×104mPa•s / 25°C, add epoxy resin and stir to react for 0.5-2h to obtain component A; Preparation of component B: Mix the diisocyanate and the solvent evenly, and heat to 40-60°C; gradually add the polyglycol while stirring, heat and stir to react until the viscosity of the reactant reaches 1.0×103~2.0×104mPa•s / 25°C, add dithiol for end-capping reaction for 0.5-2h to obtain component B; Component A and component B are mixed at an epoxy group / active hydrogen molar ratio of 0.95-1.2, and a tertiary amine catalyst is added, stirred evenly, and then added to obtain a formaldehyde-free quick-drying two-component polyurethane resin. The obtained formaldehyde-free quick-drying two-component polyurethane resin is used to bond the synthetic leather surface layer and the base fabric, and the final synthetic leather is obtained by baking at 130-170°C for 5-15 minutes.
[0016] Preferably, the molar ratio of the component A to the component B is 1.10 based on the epoxy group / active hydrogen.
[0017] Preferably, the added amount of the tertiary amine catalyst is 1-5% of the mass of component A; the tertiary amine catalyst is at least one of triethylenediamine, tetramethylethylenediamine, and N,N-dimethylcyclohexylamine.
[0018] The preparation method provided in this application is relatively simple, has low implementation difficulty, and is easy to implement for industrial production.
[0019] In summary, this application has the following advantages: 1. This application must ensure both product peeling strength and production efficiency, as well as formaldehyde-free product release and environmental protection standards.
[0020] 2. The preparation method provided in this application is relatively simple, has low implementation difficulty, and is easy to implement for industrial production. DETAILED DESCRIPTION
[0021] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples. Example
[0022] A formaldehyde-free quick-drying two-component polyurethane resin is made of component A and component B, wherein component A is an epoxy-terminated polyurethane prepolymer; component B is a thiol-terminated polyurethane prepolymer. The ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is (0.95-1.20):1. Preferably, the ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is (1.06-1.12):1. Further preferably, the ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is 1.10:1.
[0023] Component A comprises diisocyanate, polydiol, chain extender, catalyst, functional additive and epoxy resin.
[0024] The molar amount of active hydroxyl groups in the polyglycol and chain extender in component A is equal to 0.90-0.97 times the molar amount of -NCO in diisocyanate. The sum of the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A and the molar amount of epoxy groups in the epoxy resin is greater than the molar amount of -NCO in diisocyanate. Preferably, the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A is equal to 0.94-0.97 times the molar amount of -NCO in diisocyanate; the molar amount of epoxy groups in the epoxy resin is 1.2-3.0 times the difference between the molar amount of -NCO in diisocyanate and the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A.
[0025] The epoxy resin in component A includes at least one of E51, E44, E20 and E12.
[0026] The chain extender in component A is at least one of diol and triol with a molecular weight of 61-500 g / mol.
[0027] The B component comprises diisocyanate, polydiol, catalyst, functional additive and dithiol.
[0028] The molar amount of active hydroxyl groups in the polydiol in component B is equal to 0.30-0.95 times the molar amount of -NCO in diisocyanate. The sum of the molar amount of neutral hydroxyl groups in the polydiol in component A and the molar amount of sulfide groups in dithiol is greater than the molar amount of -NCO in diisocyanate. The dithiol in component B includes at least one of ethanedithiol, 1,3 propanedithiol, 1,4 butanedithiol, and 1,6 hexanedithiol. Preferably, the molar amount of active hydroxyl groups in the polydiol in component B is equal to 0.70-0.92 times the molar amount of -NCO in diisocyanate. The ratio of the molar amount of neutral hydroxyl groups in the polydiol in component B to the molar amount of sulfide groups in dithiol is (0.5-1.8):1. Preferably, the ratio of the molar amount of neutral hydroxyl groups in the polydiol in component B to the molar amount of sulfide groups in dithiol is (1.4-1.8):1.
[0029] The diisocyanate in the A component and the B component is at least one of 4,4-diphenylmethane diisocyanate, MDI-50, toluene diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate and 1,6-hexyl diisocyanate.
[0030] The polyglycol in the A component and the B component is at least one of polyester glycol, polyether glycol and polycarbonate glycol having a number average molecular weight of 1000-4000 g / mol.
[0031] The catalyst in the A component and the B component is organic tin and / or organic bismuth.
[0032] The functional auxiliary agent in component A and component B is at least one of an antioxidant, an ultraviolet absorber, a stabilizer, an anti-hydrolysis agent, and a flame retardant.
[0033] A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin comprises the following steps: Preparation of component A: Evenly mix diisocyanate, catalyst, some functional additives and solvent, and heat to 40-60°C; gradually add polyglycol, chain extender and remaining functional additives under stirring, heat and stir to react until the viscosity of the reactant reaches 2.0×104~14.0×104mPa•s / 25°C, add epoxy resin and stir to react for 0.5-2h to obtain component A; Preparation of component B: Mix the diisocyanate and solvent evenly, raise the temperature to 40-60°C; gradually add polyglycol while stirring, heat and stir until the viscosity of the reactant reaches 1.0×10 3 ~2.0×10 4 mPa•s / 25℃, add dithiol capping reaction for 0.5-2h to obtain component B; Component A and component B are mixed at an epoxy group / active hydrogen molar ratio of 0.95-1.2, and a tertiary amine catalyst is added, stirred evenly, and then added to obtain a formaldehyde-free quick-drying two-component polyurethane resin. The obtained formaldehyde-free quick-drying two-component polyurethane resin is used to bond the synthetic leather surface layer and the base fabric, and the final synthetic leather is obtained by baking at 130-170°C for 5-15 minutes.
[0034] Preferably, the molar ratio of component A to component B is 1.10 based on the epoxy group / active hydrogen.
[0035] Preferably, the added amount of the tertiary amine catalyst is 1-5% of the mass of component A; the tertiary amine catalyst is at least one of triethylenediamine, tetramethylethylenediamine, and N,N-dimethylcyclohexylamine.
[0036] Embodiment 1: A formaldehyde-free quick-drying two-component polyurethane resin is prepared from component A, component B and triethylenediamine, wherein component A is an epoxy-terminated polyurethane prepolymer; component B is a thiol-terminated polyurethane prepolymer.
[0037] Component A was made of 27 g of TDI (toluene diisocyanate), 100 g of polyethylene adipate diol (molecular weight 2000, Zhejiang Hexin Technology Co., Ltd.), 10 g of neopentyl glycol, 0.1 g of bismuth carboxylate, 0.5 g of triphenyl phosphate, 10 g of E-51 epoxy resin Phoenix brand (Guangzhou Taili Chemical Co., Ltd.), and 160 g of DMF (dimethylformamide).
[0038] Component B was prepared from 26 g of MDI (4,4′-diphenylmethane diisocyanate), 150 g of polyethylene adipate 1,4-butanediol ester diol (number average molecular weight 2000, Zhejiang Hexin Technology Co., Ltd.), 0.2 g of antioxidant 1010, 0.1 g of bismuth carboxylate, 5 g of ethanedithiol, and 180 g of DMF (dimethylformamide).
[0039] A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin comprises the following steps: Preparation of component A: TDI, DMF and triphenyl phosphate are all put into a reactor, and the temperature is raised to 50°C and stirred evenly; 100g of polyethylene adipate glycol is put into the reactor, and the reactor temperature is kept at 80°C for reaction for 1h; 10.0g of neopentyl glycol is put into the reactor, and the reactor temperature is kept at 85°C for reaction for 1h, and then bismuth carboxylate is put into the reactor, and the reactor temperature is kept at 85°C for reaction for further reaction. When the viscosity of the reactant reaches 40,000-140,000 cps (25°C), E-51 epoxy resin is added, and the reaction temperature is controlled to 85°C for reaction for 1h. After the NCO content is detected to be 0, component A is obtained by discharging the material; Preparation of component B: 20 g of MDI, 0.2 g of antioxidant, and 180 g of DMF were added to the reactor, heated to 45 ° C, stirred evenly, and 150 g of polyethylene adipate glycol butylene glycol was added. The kettle temperature was controlled at 75 ° C for 1.5 hours, and bismuth carboxylate was added. The kettle temperature was maintained at 75 ° C and the reaction was continued. When the viscosity reached 1.0 × 10 3 ~2.0×10 3 Then ethanedithiol was added, and the kettle temperature was controlled at 75°C for 1 hour. After the NCO content was detected to be 0, the material was discharged to obtain component B; When in use, A and B are mixed in a mass ratio of 1:1.2 (the molar ratio of A to B is 1:0.99), and 4% of the mass of A material is added with triethylenediamine. After rapid stirring, the material is added, and the synthetic leather surface layer (made of HX-6015 surface layer polyurethane produced by Zhejiang Hexin Technology Co., Ltd.) is bonded to the base fabric (stretch fabric), and the final synthetic leather is obtained by baking at 145°C for 10 minutes.
[0040] The difference between Example 2 and Example 1 is that component A is made of 78g of MDI-50, 100g of polyethylene adipate diol (molecular weight 2000, Zhejiang Hexin Technology Co., Ltd.), 100g of polytetrahydrofuran diol (molecular weight 2000, Xiaoxing Chemical), 15g of 1,4-butanediol, 3g of 1,2,3-propylene glycol, 0.02g of bismuth carboxylate, 1g of antioxidant 1010, 10g of E-44 epoxy resin (Phoenix brand bisphenol A type epoxy resin E-44 6101, Jinan Yanglan New Material Technology Co., Ltd.), 100g of ethyl acetate, and 100g of DMF.
[0041] Component B is made of 25 g of MDI (4,4′-diphenylmethane diisocyanate), 150 g of polyoxypropylene glycol (number average molecular weight 2000, Shanghai Dongda Chemical Co., Ltd.), 0.2 g of antioxidant 1010, 0.01 g of stannous octoate, 5.4 g of 1,3-propanedithiol, and 120 g of methyl ethyl ketone.
[0042] A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin comprises the following steps: Preparation of component A: MDI-50, DMF, ethyl acetate, and antioxidant 1010 are all put into a reactor, and the temperature is raised to 50°C and stirred evenly; 100g of polyethylene glycol 1,4-butylene glycol adipate and 100g of polytetrahydrofuran diol are put into the reactor, and the reactor temperature is kept at 75°C for reaction for 1h; 1,4-butanediol and 1,2,3-propylene glycol are put into the reactor, and the reactor temperature is kept at 75°C for reaction for 1h, and bismuth carboxylate is put into the reactor, and the reactor temperature is kept at 75°C for reaction, and when the viscosity of the reactant reaches 20,000-30,000 cps (25°C), E-44 epoxy resin is added, and the reaction temperature is controlled to 85°C for reaction for 1h, and component A is obtained after the NCO content is detected to be 0; Preparation of component B: Add MDI, antioxidant 1010, and methyl ethyl ketone into the reactor, heat to 45°C, stir evenly, add polypropylene oxide glycol, control the kettle temperature at 75°C, react for 1.5 hours, add stannous octoate, keep the kettle temperature at 75°C and continue to react. When the viscosity reaches 5.0×10 3 ~6.0×10 3 Then, 1,3-propanedithiol was added, and the kettle temperature was kept at 75°C for 1 hour. After the NCO content was detected to be 0, the material was discharged to obtain component B; When in use, A and B are mixed in a mass ratio of 1.8:1 (the molar ratio of A to B is 0.97:1), and 2% of the mass of A material is added with N,N-dimethylcyclohexylamine. After rapid stirring, the material is added, the synthetic leather surface layer is bonded to the base fabric, and the final synthetic leather is obtained by baking at 145°C for 10 minutes.
[0043] The difference between Example 3 and Example 1 is that component A is made of 75g of MDI (toluene diisocyanate), 100g of poly(1,4-butylene adipate neopentyl glycol) (molecular weight 3000, Zhejiang Hexin Technology Co., Ltd.), 100g of poly(diethylene phthalate) (molecular weight 2000, Zhejiang Hexin Technology Co., Ltd.), 18g of 1,4-butanediol, 0.02g of bismuth carboxylate, 1g of trimethylolpropane, 0.2g of antioxidant 1010, 10g of E-20 epoxy resin (Baling Petrochemical Epoxy Resin E20, Guangzhou Taili Chemical Co., Ltd.), 200g of DMF (dimethylformamide), and 110g of toluene.
[0044] Component B is made of 15 g of TDI, 20 g of MDI, 150 g of polyneopentyl adipate diol (number average molecular weight 1000, Zhejiang Hexin Technology Co., Ltd.), 0.2 g of antioxidant 1010, 0.02 g of dioctyltin dilaurate, 5 g of 1,4-butanedithiol, and 180 g of DMF (dimethylformamide).
[0045] A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin comprises the following steps: Preparation of component A: MDI, DMF, toluene, and antioxidant 1010 are all put into a reactor, and the temperature is raised to 50°C and stirred evenly; 100g of poly(1,4-butylene adipate) neopentyl glycol ester diol and 100g of poly(diethylene phthalate) diol are put into the reactor, and the reactor temperature is kept at 75°C for reaction for 1h; 1,4-butanediol and trimethylolpropane are put into the reactor, and the reactor temperature is kept at 75°C for reaction for 1h, and then bismuth carboxylate is put into the reactor, and the reactor temperature is kept at 75°C for reaction, and when the viscosity of the reactant reaches 50,000-70,000 cps (25°C), E-20 epoxy resin is added, and the reaction temperature is controlled to 85°C for reaction for 1h. After the NCO content is detected to be 0, component A is obtained; Preparation of component B: Add MDI, antioxidant 1010, and DMF into the reactor, heat to 45°C, stir evenly, add poly(neopentyl adipate glycol) ester diol, control the kettle temperature at 75°C, react for 1.5 hours, add dioctyltin dilaurate, keep the kettle temperature at 75°C and continue to react. When the viscosity reaches 5.0×10 3 ~6.0×10 3 Then add 1,4-butanedithiol, keep the kettle temperature at 75°C for 1 hour, and discharge after the NCO content is detected to be 0 to obtain component B; When in use, A and B are mixed in a mass ratio of 3.06:1 (the molar ratio of A to B is 1.1:1), and 1% of the mass of A material is added with tetramethylethylenediamine. After rapid stirring, the material is added, the synthetic leather surface layer is bonded to the base fabric, and the final synthetic leather is obtained by baking at 145°C for 15 minutes.
[0046] The difference between Example 4 and Example 1 is that component A is made of 48g of 1,6-hexanediisocyanate, 100g of polycaprolactone diol (molecular weight 2000, Hunan Juren Chemical New Material Technology Co., Ltd.), 100g of polytetramethylene glycol (molecular weight 3000, Xiaoxing Chemical), 50g of polycarbonate diol UH-CARB100 (molecular weight 1000, Ube Corporation of Japan), 15g of 1,6-hexanediol, 0.02g of stannous octoate, 0.5g of antioxidant 1010, 10g of E-12 epoxy resin [bisphenol A type epoxy resin E-12 (604), CAS No. 25036-25-3, brand Smek], 75g of dimethyl carbonate, and 150g of DMF (dimethylformamide).
[0047] Component B was prepared from 53 g of H12MDI (dicyclohexylmethane diisocyanate), 150 g of polyhexane adipate diol (number average molecular weight 2000, Zhejiang Hexin Technology Co., Ltd.), 0.2 g of antioxidant 1010, 0.02 g of stannous octoate, 5 g of 1,6-hexanedithiol, and 150 g of DMF (dimethylformamide).
[0048] A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin comprises the following steps: Preparation of component A: put all 1,6-hexanediisocyanate, DMF, dimethyl carbonate, and antioxidant 1010 into a reactor, heat it to 50°C, and stir evenly; put 100g of polycaprolactone diol, 100g of polytetrahydrofuran diol, and 50g of polycarbonate diol into the reactor, keep the reactor temperature at 90°C and react for 1h; put 1,6-hexanediol and trimethylolpropane into the reactor, keep the reactor temperature at 90°C and react for 1h, then put stannous octoate into the reactor, keep the reactor temperature at 85°C and continue to react, when the viscosity of the reactant reaches 100,000-120,000 cps (25°C), add E-12 epoxy resin, control the reaction temperature to 85°C and react for 1h, and after the NCO content is detected to be 0, component A is obtained; Preparation of component B: H12MDI, antioxidant 1010, and DMF were added to the reactor, heated to 45°C, stirred evenly, and then poly(hexanediol adipate) diol was added. The kettle temperature was controlled at 90°C for 1.5 hours, and then stannous octoate was added. The kettle temperature was maintained at 90°C and the reaction was continued until the viscosity reached 3.0×10 4 ~4.0×10 4 Then add 1,6-hexanedithiol, keep the kettle temperature at 90°C for 1 hour, and discharge after the NCO content is detected to be 0 to obtain component B; When in use, A and B are mixed in a mass ratio of 8:1 (the molar ratio of A to B is 1.19:1), and 3% of the mass of A material is added with tetramethylpropylenediamine. After rapid stirring, the material is added, the synthetic leather surface layer is bonded to the base fabric, and the final synthetic leather is obtained by baking at 145°C for 10 minutes.
[0049] The difference between Comparative Example 1 and Example 1 is that the two-component polyurethane resin is made of component A, component B and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is an isocyanate curing agent Wanhua TL-75E.
[0050] Component A is prepared from 27 g of TDI (toluene diisocyanate), 100 g of polyethylene adipate diol, 10 g of neopentyl glycol, 0.1 g of bismuth carboxylate, 0.5 g of triphenyl phosphate, 1.58 g of ethylene glycol, and 160 g of DMF.
[0051] The preparation method of a two-component polyurethane resin comprises the following steps: Preparation of component A: TDI, DMF and triphenyl phosphate are all put into a reactor, and the temperature is raised to 50°C and stirred evenly; 100g of polyethylene adipate glycol is put into the reactor, and the reactor temperature is kept at 80°C for reaction for 1h; 10.0g of neopentyl glycol is put into the reactor, and the reactor temperature is kept at 85°C for reaction for 1h, and then bismuth carboxylate is put into the reactor, and the reactor temperature is kept at 85°C for reaction, and when the viscosity of the reactant reaches 40,000-140,000 cps (25°C), ethylene glycol is added, and the reaction temperature is controlled to 85°C for reaction for 1 hour, and after the NCO content is detected to be 0, component A is obtained; Resin B: Use TL-75E isocyanate curing agent from Wanhua Company; When in use, A and B are mixed evenly in a mass ratio of 100:5 and then added, and 0.01% of the mass of A material, stannous octoate, is added, and the synthetic leather surface layer is bonded to the base fabric, and then baked at 145°C for 10 minutes to obtain the final synthetic leather.
[0052] The difference between Comparative Example 2 and Example 1 is that the two-component polyurethane resin is made of component A and component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is a melamine curing agent.
[0053] Component A is prepared from 27 g of TDI (toluene diisocyanate), 100 g of polyethylene adipate diol, 10 g of neopentyl glycol, 0.1 g of bismuth carboxylate, 0.5 g of triphenyl phosphate, 1.58 g of ethylene glycol, and 160 g of DMF.
[0054] The preparation method of a two-component polyurethane resin comprises the following steps: Preparation of component A: TDI, DMF and triphenyl phosphate are all put into a reactor, and the temperature is raised to 50°C and stirred evenly; 100g of polyethylene adipate glycol is put into the reactor, and the reactor temperature is kept at 80°C for reaction for 1h; 10.0g of neopentyl glycol is put into the reactor, and the reactor temperature is kept at 85°C for reaction for 1h, and then bismuth carboxylate is put into the reactor, and the reactor temperature is kept at 85°C for reaction, and when the viscosity of the reactant reaches 40,000-140,000 cps (25°C), ethylene glycol is added, and the reaction temperature is controlled to 85°C for reaction for 1 hour, and after the NCO content is detected to be 0, component A is obtained; Resin B: Use melamine curing agent (Jiaxing Huhang New Materials Co., Ltd. H-A1360); When in use, A and B are mixed evenly in a mass ratio of 100:5 and then added, and 0.01% of the mass of A material is added with p-toluenesulfonic acid, which is quickly stirred and then added. The synthetic leather surface layer is bonded to the base fabric and baked at 145°C for 10 minutes to obtain the final synthetic leather.
[0055] The difference between Comparative Example 3 and Example 2 is that the two-component polyurethane resin is made of component A, component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is an isocyanate curing agent Wanhua TL-75E.
[0056] Component A is prepared from 78 g of MDI-50, 100 g of polyethylene adipate diol, 100 g of polytetramethylene glycol diol, 15 g of 1,4-butanediol, 3 g of 1,2,3-propylene glycol, 0.02 g of bismuth carboxylate, 1 g of antioxidant 1010, 1.38 g of ethylene glycol, 100 g of ethyl acetate, and 100 g of DMF.
[0057] The difference between Comparative Example 4 and Example 2 is that the two-component polyurethane resin is made of component A, component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is a melamine curing agent.
[0058] Component A is prepared from 78 g of MDI-50, 100 g of polyethylene adipate diol, 100 g of polytetramethylene glycol diol, 15 g of 1,4-butanediol, 3 g of 1,2,3-propylene glycol, 0.02 g of bismuth carboxylate, 1 g of antioxidant 1010, 1.38 g of ethylene glycol, 100 g of ethyl acetate, and 100 g of DMF.
[0059] The difference between Comparative Example 5 and Example 3 is that the two-component polyurethane resin is made of component A, component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is an isocyanate curing agent Wanhua TL-75E.
[0060] Component A is prepared from 75 g of MDI (toluene diisocyanate), 100 g of poly(1,4-butylene adipate neopentyl glycol) ester diol, 100 g of poly(diethylene phthalate) ester diol, 18 g of 1,4-butylene glycol, 0.02 g of bismuth carboxylate, 1 g of trimethylolpropane, 0.2 g of antioxidant 1010, 0.98 g of ethylene glycol, 200 g of DMF, and 110 g of toluene.
[0061] The difference between Comparative Example 6 and Example 3 is that the two-component polyurethane resin is made of component A, component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is a melamine curing agent.
[0062] Component A is prepared from 75 g of MDI (toluene diisocyanate), 100 g of poly(1,4-butylene adipate neopentyl glycol) ester diol, 100 g of poly(diethylene phthalate) ester diol, 18 g of 1,4-butylene glycol, 0.02 g of bismuth carboxylate, 1 g of trimethylolpropane, 0.2 g of antioxidant 1010, 0.98 g of ethylene glycol, 200 g of DMF, and 110 g of toluene.
[0063] The difference between Comparative Example 7 and Example 4 is that the two-component polyurethane resin is made of component A, component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is an isocyanate curing agent Wanhua TL-75E.
[0064] Component A is prepared from 57 g of 1,6-hexamethylene diisocyanate, 100 g of polycaprolactone diol, 100 g of polytetramethylene glycol, 50 g of polycarbonate diol, 15 g of 1,6-hexanediol, 0.02 g of stannous octoate, 0.5 g of antioxidant 1010, 1.33 g of ethylene glycol, 75 g of dimethyl carbonate, and 150 g of DMF (dimethylformamide).
[0065] The difference between Comparative Example 8 and Example 4 is that the two-component polyurethane resin is made of component A, component B, and stannous octoate, wherein component A is a hydroxyl-terminated polyurethane prepolymer; and component B is a melamine curing agent.
[0066] Component A is prepared from 57 g of 1,6-hexamethylene diisocyanate, 100 g of polycaprolactone diol, 100 g of polytetramethylene glycol, 50 g of polycarbonate diol, 15 g of 1,6-hexanediol, 0.02 g of stannous octoate, 0.5 g of antioxidant 1010, 1.33 g of ethylene glycol, 75 g of dimethyl carbonate, and 150 g of DMF (dimethylformamide).
[0067] Table 1: Test parameter table of the final synthetic leather in Examples 1-4 and Comparative Examples 1-8
[0068] Note: Peel strength is tested in accordance with 5.9.2 of QB-T 4197-2011.
[0069] It can be seen from the above data that compared with the isocyanate curing agent solution, the solution of the present invention does not require 24 hours of curing, and the peel strength is basically similar; compared with the melamine curing agent solution, the solution of the present invention has obvious advantages in peel strength; and the present invention does not contain or produce formaldehyde, and has obvious environmental advantages.
[0070] In summary, when synthesizing component A of the formaldehyde-free quick-drying two-component polyurethane resin in this application, since epoxy resin contains hydroxyl groups, the hydroxyl groups will react with isocyanate and be connected to the molecular chain; after mixing with component B, at 150-170°C, the epoxy groups will open the ring and react with the active hydrogen on the thiol to form a spatial network structure, improve the mechanical properties of the resin, and thus produce suitable bonding strength. The final product can meet environmental protection requirements, and at the same time has the performance of quick drying and high peel strength, ensuring the production efficiency and production quality of the product.
[0071] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A formaldehyde-free quick-drying two-component polyurethane resin, characterized in that: The formaldehyde-free quick-drying two-component polyurethane resin is made of component A and component B, wherein component A is an epoxy-terminated polyurethane prepolymer; component B is a thiol-terminated polyurethane prepolymer; the ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is (0.95-1.20):1; The component A comprises diisocyanate, polydiol, chain extender, catalyst, functional additive and epoxy resin; The molar amount of active hydroxyl groups in the polyglycol and chain extender in component A is equal to 0.90-0.97 times the molar amount of -NCO in the diisocyanate; the sum of the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A and the molar amount of epoxy groups in the epoxy resin is greater than the molar amount of -NCO in the diisocyanate; The epoxy resin in component A includes at least one of E51, E44, E20, and E12; The chain extender in the A component is at least one of a diol or a triol having a molecular weight of 61-500 g / mol; The B component includes diisocyanate, polydiol, catalyst, functional additive and dithiol; The molar amount of active hydroxyl groups in the polyglycol in the B component is equal to 0.30-0.95 times the molar amount of -NCO in the diisocyanate; the sum of the molar amount of neutral hydroxyl groups in the polyglycol in the A component and the molar amount of sulfide groups in the dithiol is greater than the molar amount of -NCO in the diisocyanate; the dithiol in the B component includes at least one of ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, and 1,6-hexanedithiol; The diisocyanate in the A component and the B component is at least one of 4,4-diphenylmethane diisocyanate, MDI-50, toluene diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate and 1,6-hexyl diisocyanate; The polyglycol in the A component and the B component is at least one of a polyester diol, a polyether diol and a polycarbonate diol having a number average molecular weight of 1000-4000 g / mol; The catalyst in the components A and B is organic tin and / or organic bismuth; the functional additive in the components A and B is at least one of an antioxidant, an ultraviolet absorber, a stabilizer, an anti-hydrolysis agent, and a flame retardant.
2. The formaldehyde-free quick-drying two-component polyurethane resin according to claim 1, characterized in that: The ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is (1.06-1.12):
1.
3. A formaldehyde-free quick-drying two-component polyurethane resin according to claim 2, characterized in that: The ratio of the molar amount of epoxy groups in the epoxy-terminated polyurethane prepolymer to the molar amount of active hydrogen in the thiol-terminated polyurethane prepolymer is 1.10:
1.
4. The formaldehyde-free quick-drying two-component polyurethane resin according to claim 1, characterized in that: The molar amount of active hydroxyl groups in the polyglycol and chain extender in component A is equal to 0.94-0.97 times the molar amount of -NCO in the diisocyanate; the molar amount of epoxy groups in the epoxy resin is 1.2-3.0 times the difference between the molar amount of -NCO in the diisocyanate and the molar amount of active hydroxyl groups in the polyglycol and chain extender in component A.
5. The formaldehyde-free quick-drying two-component polyurethane resin according to claim 1, characterized in that: The molar amount of active hydroxyl groups in the polyglycol in the B component is equal to 0.70-0.92 times the molar amount of -NCO in the diisocyanate; the ratio of the molar amount of neutral hydroxyl groups in the polyglycol in the A component to the molar amount of sulfhydryl groups in the dithiol is (0.5-1.8):
1.
6. The formaldehyde-free quick-drying two-component polyurethane resin according to claim 5, characterized in that: The ratio of the molar amount of neutral hydroxyl groups in the polyglycol in the A component to the molar amount of sulfhydryl groups in the dithiol is (1.4-1.8):
1.
7. A method for preparing a formaldehyde-free quick-drying two-component polyurethane resin according to any one of claims 1 to 6, characterized in that: The following steps are involved: Preparation of component A: Mix diisocyanate, catalyst, some functional additives and solvent evenly, and heat to 40-60°C; Under stirring, gradually add polyglycol, chain extender, and the remaining functional additives, heat and stir to react until the viscosity of the reactant reaches 2.0×10 4 ~14.0×10 4 mPa•s / 25℃, add epoxy resin and stir to react for 0.5-2h to obtain component A; Preparation of component B: Mix the diisocyanate and solvent evenly, raise the temperature to 40-60°C; gradually add polyglycol while stirring, heat and stir until the viscosity of the reactant reaches 1.0×10 3 ~2.0×10 4 mPa•s / 25℃, add dithiol capping reaction for 0.5-2h to obtain component B; Component A and component B are mixed at an epoxy group / active hydrogen molar ratio of 0.95-1.2, and a tertiary amine catalyst is added, stirred evenly, and then added to obtain a formaldehyde-free quick-drying two-component polyurethane resin. The obtained formaldehyde-free quick-drying two-component polyurethane resin is used to bond the synthetic leather surface layer and the base fabric, and the final synthetic leather is obtained by baking at 130-170°C for 5-15 minutes.
8. The method for preparing a formaldehyde-free quick-drying two-component polyurethane resin according to claim 7, characterized in that: The molar ratio of the component A to the component B is 1.10 based on the epoxy group / active hydrogen.
9. The method for preparing a formaldehyde-free quick-drying two-component polyurethane resin according to claim 7, characterized in that: The addition amount of the tertiary amine catalyst is 1-5% of the mass of component A; the tertiary amine catalyst is at least one of triethylenediamine, tetramethylethylenediamine, and N,N-dimethylcyclohexylamine.