Polyisocyanate composition as well as preparation method and application thereof
By introducing a specific molar ratio of substituted biuret and substituted urea groups into polyisocyanates, the problem of high viscosity in polyisocyanate compositions is solved, resulting in polyisocyanate compositions with low viscosity and high stability, suitable for coatings and adhesives.
Patent Information
- Application Number
- CN202411297667.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-18
AI Technical Summary
Existing polyisocyanate compositions have problems such as dilution and bluish tint due to the need to add a large amount of solvent in downstream applications because of their high viscosity. Furthermore, the modification of polyols reduces the -NCO content or the diuretic structure, which affects the hardness and chemical resistance of the paint film.
By introducing substituted biuret groups and substituted urea groups into polyisocyanates and controlling their molar ratio to be greater than 0 and less than or equal to 0.5, a polyisocyanate composition with a viscosity of less than 10000 mPa·s was prepared, and its structure was optimized by aliphatic amine reaction.
This achieved a reduction in viscosity and an improvement in storage stability of the polyisocyanate composition, while maintaining good crosslinking properties and film quality.
Smart Images

Figure BDA0005046571410000021 
Figure BDA0005046571410000031 
Figure BDA0005046571410000111
Abstract
Description
Technical Field
[0001] The present invention relates to a polyisocyanate composition, in particular to a polyisocyanate composition with good storage stability. Background Art
[0002] Aliphatic / alicyclic polyisocyanates have excellent properties such as weather resistance, wear resistance, and corrosion resistance, and are widely used in coatings, adhesives, and elastomer industries. Especially in the coatings industry, the most widely used are polyisocyanate curing agents containing isocyanate groups.
[0003] Aliphatic polyisocyanate compositions containing isocyanurate groups have excellent yellowing resistance. In addition, they have the advantages of low free monomer content, saturated vapor concentration far below the occupational safety limit, high functionality, and high downstream crosslinking density.
[0004] In view of the diversity of downstream application formulation systems, curing agents often need to be used in combination with high-hydroxy resins to improve the crosslinking density, mechanical properties and chemical resistance of the paint film. However, due to the rigid structure of the isocyanurate ring itself, the polyisocyanates prepared from it often have a high viscosity. In downstream use, a large amount of solvent needs to be added to reduce the viscosity, which causes the composition to become thin and turbid, with a blue glow, etc., affecting the glossiness of the formed paint film.
[0005] The existing technology mainly reduces the viscosity of polyisocyanates by polyol modification and introduction of other structures. However, polyol modification will reduce the -NCO content of the prepared polyisocyanates; the structure of uretdione will reduce the hardness and chemical resistance of the paint film prepared by polyisocyanates compared with the isocyanurate structure. Summary of the invention
[0006] In order to overcome at least one defect of the above-mentioned prior art, in the first aspect, an embodiment of the present invention provides a polyisocyanate composition, including a plurality of diisocyanate derivatives, wherein the diisocyanate derivative is obtained by replacing at least one isocyanate group in the diisocyanate with at least one substituent group, and the at least one substituent group includes one or more of an isocyanurate group, a substituted biuret group, and a substituted urea group; the molar ratio of the substituted biuret group to the substituted urea group contained in the polyisocyanate composition is greater than 0 and less than or equal to 0.5; the viscosity of the polyisocyanate composition is less than 10000 mPa.s; the diisocyanate includes one or more of an aliphatic diisocyanate and an alicyclic diisocyanate; the viscosity is measured by a viscometer at 23°C;
[0007] Wherein, the structures of the substituted biuret group and the substituted urea group are as follows:
[0008]
[0009] R1 and R2 are each independently selected from C1 to C 12 A straight chain or branched alkyl group.
[0010] In a second aspect, an embodiment of the present invention provides a method for preparing the above-mentioned polyisocyanate composition, comprising reacting the diisocyanate and a fatty amine to obtain the polyisocyanate composition.
[0011] In a third aspect, one embodiment of the present invention provides the use of the above-mentioned polyisocyanate composition or the polyisocyanate composition prepared by the above-mentioned preparation method as a cross-linking agent or a curing agent.
[0012] The polyisocyanate composition according to one embodiment of the present invention has the characteristics of low viscosity and good storage stability. DETAILED DESCRIPTION
[0013] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions therein are essentially used as illustrations rather than to limit the present invention.
[0014] One embodiment of the present invention provides a polyisocyanate composition, including a plurality of diisocyanate derivatives, wherein the diisocyanate derivatives are obtained by replacing at least one (e.g., one or two) isocyanate groups in a diisocyanate with at least one substituent group, wherein the at least one substituent group includes one or more of an isocyanurate group, a substituted biuret group, and a substituted urea group; the molar ratio of the substituted biuret group to the substituted urea group contained in the polyisocyanate composition (or the plurality of diisocyanate derivatives) is greater than 0 and less than or equal to 0.5; the viscosity of the polyisocyanate composition is less than 10000 mPa.s; the diisocyanate includes one or more of an aliphatic diisocyanate and an alicyclic diisocyanate; the above viscosity is measured by a viscometer at 23°C;
[0015] Among them, the structures of the substituted biuret group and the substituted urea group are as follows:
[0016]
[0017] R1 and R2 are each independently selected from C1 to C 12 A straight chain or branched alkyl group.
[0018] In one embodiment, the viscosity of the polyisocyanate composition is less than 10000 mPa.s, and can further be 900 to 10000 mPa.s, for example, 920 mPa.s, 930 mPa.s, 1000 mPa.s, 2000 mPa.s, 3000 mPa.s, 40000 mPa.s, 5000 mPa.s, 5330 mPa.s, 5340 mPa.s, 5500 mPa.s, .s, 6000mPa.s, 7000mPa.s, 7460mPa.s, 7470mPa.s, 7500mPa.s, 8000mPa.s, 8500mPa.s, 8900mPa.s, 8940mPa.s, 8950mPa.s, 9000mPa.s, 9500mPa.s, 9710mPa.s, 9720mPa.s, 9800mPa.s. The above viscosity is measured at 23°C by a viscometer (e.g., BrookField DV-IPrime viscometer).
[0019] In one embodiment, the molar ratio of the substituted biuret group to the substituted urea group contained in the polyisocyanate composition (or a derivative of a plurality of diisocyanates) may be (0.05-0.50):1, and may further be (0.10-0.45):1, for example, 0.11:1, 0.15:1, 0.2:1, 0.25:1, 0.28:1, 0.3:1, 0.35:1, 0.38:1, 0.4:1, 0.44:1.
[0020] In one embodiment, the number of carbon atoms contained in R1 and R2 in the substituted biuret group and the substituted urea group can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12.
[0021] In one embodiment, R1 and R2 may be the same or different; further, R1 and R2 are each independently selected from ethyl, propyl, n-butyl, isobutyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, isooctyl, and n-nonyl.
[0022] In one embodiment, some diisocyanate derivatives include substituted groups, and other diisocyanate derivatives include isocyanate groups and substituted groups. Further, the content of isocyanate groups in the polyisocyanate composition can be 18-26wt%, such as 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, and the above mass content is based on the total mass of the polyisocyanate composition.
[0023] In one embodiment, the polyisocyanate composition includes less than 0.5wt% of diisocyanate, for example, the content of diisocyanate in the polyisocyanate composition can be 0.05wt%, 0.07wt%, 0.08wt%, 0.1wt%, 0.15wt%, 0.16wt%, 0.18wt%, 0.2wt%, 0.24wt%, 0.25wt%, 0.3wt%, or 0.4wt%.
[0024] In one embodiment, the isocyanurate group of the diisocyanate derivative is obtained by self-polymerization of three isocyanate groups.
[0025] In one embodiment, the substituted groups contained in the polyisocyanate composition include isocyanurate groups, substituted biuret groups and substituted urea groups. Further, the sum of the mass contents of the substituted biuret groups and the substituted urea groups is ≤10%, and the mass content of the isocyanurate groups can be greater than or equal to 90% and less than 100%, and the above mass content is based on the total mass of the substituted groups (i.e., the sum of the mass of the substituted biuret groups, the substituted urea groups, and the isocyanurate groups).
[0026] In one embodiment, the polyisocyanate composition is obtained by reacting a diisocyanate and a fatty amine.
[0027] In one embodiment, the structural formula of the diisocyanate is: OCN-R-NCO, wherein R is an alkylene group containing 5 to 10 (e.g., 6, 7, 8, 9, 10) carbon atoms, and the alkylene group includes an open chain alkylene group (e.g., -CH2-CH2-CH2-CH2-CH2-), a cycloalkylene group (e.g., cyclohexylene-C6H 10 -), and open chain alkylene groups including cycloalkyl substituents.
[0028] In one embodiment, the diisocyanate includes one or more of hexamethylene diisocyanate (HDI), pentamethylene diisocyanate (PDI), 2-methylpentane-1,5-diisocyanate, 2,2,4-trimethyl-1,6-hexane diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 1,4-bis(isocyanatomethyl)cyclohexane.
[0029] In one embodiment, the fatty amine may be a primary amine and / or a secondary amine, and further may be a secondary amine.
[0030] In one embodiment, the fatty amine includes 2 to 24 carbon atoms; further, the fatty amine includes 4 to 20 carbon atoms, for example, the number of carbon atoms contained in the fatty amine can be 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23.
[0031] In one embodiment, the structural formula of the fatty amine is R1-NH-R2, and the above definitions apply to R1 and R2.
[0032] In one embodiment, the fatty amine includes one or more of diethylamine, dipropylamine, di-n-butylamine, diisobutylamine, di-n-pentylamine, diisopentylamine, di-n-hexylamine, di-n-heptylamine, di-n-octylamine, diisooctylamine, and di-n-nonylamine.
[0033] One embodiment of the present invention provides a method for preparing the polyisocyanate composition, comprising reacting the diisocyanate and the fatty amine to prepare the polyisocyanate composition.
[0034] In one embodiment, the specific amounts of diisocyanate and fatty amine are based on the molar ratio of substituted biuret groups and substituted urea groups contained in the prepared polyisocyanate composition meeting the above-mentioned definition. Further, the molar ratio of amino groups (or nitrogen atoms) contained in the fatty amine to isocyanate groups contained in the diisocyanate can be greater than 0 and less than or equal to 0.06, for example, 0.01, 0.02, 0.03, 0.04, 0.05.
[0035] In one embodiment, the reaction temperature of diisocyanate and fatty amine can be 10-150°C, further can be 30-79°C, further can be 45-75°C, for example 20°C, 35°C, 40°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 90°C, 100°C, 120°C.
[0036] In one embodiment, the reaction of diisocyanate and fatty amine is carried out under the action of a catalyst, which can be one or more of quaternary ammonium hydroxide, quaternary ammonium carboxylate, aminosilyl-containing compound, tertiary amine compound, Mannich base compound, and metal salt compound.
[0037] In one embodiment, the quaternary ammonium hydroxide can be one or more of tetramethylammonium hydroxide, trimethylbenzylammonium hydroxide, tetraethylammonium hydroxide, dimethylethylcyclohexylammonium hydroxide and hydrates thereof, preferably one or more of tetramethylammonium hydroxide and trimethylbenzylammonium hydroxide and hydrates thereof.
[0038] In one embodiment, the quaternary ammonium carboxylate may be one or more of tetramethylammonium hydroxide-2-ethylhexanoate, tetramethylammonium hydroxide-octanoate, trimethylbenzylammonium hydroxide-2-ethylhexanoate, trimethylbenzylammonium hydroxide-octanoate, tetramethylammonium hydroxide-formate, tetramethylammonium hydroxide-acetate, tetramethylammonium hydroxide-pivalate, trimethylbenzylammonium hydroxide-pivalate, tetramethylammonium hydroxide-decanoate, trimethylbenzylammonium hydroxide-decanoate, tetramethylammonium hydroxide-tetradecanoate, tetramethylammonium hydroxide-tetradecanoate, tetramethylammonium hydroxide-2-ethylhexanoate, tetramethylammonium hydroxide-octanoate, trimethylbenzylammonium hydroxide-2-ethylhexanoate, and trimethylbenzylammonium hydroxide-octanoate.
[0039] In one embodiment, the compound containing an aminosilyl group may be one or more of hexamethyldisilazane, silylamine, and heptamethyldisilazane, preferably hexamethyldisilazane.
[0040] In one embodiment, the tertiary amine compound can be one or both of triethylamine and tripropylamine, preferably triethylamine.
[0041] In one embodiment, the Mannich base compound may be 2,4,6-tris(dimethylaminomethyl)phenol.
[0042] In one embodiment, the metal salt compound may be tin isooctanoate.
[0043] In one embodiment, the catalyst can be used as a pure substance or dissolved in a solvent at any concentration.
[0044] In one embodiment, the mass of the catalyst is 0.001-0.1% of the mass of the diisocyanate as the raw material, and further 0.005-0.05%, for example 0.001%, 0.005%, 0.01%, 0.02wt%, 0.03wt%, 0.04wt%, 0.06wt%, 0.08wt%.
[0045] In one embodiment, the end point of the reaction of diisocyanate and fatty amine is that the NCO% value (or the mass content of isocyanate groups) of the reaction system is 30-50%, such as 30%, 35%, 37%, 40%, 43%, 45%, 47%, 50%. When the NCO% value of the reaction system is greater than 50%, it often leads to problems such as low conversion rate, large monomer consumption, increased energy consumption required for subsequent removal of diisocyanate, and low functionality of the composition; when the NCO% value is less than 30%, the viscosity of the polyisocyanate composition is too high, which will have an adverse effect on the convenience of downstream construction and the leveling of the paint film.
[0046] The NCO% in this article is determined according to the method of GB / T 12009.4-2016, wherein NCO% refers to the mass percentage of isocyanate groups (-NCO).
[0047] In one embodiment, when the reaction system reaches the target NCO%, the polymerization reaction is terminated. The reaction can be terminated by adding a catalyst poison to the reaction system. Further, the catalyst poison can be one or more of an acidic reactive substance (e.g., protic acid), an acylating agent (e.g., isophthalic acid dichloride, benzenesulfonyl chloride).
[0048] In one embodiment, the catalyst poison is selected from one or more of protonic acid and acylating agent, for example, it can be one or more of phosphoric acid, benzoic acid, diisooctyl phosphate, dibutyl phosphate, p-toluenesulfonic acid.
[0049] In one embodiment, the catalyst poison is added in an amount sufficient to inactivate the catalyst in the system.
[0050] In one embodiment, the mixture after the reaction of diisocyanate and fatty amine can be evaporated to remove unreacted diisocyanate therein, and the residual monomer content in the polyisocyanate composition is maintained below 0.5wt%. Further, the mixture after the reaction of diisocyanate and fatty amine can be treated using a single-stage or multi-stage thin film evaporator.
[0051] One embodiment of the present invention provides the use of the above-mentioned polyisocyanate composition as a crosslinking agent or a curing agent, especially a crosslinking agent or a curing agent in a coating composition.
[0052] The polyisocyanate composition according to one embodiment of the present invention can significantly reduce the viscosity of the polyisocyanate composition while maintaining good storage stability by introducing a specific amount of substituted biuret groups and substituted urea groups into the polyisocyanate containing isocyanurate groups.
[0053] The preparation of the polyisocyanate composition according to one embodiment of the present invention is further described below in conjunction with examples. The raw materials and test methods involved in each example and comparative example are as follows.
[0054] raw material
[0055] 1. PDI: Pentamethylene diisocyanate, Wanhua Chemical Group Co., Ltd.;
[0056] 2. Dibutylamine: Aladdin Reagent Company;
[0057] 3. Dioctylamine: Aladdin Reagent Company;
[0058] 4.Tetramethylammonium hydroxide-2-ethylhexanoate: Kent Chemical Co., Ltd.;
[0059] 5. Hexamethyldisilazane: Inokite Technology Co., Ltd.
[0060] 6. Tetramethylammonium hydroxide pentahydrate: Inokai Technology Co., Ltd.;
[0061] 7.Tetraethylammonium hydroxide: Inokai Technology Co., Ltd.
[0062] 8. Acetone: Inokai Technology Co., Ltd.
[0063] Test Method
[0064] 1.-NCO content
[0065] The -NCO content was determined according to the method of GB / T 12009.4-2016.
[0066] 2. Residual diisocyanate content
[0067] According to the method of GB / T18583-2008, the residual diisocyanate content in the reaction system was determined by gas chromatography.
[0068] 3. Viscosity
[0069] Viscosity was measured at 23°C using a BrookField DV-IPrime viscometer with an S21 spindle.
[0070] 4. Content of substituted biuret groups and substituted urea groups
[0071] The content (mol%) and molar ratio (equivalent ratio) of substituted biuret groups and substituted urea groups in the polyisocyanate composition are as follows: 1 The specific test conditions are as follows:
[0072] 1 H-NMR equipment: AVANCE600 (Bruker), equipped with BBO probe (Bruker); sample concentration: 5wt%; resonance frequency: 600MHz; shift reference: 0ppm (TMS); pulse program: zg30; spectral width: 24ppm; spectral center: 6ppm.
[0073] The molar ratio of the substituted urea group to the substituted biuret group was calculated from the ratio of the integrated value near 5.7 ppm to the integrated value near 6.0 ppm.
[0074] Example 1
[0075] 850 g of PDI was added into a reaction kettle, and the temperature was raised to 50° C. under stirring under a nitrogen atmosphere. Then 12.5 g of di-n-butylamine was added into the reaction kettle and the temperature was maintained at 50° C. 0.64 g of tetraethylammonium hydroxide solution (20 wt %, acetone solution) was added dropwise into the system, and the NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 38.7%, 0.09 g of p-toluenesulfonic acid was added into the system to terminate the reaction.
[0076] The reaction liquid was separated by using a short-path evaporator (separation temperature: 150° C., pressure: 12 Pa) to remove unreacted PDI monomer, thereby obtaining a polyisocyanate composition 1.
[0077] Example 2
[0078] 850 g of PDI was added to a reaction kettle, and the temperature was raised to 55° C. under stirring under a nitrogen atmosphere. Then, 18.7 g of di-n-butylamine was added to the reaction kettle and the temperature was maintained at 55° C. 1.02 g of tetramethylammonium hydroxide-2-ethylhexanoate solution (20 wt %, n-butanol solution) was added dropwise to the system, and the NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 38.5%, 0.14 g of dibutyl phosphate was added to the system to terminate the reaction.
[0079] The reaction liquid was separated by using a short-path evaporator (separation temperature 160° C., pressure 12 Pa) to remove unreacted PDI monomer, thereby obtaining a polyisocyanate composition 2.
[0080] Example 3
[0081] 850g of PDI was added into the reactor, and the temperature was raised to 120°C under stirring under nitrogen atmosphere. Then, 10g of di-n-octylamine was added into the reactor and the temperature was maintained at 120°C. 0.8g of hexamethyldisilazane was added dropwise into the system, and the NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 39.0%, 1g of n-butanol was added into the system to terminate the reaction.
[0082] The reaction liquid was separated by using a short-path evaporator (separation temperature: 150° C., pressure: 12 Pa) to remove unreacted PDI monomer, thereby obtaining a polyisocyanate composition 3.
[0083] Example 4
[0084] 850 g of PDI was added into a reaction kettle, and the temperature was raised to 90° C. under stirring under a nitrogen atmosphere. Then 14.4 g of di-n-propylamine was added into the reaction kettle and the temperature was maintained at 90° C. 0.43 g of tetramethylammonium hydroxide pentahydrate solution (20 wt %, acetone solution) was added dropwise into the system, and the NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 48.3%, 0.03 g of phosphoric acid was added into the system to terminate the reaction.
[0085] The reaction liquid was separated by using a short-path evaporator (separation temperature 155° C., pressure 10 Pa) to remove unreacted PDI monomer, thereby obtaining a polyisocyanate composition 4.
[0086] Example 5
[0087] 850 g of PDI was added into a reactor, and the temperature was raised to 55° C. under stirring under a nitrogen atmosphere. Then, 30 g of diisopropylamine was added into the reactor and the temperature was maintained at 55° C. 0.77 g of tin isooctanoate solution (20 wt %, n-butanol solution) was added dropwise into the system, and the NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 36.4%, 0.10 g of benzenesulfonyl chloride was added into the system to terminate the reaction.
[0088] The reaction liquid was separated by using a short-path evaporator (separation temperature 155° C., pressure 10 Pa) to remove unreacted PDI monomer, thereby obtaining a polyisocyanate composition 5.
[0089] Comparative Example 1
[0090] 850 g of PDI was added into the reaction kettle, and the temperature was raised to 55° C. under stirring under a nitrogen atmosphere. Then 1.02 g of tetramethylammonium hydroxide-2-ethylhexanoate solution (20 wt %, n-butanol solution) was added dropwise into the system. The NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 38.5%, 0.14 g of dibutyl phosphate was added into the system to terminate the reaction.
[0091] The reaction liquid was separated by a short-path evaporator (separation temperature 160° C., pressure 12 Pa) to remove unreacted PDI monomers, thereby obtaining a polyisocyanate composition A.
[0092] Comparative Example 2
[0093] 850 g of PDI was added into a reaction kettle, and the temperature was raised to 100° C. with stirring under a nitrogen atmosphere. Then, 18.7 g of di-n-butylamine was added into the reaction kettle, and 1.02 g of tetramethylammonium hydroxide-2-ethylhexanoate solution (20 wt %, n-butanol solution) was added dropwise into the system while maintaining the temperature at 100° C. The NCO% of the reaction solution was tracked and measured. When the NCO% value dropped to 36.5%, 0.14 g of dibutyl phosphate was added into the system to terminate the reaction.
[0094] The reaction liquid was separated by a short-path evaporator (separation temperature 160° C., pressure 12 Pa) to remove unreacted PDI monomer, thereby obtaining a polyisocyanate composition B.
[0095] Comparative Example 3
[0096] 850 g of PDI was added to the reactor, stirred and heated to 40°C under a nitrogen atmosphere, and then 0.42 g of tri(dimethylamino)phosphine was added to the reactor. After reacting for 1 hour, 4.9 wt% of pivalic acid based on PDI was added, the temperature was raised to 110°C, 7.2 g of water was slowly added, and the reaction was stirred for 2 hours.
[0097] The reaction liquid was separated by a short-path evaporator (separation temperature 160° C., pressure 12 Pa) to remove unreacted PDI monomers, thereby obtaining a polyisocyanate composition C.
[0098] The polyisocyanate compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were subjected to relevant tests according to the aforementioned methods. The results are shown in Table 1.
[0099] Table 1 Performance results of the polyisocyanate compositions of various embodiments and comparative examples
[0100]
[0101]
[0102] According to the results in Table 1, the molar ratio of the substituted biuret group to the substituted urea group of the polyisocyanate compositions of Examples 1 to 5 is greater than 0 and less than or equal to 0.5, the corresponding molar ratios of Comparative Examples 1 and 3 are 0, and the corresponding molar ratio of Comparative Example 2 is 0.55, which is greater than 0.5. According to the viscosity values of the polyisocyanate compositions, the viscosity of the polyisocyanate compositions of Examples 1 to 5 is less than that of Comparative Examples 1 to 3. Therefore, by limiting the molar ratio of the substituted biuret group to the substituted urea group of the polyisocyanate composition to greater than 0 and less than or equal to 0.5, its viscosity can be greatly reduced.
[0103] The polyisocyanate compositions of Examples 1 to 5 and Comparative Examples 1 to 3 were stored at 50° C. for 3 months and tested for viscosity change and diisocyanate content. The results are shown in Table 2.
[0104] Table 2 Viscosity index of polyisocyanate compositions of various embodiments and comparative examples
[0105]
[0106] According to the results in Table 2, after storage for 3 months, the viscosity of the polyisocyanate compositions of Examples 1 to 5 changed little, and the free diisocyanate content was low, indicating that they had good storage stability. In addition, since the composition of Comparative Example 3 contained a certain amount of uretdione, it would decompose into diisocyanate during the heating and storage process, resulting in a diisocyanate content of >0.5%.
[0107] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.
[0108] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.
Claims
1. A polyisocyanate composition, comprising a plurality of diisocyanate derivatives, wherein the diisocyanate derivatives are obtained by replacing at least one isocyanate group in the diisocyanate with at least one substituent group, wherein the at least one substituent group comprises one or more of an isocyanurate group, a substituted biuret group, and a substituted urea group; the molar ratio of the substituted biuret group to the substituted urea group in the polyisocyanate composition is greater than 0 and less than or equal to 0.5; the viscosity of the polyisocyanate composition is less than 10000 mPa.s; the diisocyanate comprises one or more of an aliphatic diisocyanate and an alicyclic diisocyanate; and the viscosity is measured by a viscometer at 23°C; in, The structures of the substituted biuret group and the substituted urea group are as follows: R1 and R2 are each independently selected from C1 to C 12 A straight chain or branched alkyl group.
2. The composition according to claim 1, wherein The molar ratio of the substituted biuret group to the substituted urea group contained in the polyisocyanate composition is (0.05-0.50):1; and / or, The viscosity of the polyisocyanate composition is 900 to 10000 mPa.s; and / or, The polyisocyanate composition comprises less than 0.5 wt % of the diisocyanate; and / or, R1 and R2 are the same or different; and / or, The polyisocyanate composition is obtained by reacting the diisocyanate and aliphatic amine, and the structural formula of the aliphatic amine is R1-NH-R2.
3. The composition according to claim 1, wherein R1 and R2 are each independently selected from one or more of ethyl, propyl, n-butyl, isobutyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, isooctyl and n-nonyl; and / or, R1 and R2 are each independently selected from a C1-C8 straight chain or branched alkyl group; and / or, The structural formula of the diisocyanate is: OCN-R-NCO, wherein R is an alkylene group containing 5 to 10 carbon atoms; and / or, The substituted groups contained in the polyisocyanate composition include the isocyanurate group, the substituted biuret group and the substituted urea group. Based on the total mass of the substituted groups, the sum of the mass contents of the substituted biuret group and the substituted urea group is less than or equal to 10%.
4. The composition according to claim 1, wherein The molar ratio of the substituted biuret group to the substituted urea group contained in the polyisocyanate composition is (0.10-0.45):1; and / or, The polyisocyanate composition comprises 18 to 26 wt % of isocyanate groups; and / or, The diisocyanate includes one or more of hexamethylene diisocyanate, pentamethylene diisocyanate, 2-methylpentane-1,5-diisocyanate, 2,4,4-trimethyl-1,6-hexane diisocyanate, 2,2,4-trimethyl-1,6-hexane diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane and 1,4-bis(isocyanatomethyl)cyclohexane.
5. The method for preparing the polyisocyanate composition according to any one of claims 1 to 4, comprising reacting the diisocyanate and aliphatic amine to obtain the polyisocyanate composition.
6. The preparation method according to claim 5, wherein: The molar ratio of the amino group contained in the fatty amine to the isocyanate group contained in the diisocyanate is greater than 0 and less than or equal to 0.06; and / or, The reaction end point of the reaction is when the isocyanate group content of the reaction system is 30 to 50 wt %.
7. The preparation method according to claim 5, wherein: The fatty amine comprises 2 to 24 carbon atoms; and / or, The fatty amine is a primary amine and / or a secondary amine; and / or, The reaction temperature is 10 to 150° C.; and / or, The reaction is carried out under the action of a catalyst, and the catalyst includes one or more of quaternary ammonium hydroxides, quaternary ammonium carboxylates, compounds containing aminosilyl groups, tertiary amine compounds, Mannich base compounds, and metal salt compounds.
8. The preparation method according to claim 7, wherein: The fatty amine comprises 4 to 20 carbon atoms; and / or, The reaction temperature is 30-79°C; and / or, The mass of the catalyst is 0.001 to 0.1% of the mass of the diisocyanate.
9. The preparation method according to claim 7, wherein: The fatty amine includes one or more of diethylamine, dipropylamine, di-n-butylamine, diisobutylamine, di-n-pentylamine, diisopentylamine, di-n-hexylamine, di-n-heptylamine, di-n-octylamine, diisooctylamine, and di-n-nonylamine; and / or, The reaction temperature is 45-75°C; and / or, The mass of the catalyst is 0.005-0.05% of the mass of the diisocyanate.
10. Use of the polyisocyanate composition according to any one of claims 1 to 4 or the polyisocyanate composition prepared by the preparation method according to any one of claims 5 to 9 as a crosslinking agent or curing agent.
Citation Information
Patent Citations
Polyisocyanate composition as well as preparation method and application thereof
CN113698572A
Biuretized polyisocyanates and blocked biuretized polyisocyanates
CN1762987A
Stable liquid biuret modified and biuret allophanate modified diphenylmethane diisocyanates, prepolymers thereof, and processes for their preparation
US20050020795A1
Solidification-stable blocked polyisocyanates
US20050070683A1
Biuretized isocyanates and blocked biuretized isocyanates
US20060089480A1