Soluble polyarylene ether nitrile resin material as well as preparation method and application thereof
By developing soluble polyarylethernitrile resin materials, the difficulty of polyaryletherketones in processing and application is solved, the soluble and easy processability of the material is realized, the binding force with fiber is enhanced, and it is suitable for a variety of high performance application.
Patent Information
- Application Number
- CN202411158794.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
Smart Images

Figure CN119019674A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials, and in particular relates to a soluble polyarylethernitrile resin material and a preparation method and application thereof. Background Art
[0002] Structural adhesives are adhesives that can transfer large dynamic and static loads for structural connection at a certain application temperature. Because of their high strength and high durability, they are important structural bonding materials in the manufacture of high-temperature load-bearing structural parts of aerospace vehicles. Therefore, they are widely used in high-tech fields such as aviation and aerospace, and are an irreplaceable type of connection material. In recent years, due to the rapid development of aviation, aerospace and space technology, organic high-temperature resistant adhesives have been used more and more widely, especially thermosetting structural adhesive films that do not release small molecules during the curing process and can be used for paving processes. More and more attention and research have been paid to typical foreign products such as Hexcel's Redux319 and Cytee's FM-300 epoxy film; Cytec's FM2550, Hexcel's Redux326 and Henkel's Hysol EA9673 double-male adhesive film, all of which have the above advantages.
[0003] Polyaryletherketone (PEEK) is a crystalline high-performance special engineering plastic with excellent high temperature resistance, self-lubrication, corrosion resistance, flame retardancy, mechanical properties, electrical properties, hydrolysis resistance, weather resistance, etc. Since PEEK has extremely excellent comprehensive physical, mechanical, electrical, thermal, and chemical properties, it can be made into various parts by traditional thermoplastic molding methods such as injection, extrusion, molding, coating, and mechanical cutting. It has received extensive attention and attention from sample designers, molding processing companies, and product manufacturing suppliers. Therefore, PEEK has been widely used in the fields of petrochemicals, transportation, electronics and electrical, medical and health, food processing, aerospace, etc.
[0004] PEEK has a dense molecular structure and high crystallinity. It cannot be directly used as a base material for equipment seals, non-metallic hoses, coatings and adhesives for the following reasons: First, PEEK has extremely high chemical stability. Except for concentrated sulfuric acid, it is insoluble in any solvents and strong acids and alkalis. Therefore, coatings and adhesives cannot be prepared by the solvent method; second, the melting temperature (Tm) of PEEK is as high as 330°C, and the molding temperature exceeds 370°C, making the processing and molding of downstream structural parts difficult; third, traditional PEEK and substrates are not easy to combine, which makes it easy for defects such as lack of glue and pores to exist in composite components. Summary of the invention
[0005] Purpose of the invention: In view of the problems existing in the prior art, the present invention aims to provide a soluble polyarylethernitrile resin material.
[0006] The invention also provides a preparation method and application of the soluble polyarylethernitrile resin material.
[0007] Technical solution: In order to achieve the above-mentioned purpose, the present invention provides a soluble polyarylether nitrile resin material, and the structural formula of the soluble polyarylether nitrile resin material is as follows:
[0008]
[0009] Wherein R1 is a chiral structure monomer and a cyclic plane twisted monomer;
[0010] R2 is an aromatic structure or a straight chain structure.
[0011] Furthermore, the chiral monomer is isosorbide, and the cyclic plane-distorted monomer is 1,4-cyclohexanedimethanol.
[0012] Furthermore, the molecular structure of the 1,4-cyclohexanedimethanol is as follows:
[0013]
[0014] Furthermore, the R2 is an aromatic structure or a 2-4 membered carbon chain.
[0015] Preferably, the R2 is 2'6-difluorobenzonitrile.
[0016] The method for preparing the soluble poly(arylene ether nitrile) resin material of the present invention comprises the following steps:
[0017] (1) adding isosorbide, 1,4-cyclohexanedimethanol, hydroquinone, 4'4-difluorobenzophenone, 2'6-difluorobenzonitrile, sodium hydroxide and sulfolane into a flask respectively, mixing them, and then performing a salt-forming reaction in the dark under an inert gas;
[0018] (2) adding K2CO3 to carry out light-protected reaction, and after the reaction is completed, pouring the mixture into water and stirring to obtain crude poly(arylene ether nitrile) particles, crushing the crude particles, washing them, and drying them to obtain a poly(arylene ether nitrile) resin material.
[0019] Preferably, the preparation method of the soluble poly(arylether nitrile) resin material adopts a "one-pot two-step" synthesis: under continuous argon gas conditions, isosorbide, 1,4-cyclohexanedimethanol, hydroquinone, 4'4-difluorobenzophenone, 2'6-difluorobenzonitrile are added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then sodium hydroxide and cyclopentane sulfone are added. Under light-proof conditions, the salt-forming reaction is carried out at 150-180°C for 4-5 hours; after the salt-forming reaction is completed, a certain mass of K2CO3 is added, the temperature is programmed to 240-260°C, the reaction is carried out for a certain period of time, and the material is discharged, and washed with ethanol and deionized water to obtain a white poly(arylether nitrile) resin material.
[0020] Furthermore, the total mole number of isosorbide, 1,4-cyclohexanedimethanol and hydroquinone in step (1) is equal to the total mole number of 4'4-difluorobenzophenone and 2'6-difluorobenzonitrile.
[0021] Furthermore, in step (1), the molar ratio of isosorbide to 1,4-cyclohexanedimethanol is preferably 1:1, and the molar ratio of 2'6-difluorobenzonitrile to 4'4-difluorobenzophenone is preferably 2:8.
[0022] Furthermore, the molar ratio of (isosorbide + 1,4-cyclohexanedimethanol) to hydroquinone in step (1) is 1:(1-4);
[0023] Furthermore, the amount of sodium hydroxide used in step (1) is twice the total mole number of isosorbide, 1,4-cyclohexanedimethanol and hydroquinone (or the total mole number of 4'4-difluorobenzophenone and 2'6-difluorobenzonitrile).
[0024] Furthermore, the salt-forming reaction temperature in step (1) is 150-180° C., and the reaction time is 4-5 hours. The light-shielding reaction temperature in step (2) is 240-260° C., and the reaction time is 0.5-1 hour.
[0025] The soluble polyarylethernitrile resin material of the present invention is used in aerospace, petrochemical industry, transportation, and electronic and electrical fields.
[0026] Preferably, the soluble polyarylethernitrile resin material is used as an adhesive in aerospace, petrochemical, transportation, and electronic and electrical applications.
[0027] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0028] 1. The introduction of chiral structure monomers (isosorbide) and cyclic plane distortion monomers (1,4-cyclohexanedimethanol) in the material of the present invention and their combined use can cause the plane of the polyarylethernitrile polymer to be distorted, greatly reducing the crystallinity and melting point of the polymer and reducing the processing difficulty; the polymer can be dissolved in many common solvents and is easier to process by film forming, spinning, extrusion, etc.; the polyarylethernitrile material of the present invention is a linear block copolymer containing a hard segment with a dense aromatic structure and a polyether soft segment, which has both the excellent elasticity of rubber and the easy processability of thermoplastics, and has adjustable hardness and hardness and free design, and is a new thermoplastic elastomer.
[0029] 2. The present invention adopts a "one-pot two-step" preparation method to effectively regulate the types and quantities of polar groups in the polyarylethernitrile polymer, making the polymer easier to combine with carbon fiber, glass fiber, glass, steel plate, etc., to form a strong large component with strong intermolecular forces such as hydrogen bonds and van der Waals forces; the prepared polyarylethernitrile polymer material can not only effectively resist ultraviolet radiation, but also has good resistance to acids and alkalis. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the infrared spectrum of the polyarylethernitrile product of Example 2;
[0031] Figure 2 The deuterated DMSO phase of the poly(arylether nitrile) product of Example 2 1 H-NMR spectrum. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0033] The experimental methods used in the present invention are conventional methods unless otherwise specified. The materials, reagents, etc. used in the experiments can be obtained from commercial sources unless otherwise specified. All the following reagents used in the examples are commercially available analytically pure or chemically pure.
[0034] In the embodiment of the present invention, R1 is a combination of isosorbide and 1,4-cyclohexanedimethanol (CHDM), and R2 is 2'6-difluorobenzonitrile.
[0035] Example 1
[0036] Under the condition of continuous high-purity argon, 1.09 g of isosorbide, 1.08 g of 1,4-cyclohexanedimethanol (CHDM), 6.61 g of hydroquinone, 13.10 g of 4'4-difluorobenzophenone, and 2.09 g of 2'6-difluorobenzonitrile were added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then 6 g of sodium hydroxide and 85 g of cyclopentane sulfone were added. The salt-forming reaction was carried out at 175° C. for 5 hours under light-proof conditions. After the salt-forming reaction was completed, 1.6 g of K2CO3 was added, the temperature was programmed to 260° C., and the reaction was continued in the dark for 1 hour, then the reactant was quickly poured into deionized water and stirred continuously, and the crude particles of polyarylethernitrile were obtained by filtration.
[0037] The crude poly(arylene ether nitrile) particles were crushed, washed repeatedly with ethanol and deionized water for 6 times, and dried to obtain a white poly(arylene ether nitrile) resin material.
[0038] Example 2
[0039] Under the condition of continuous high-purity argon, 1.64 g of isosorbide, 1.62 g of CHDM, 5.78 g of hydroquinone, 13.10 g of 4'4-difluorobenzophenone, and 2.09 g of 2'6-difluorobenzonitrile were added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then 6 g of sodium hydroxide and 85 g of cyclopentane sulfone were added. Under the condition of avoiding light, the salt-forming reaction was carried out at 175° C. for 5 hours. After the salt-forming reaction was completed, 1.6 g of K2CO3 was added, the temperature was raised to 260° C., and the reaction was continued in the dark for 1 hour, and then the reactant was quickly poured into deionized water and stirred continuously to obtain crude polyarylethernitrile particles.
[0040] The crude poly(arylether nitrile) particles were crushed, washed repeatedly with ethanol and deionized water for 6 times, and dried to obtain a white poly(arylether nitrile) product. Figure 1 As shown, the product was characterized by infrared spectroscopy, and the results are shown in the following figure: -1 It is the characteristic peak of C=N in polymer; 1234cm -1 Characteristic peak of aliphatic aromatic ether COC; 839cm -1 It is the characteristic peak of para-substituted benzene ring =CH. Figure 2 As shown, the deuterated DMSO phase of the sample 1 H-NMR spectrum characterization, the results are shown in the figure below: in the figure, 3.95-4.04ppm is the H peak of the methylene proton of the synthetic monomer of isosorbide in the polymer, 4.37-5.08ppm is the H peak of the methine proton of the synthetic monomer of isosorbide in the polymer, and 6.51-7.70ppm is the H peak of the proton on the benzene ring in the polymer.
[0041] Example 3
[0042] Under the condition of continuous high-purity argon, 2.19 g of isosorbide, 2.16 g of CHDM, 4.95 g of hydroquinone, 13.10 g of 4'4-difluorobenzophenone, and 2.09 g of 2'6-difluorobenzonitrile were added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then 6 g of sodium hydroxide and 85 g of cyclopentane sulfone were added. Under the condition of avoiding light, the salt-forming reaction was carried out at 175° C. for 5 hours. After the salt-forming reaction was completed, 1.6 g of K2CO3 was added, the temperature was programmed to 260° C., and the reaction was continued in the dark for 1 hour, and then the reactant was quickly poured into deionized water and stirred continuously to obtain crude polyarylethernitrile particles.
[0043] The crude poly(arylene ether nitrile) particles were crushed, washed repeatedly with ethanol and deionized water for 6 times respectively, and dried to obtain a white poly(arylene ether nitrile) product.
[0044] Example 4
[0045] Under the condition of continuous high-purity argon, 2.74 g of isosorbide, 2.70 g of CHDM, 4.13 g of hydroquinone, 13.10 g of 4'4-difluorobenzophenone, and 2.09 g of 2'6-difluorobenzonitrile were added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then 6 g of sodium hydroxide and 85 g of cyclopentane sulfone were added. Under the condition of avoiding light, the salt-forming reaction was carried out at 175° C. for 5 hours. After the salt-forming reaction was completed, 1.6 g of K2CO3 was added, the temperature was programmed to 260° C., and the reaction was continued in the dark for 1 hour, and then the reactant was quickly poured into deionized water and stirred continuously to obtain crude polyarylethernitrile particles.
[0046] The crude poly(arylene ether nitrile) particles were crushed, washed repeatedly with ethanol and deionized water for 6 times respectively, and dried to obtain a white poly(arylene ether nitrile) product.
[0047] Comparative Example 1
[0048] Under the condition of continuous high-purity argon, 3.29 g of isosorbide, 5.78 g of hydroquinone, 13.10 g of 4'4-difluorobenzophenone, and 2.09 g of 2'6-difluorobenzonitrile were added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then 6 g of sodium hydroxide and 85 g of cyclopentane sulfone were added. Under the condition of avoiding light, the salt-forming reaction was carried out at 175° C. for 5 hours. After the salt-forming reaction was completed, 1.6 g of K2CO3 was added, the temperature was programmed to 260° C., and the reaction was continued in the dark for 1 hour, and then the reactant was quickly poured into deionized water and stirred continuously to obtain crude polyarylethernitrile particles.
[0049] The crude poly(arylene ether nitrile) particles were crushed, washed repeatedly with ethanol and deionized water for 6 times respectively, and dried to obtain a white poly(arylene ether nitrile) product.
[0050] Comparative Example 2
[0051] Under the condition of continuous high-purity argon, 3.24 g CHDM, 5.78 g hydroquinone, 13.10 g 4'4-difluorobenzophenone, 2.09 g 2'6-difluorobenzonitrile were added to a round-bottom flask equipped with a mechanical stirrer and a condenser, and then 6 g sodium hydroxide and 85 g sulfolane were added. The salt-forming reaction was carried out at 175° C. for 5 hours under the condition of avoiding light. After the salt-forming reaction was completed, 1.6 g K2CO3 was added, the temperature was raised to 260° C., and the reaction was continued for 1 hour in the dark, then the reactant was quickly poured into deionized water and stirred continuously to obtain crude polyarylethernitrile particles.
[0052] The crude poly(arylene ether nitrile) particles were crushed, washed repeatedly with ethanol and deionized water for 6 times respectively, and dried to obtain a white poly(arylene ether nitrile) product.
[0053] The intrinsic viscosity and solubility of the poly(arylene ether nitrile) resin materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were tested.
[0054] Intrinsic viscosity [η] test: Weigh 0.125 g of the prepared sample respectively, prepare 25 mL of 0.5% NMP solution and measure it by four-point method in Ubbelohde viscometer at 25°C±0.5°C.
[0055] Table 1. Intrinsic viscosity of poly(arylene ether nitrile)
[0056] sample Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 η(dL / g) 1.41 1.36 1.29 1.21 1.30 1.31
[0057] As can be seen from Table 1, all samples have a relatively high intrinsic viscosity, ranging from 1.21 to 1.41. The intrinsic viscosity of the poly(arylether nitrile) is related to the activity and chemical structure of the reactants. The rigid structure of raw materials such as hydroquinone leads to a relatively high intrinsic viscosity of the obtained poly(arylether nitrile). However, compared with Example 2 and Comparative Examples 1-2, with the simultaneous addition of isosorbide and CHDM, the intrinsic viscosity of the poly(arylether nitrile) has increased significantly compared with the single addition of an equal amount of isosorbide or CHDM. The intrinsic viscosity of Comparative Examples 1 and 2 is basically the same, indicating that the activity is basically the same regardless of whether isosorbide or CHDM participates in the reaction. At the same time, the specific raw material ratio in the formulation system of the present invention also has a significant effect on the intrinsic viscosity of the poly(arylether nitrile). It can be seen from Table 1 that the intrinsic viscosity of Example 1 is significantly better than that of Examples 3 and 4.
[0058] The solubility of poly(arylene ether nitrile) in NMP and other common solvents is listed in Table 2.
[0059] Table 2. Solubility of poly(arylene ether nitrile)
[0060] sample NMP DMAc DMSO Resorcinol Chloroform Ethylene dichloride Toluene Example 1 ++ ++ + + +- +- +- Example 2 ++ ++ ++ ++ + + +- Example 3 ++ ++ ++ ++ + + +- Example 4 ++ ++ ++ ++ ++ + + Comparative Example 1 ++ ++ ++ +- +- +- +- Comparative Example 2 ++ ++ + +- +- +- +-
[0061] Note: ++ means easily soluble; + means soluble; +- means partially soluble; - means insoluble
[0062] As can be seen from Table 2, the solubility of the poly(arylether nitrile) added with isosorbide and CHDM is greatly improved. It is not only easily soluble in aprotic polar solvents, but also has a certain solubility in medium polar solvents. The reason may be that the ether bond is introduced into the main chain of the macromolecule, which increases the flexibility of the chain. The polymers of Comparative Example 1 (without CHDM) and Comparative Example 2 (without isosorbide) have certain solubility, but the solubility of both is worse than that of Examples 1 to 4, indicating that the chiral structure of the isosorbide molecule and the planar twisted structure of the CHDM molecule work together to significantly improve the solubility of the polymer.
[0063] The poly(arylether nitrile) polymer was dissolved in ethylene dichloride solvent, and the aramid fabric was impregnated. The laminate was made in a molding machine, and the shear strength was tested using D2344 / D2344M. The experiments were conducted three times in parallel, and the average values of the data are listed in Table 3.
[0064] Table 3. Shear strength of poly(arylene ether nitrile aramid) laminates
[0065] sample Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 <![CDATA[τ sbs (MPa)]]> 39.5 47.3 40.6 35.1 34.0 31.9
[0066] As can be seen from Table 3, the shear strength of the laminate made of Example 2 as an adhesive is the largest, indicating that it has the best adhesive performance in the composite material. Comparison of the shear strength data of Example 2 with Comparative Examples 1 and 2 shows that when CHDM or isosorbide alone is used to react with hydroquinone, 4'4-difluorobenzophenone, and 2'6-difluorobenzonitrile to prepare polymers, the shear strength of the laminate made of these polymers and aramid fibers is significantly reduced compared with the laminate made of Example 2, indicating that the cyclic planar twisted structure of CHDM and the chiral structure of isosorbide can greatly improve the adhesive performance of the polymer after synergy, making it widely and important in polymer-based composite materials.
Claims
1. A soluble polyarylethernitrile resin material, characterized in that: The structural formula of the soluble polyarylethernitrile resin is as shown below: Wherein R1 is a chiral structure monomer and a cyclic plane twisted monomer; R2 is an aromatic structure or a straight chain structure.
2. The soluble polyarylethernitrile resin material according to claim 1, characterized in that: The chiral monomer is isosorbide, and the cyclic plane-distorted monomer is 1,4-cyclohexanedimethanol.
3. The soluble polyarylethernitrile resin material according to claim 1, characterized in that: The R2 is an aromatic benzene ring or a 2-4 membered carbon chain.
4. The soluble polyarylethernitrile resin material according to claim 1, characterized in that: The R2 is 2'6-difluorobenzonitrile.
5. A method for preparing the soluble poly(arylene ether nitrile) resin material according to claim 1, characterized in that: The steps include: (1) mixing isosorbide, 1,4-cyclohexanedimethanol, hydroquinone, 4'4-difluorobenzophenone, 2'6-difluorobenzonitrile, sodium hydroxide and sulfolane, and performing a salt-forming reaction in the absence of light under an inert gas; (2) adding K2CO3 to carry out light-protected reaction; after the reaction is completed, pouring the mixture into water and stirring to obtain crude poly(arylene ether nitrile) particles; crushing the crude particles, washing them, and drying them to obtain a poly(arylene ether nitrile) resin material.
6. The method for preparing the soluble poly(arylene ether nitrile) resin material according to claim 5, characterized in that: The total mole number of isosorbide, 1,4-cyclohexanedimethanol and hydroquinone in step (1) is equal to the total mole number of 4'4-difluorobenzophenone and 2'6-difluorobenzonitrile.
7. The method for preparing the soluble poly(arylene ether nitrile) resin material according to claim 5, characterized in that: In step (1), the molar ratio of isosorbide to 1,4-cyclohexanedimethanol is preferably 1:1, and the molar ratio of 2'6-difluorobenzonitrile to 4'4-difluorobenzophenone is preferably 2:
8.
8. The method for preparing the soluble poly(arylene ether nitrile) resin material according to claim 5, characterized in that: The amount of sodium hydroxide used in step (1) is twice the total molar number of isosorbide, 1,4-cyclohexanedimethanol and hydroquinone.
9. The method for preparing the soluble polyarylethernitrile resin material according to claim 5, characterized in that: The salt-forming reaction temperature in step (1) is 150-180° C., and the reaction time is 4-5 hours. The light-shielding reaction temperature in step (2) is 240-260° C., and the reaction time is 0.5-1 hour.
10. Use of the soluble polyarylethernitrile resin material according to claim 1 in aerospace, petrochemical, transportation, and electronic and electrical industries.