Tear-resistant light extremely-elastic insole, preparation method thereof and shoe

By adding components such as high-elastic a-olefin elastomer and ethylene-vinyl acetate copolymer to the midsole, combined with supercritical foaming and hot pressing shaping processes, the lack of rebound and tear resistance of traditional midsole is solved. The problem is that it achieves a lightweight, high rebound and tear-resistant midsole material, extending the service life of sports shoes.

CN119019819APending Publication Date: 2024-11-26SHANGHAI ANTA SPORTING GOODS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310600058.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The traditional EVA-based chemical foam midsole cannot resilience exceed 65% while meeting the lightweight, which cannot meet consumers' high requirements for the weight and resilience of sports shoes. At the same time, the lack of tear resistance performance leads to the shoes. Short service life.

Method used

Using thermoplastic polyester elastomer or polyether block polyamide elastomer as the basis, add a-olefin elastomer with high elasticity and low density, and shaping through supercritical foaming and hot pressing, combining ethylene-ethylene acetate Components such as copolymers, zinc oxide and peroxide crosslinking agents form a lightweight and extremely elastic midsole that enhances the tear and rebound properties of the midsole.

Benefits of technology

It achieves the light weight, good rebound performance and tear resistance of the midsole, extends the service life of the sneakers, and avoids the defects of conventional supercritical foaming processes that reduce tear resistance. It is also environmentally friendly and has scraps. Reusable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a tear-resistant light extremely-elastic insole, a preparation method thereof and a shoe. The insole comprises the following components in parts by mass: 60-80 parts of a thermoplastic elastomer, 10-40 parts of an alpha-olefin elastomer, 10-40 parts of an ethylene-vinyl acetate copolymer, 1-2 parts of zinc oxide, 0.5-1 part of a peroxide crosslinking agent, 0.5-1 part of stearic acid and 1-2 parts of titanium dioxide. Wherein the thermoplastic elastomer is a thermoplastic polyester elastomer or a polyether block polyamide elastomer, and the melting point range of the thermoplastic elastomer is 150-175 DEG C; the melting point range of the alpha-olefin elastomer is 50-125 DEG C; the insole can meet the requirements for light weight and good rebound resilience, meanwhile, the tear resistance of the insole is guaranteed, and the service life of a shoe is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of midsole materials, and in particular to a tear-resistant, lightweight and extremely elastic midsole and a preparation method thereof, and shoes. Background Art

[0002] In recent years, more and more people have participated in various sports, and the requirements for sports shoes have become higher and higher. Among them, consumers have higher and higher requirements for the weight and resilience of sports shoes. Lightweight and high-elastic sports shoes are loved by more and more consumers. Among the many components of sports shoes, the midsole is the core that determines the weight and resilience of sports shoes. Although the traditional EVA-based chemical foaming material midsole can achieve a density of less than 0.16g / cm 3 The lightweight, but the rebound performance usually cannot exceed 65%, and the rebound performance cannot meet the needs of consumers. Summary of the invention

[0003] The purpose of the present invention is to overcome the above-mentioned defects or problems existing in the background technology, and to provide a tear-resistant, lightweight and extremely elastic midsole and its preparation method, and shoes, which can ensure the tear resistance of the midsole while meeting the requirements of light weight and good rebound performance, thereby improving the service life of the shoes.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] A tear-resistant, lightweight and extremely elastic midsole comprises the following components in parts by mass: 60-80 parts of a thermoplastic elastomer, 10-40 parts of an α-olefin elastomer, 10-40 parts of an ethylene-vinyl acetate copolymer, 1-2 parts of zinc oxide, 0.5-1 part of a peroxide crosslinking agent, 0.5-1 part of stearic acid, and 1-2 parts of titanium dioxide; wherein the thermoplastic elastomer is a thermoplastic polyester elastomer or a polyether block polyamide elastomer, and its melting point ranges from 150 to 175° C.; and the melting point range of the α-olefin elastomer is from 50 to 125° C.

[0006] The tear-resistant, lightweight and extremely elastic midsole provided by the present invention adopts a thermoplastic polyester elastomer or a polyether block polyamide elastomer as a base, and adds an α-olefin elastomer thereto. The α-olefin elastomer has a certain degree of crystallinity, a relatively narrow relative molecular weight, and a relatively low density. It has high elasticity, high elongation, good impact strength, good low temperature resistance and processing rheology. The saturated structure of its main chain makes it superior to traditional elastomers in terms of heat aging resistance and UV resistance. The good mobility can improve the dispersion effect of the filler. After it is added to the thermoplastic polyester elastomer or the polyether block polyamide elastomer, it can be dispersed to the thermoplastic elastomer under the action of an auxiliary agent. In the elastomer, it plays the role of bonding the thermoplastic elastomer, thereby enhancing the tear resistance of the midsole, and the low density of the α-olefin elastomer can ensure that the weight of the midsole can meet the requirements, and it has high compatibility with the thermoplastic polyester elastomer or the polyether block polyamide elastomer, which can enhance the rebound performance of the midsole; wherein, the thermoplastic elastomer with a melting point range of 150-175°C and the α-olefin elastomer with a melting point range of 50-125°C are selected, which can ensure that the two are fully mixed during the preparation process, so that the prepared midsole has excellent tear resistance, light weight and good rebound performance.

[0007] Furthermore, in the ethylene-vinyl acetate copolymer, the content of vinyl acetate is in the range of 10-40wt%.

[0008] In this technical solution, the ethylene-vinyl acetate copolymer includes a vinyl acetate component, which can enhance the elasticity of the midsole material. An appropriate range of the mass proportion of vinyl acetate can ensure that the midsole has good rebound performance while avoiding the mutual influence between it and the α-olefin elastomer, which leads to a decrease in the tear resistance of the midsole.

[0009] Furthermore, the zinc content in the zinc oxide is higher than 95wt%.

[0010] Furthermore, the peroxide cross-linking agent is selected from one or more of dicumyl peroxide and 1,4-di-tert-butyl peroxycumene.

[0011] In addition, the present invention also provides a method for preparing a tear-resistant, lightweight and extremely elastic midsole, which is prepared according to the ratio of the above-mentioned tear-resistant, lightweight and extremely elastic midsole by the following steps: step 1, weighing each raw material according to the mass proportion, and granulating after mixing to obtain a seed material; step 2, heating and melting the seed material and then injecting it into a first mold to obtain a small embryo to be foamed; step 3, foaming the small embryo by a supercritical foaming process to obtain a foaming mold embryo; step 4, after the foaming mold embryo is cooled, placing it into a second mold and hot pressing and cooling to shape it to obtain the tear-resistant, lightweight and extremely elastic midsole.

[0012] The present invention provides a method for preparing a tear-resistant, lightweight and extremely elastic midsole, which adopts a supercritical foaming process to foam a small embryo to be foamed, and the foamed embryo mold obtained after foaming is cooled and then subjected to hot pressing and cooling to obtain the tear-resistant, lightweight and extremely elastic midsole. Since the supercritical foaming process is adopted, there is no need to add a foaming agent or other auxiliary agents during the preparation of the midsole, and since gas infiltrates into the interior of the midsole during the foaming process, more cavities can be formed inside the midsole, so that the midsole has a lower density and higher resilience. However, at the same time, the conventional supercritical foaming process will reduce the tear resistance of the midsole. The present invention adds an a-olefin elastomer to the preparation components, so that the prepared midsole can maintain a higher tear resistance. In addition, since the midsole is shaped by hot pressing after foaming, compared with the thermosetting process, the scraps in the preparation process and the midsole after use can be reused, which is more environmentally friendly.

[0013] Furthermore, in step one, a twin-screw machine is used for granulation, and the temperatures of the first, second, third and fourth zones of the twin-screw machine are 185-195°C, 180-190°C, 175-185°C and 170-180°C respectively, and the screw speed is 15-20rpm.

[0014] In this technical solution, the temperature of each zone of the twin-screw machine is limited to match the melting point range of the selected thermoplastic elastomer and α-olefin elastomer, so that the mixing effect of the mixed material is better and more uniform.

[0015] Furthermore, in step 2, an injection molding machine is used for injection, and the temperatures of the first, second, third and fourth zones of the injection molding machine are 180-190° C., 175-185° C., 170-180° C. and 165-175° C. respectively, and the holding time is 20-30s.

[0016] Furthermore, in step three, the foaming temperature is 115-125° C., the foaming pressure is 20-30 MPa, and the foaming time is 110-130 min.

[0017] Furthermore, in step four, the cooling time of the foaming mold is 24-48 hours; the hot pressing temperature during the hot pressing and shaping process is 160-170°C, and the hot pressing time is 400-600s; the cooling temperature during the cooling and shaping process is 20-30°C, and the cooling time is 400-600s.

[0018] In addition, the present invention also provides a shoe, which uses the above-mentioned tear-resistant lightweight extremely elastic midsole as a midsole component. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are preferred embodiments of the present invention and should not be regarded as excluding other embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the claims and description of the present invention, unless explicitly defined otherwise, the terms "first", "second" or "third" etc. are used to distinguish different objects rather than to describe a specific order.

[0021] In the claims and description of the present invention, if the terms "include", "have" and their variations are used, they are intended to mean "including but not limited to".

[0022] The invention provides a tear-resistant, lightweight and extremely elastic midsole, which mainly comprises the following components in parts by mass: 60-80 parts of a thermoplastic elastomer, 10-40 parts of an α-olefin elastomer, 10-40 parts of an ethylene-vinyl acetate copolymer, 1-2 parts of zinc oxide, 0.5-1 part of a peroxide crosslinking agent, 0.5-1 part of stearic acid, and 1-2 parts of titanium dioxide; wherein the thermoplastic elastomer is a thermoplastic polyester elastomer or a polyether block polyamide elastomer, and the melting point ranges from 150 to 175° C.; and the melting point range of the α-olefin elastomer is from 50 to 125° C.

[0023] In addition, the vinyl acetate content of the ethylene-vinyl acetate copolymer is in the range of 10-40wt%; the zinc content of the zinc oxide is higher than 95wt%; and the peroxide crosslinking agent is selected from one or more of diisopropylbenzene peroxide and 1,4-di-tert-butylperoxyisopropylbenzene.

[0024] Specifically, the thermoplastic elastomer can be any brand within the preset melting point range, preferably HYTRER7889, UPAE6080, UPAET5050, etc. can be selected; the a-olefin elastomer can be any brand within the preset melting point range, preferably POE746, POE8080, POE8003, OBC9107, EPDM626, etc. can be selected; the ethylene-vinyl acetate copolymer can be any brand with a vinyl acetate content within the preset range, preferably 7470, 33121, etc. can be selected; zinc oxide can be any brand with a zinc content of more than 95%, preferably Zn997 can be selected; the preferred brand of stearic acid is 1801; the preferred product model of titanium dioxide is DuPont's R103 or R105; the preferred varieties of cross-linking agents are DCP PERKADOX BC-FF and BIBPPERKADOX 14S-FL.

[0025] In the tear-resistant, lightweight and extremely elastic midsole, a thermoplastic polyester elastomer or a polyether block polyamide elastomer is used as the basis, and an α-olefin elastomer is added thereto. The α-olefin elastomer has a certain degree of crystallinity, a relatively narrow molecular weight, and a relatively low density. It has high elasticity, high elongation, good impact strength, good low temperature resistance and processing rheology. The saturated structure of its main chain makes it superior to traditional elastomers in terms of heat aging resistance and UV resistance. Good mobility can improve the dispersion effect of the filler. After it is added to the thermoplastic polyester elastomer or the polyether block polyamide elastomer, it can be dispersed into these thermoplastic elastomers under the action of additives. In the invention, the thermoplastic elastomer is bonded to the midsole, thereby enhancing the tear resistance of the midsole. The low density of the α-olefin elastomer can ensure that the weight of the midsole meets the requirements. The α-olefin elastomer has high compatibility with the thermoplastic polyester elastomer or the polyether block polyamide elastomer, and can enhance the resilience of the midsole. Among them, the thermoplastic elastomer with a melting point range of 150-175°C and the α-olefin elastomer with a melting point range of 50-125°C are selected, so that the mixing of the two can be ensured to be sufficient during the preparation process, so that the prepared midsole has excellent tear resistance, light weight and good resilience.

[0026] In addition, the ethylene-vinyl acetate copolymer selected in the formula includes a vinyl acetate component, which can enhance the elasticity of the midsole material. An appropriate range of the mass proportion of vinyl acetate can ensure that the midsole has good rebound performance while avoiding the interaction between vinyl acetate and the α-olefin elastomer to reduce the tear resistance of the midsole.

[0027] According to the above-mentioned component ratio, the present invention also provides a method for preparing the above-mentioned tear-resistant lightweight elastic midsole, which adopts the following steps:

[0028] Step 1, weighing each raw material according to mass, and granulating after mixing to obtain seed material;

[0029] Step 2, heating and melting the seed material and then injecting it into a first mold to obtain a small embryo to be foamed;

[0030] Step 3, foaming the small embryo by supercritical foaming process to obtain a foaming mold embryo;

[0031] Step 4: After the foaming mold is cooled, place it into a second mold and perform hot pressing and cooling to obtain the tear-resistant, lightweight and elastic midsole.

[0032] Wherein, in step one, a twin-screw machine is used for granulation, the temperatures of the first, second, third and fourth zones of the twin-screw machine are 185-195°C, 180-190°C, 175-185°C and 170-180°C respectively, and the screw speed is 15-20rpm.

[0033] In step 2, an injection molding machine is used for injection molding, wherein the temperatures of the first, second, third and fourth zones of the injection molding machine are 180-190° C., 175-185° C., 170-180° C. and 165-175° C. respectively, and the holding time is 20-30 seconds.

[0034] In step three, the foaming temperature is 115-125° C., the foaming pressure is 20-30 MPa, and the foaming time is 110-130 min.

[0035] In step 4, the cooling time of the foaming mold is 24-48 hours; the hot pressing temperature during the hot pressing shaping process is 160-170°C, and the hot pressing time is 400-600s; the cooling temperature during the cooling and shaping process is 20-30°C, and the cooling time is 400-600s.

[0036] In the preparation method, a supercritical foaming process is adopted to foam a small embryo to be foamed. After the foaming, the foamed embryo mold obtained is cooled and then subjected to hot pressing and cooling to obtain the tear-resistant, lightweight and extremely elastic midsole. Since the supercritical foaming process is adopted, there is no need to add a foaming agent or other auxiliary agents during the preparation of the midsole, and since gas infiltrates into the interior of the midsole during the foaming process, more cavities can be formed inside the midsole, so that the midsole has a lower density and higher resilience. However, at the same time, the conventional supercritical foaming process will reduce the tear resistance of the midsole. The present invention adds an a-olefin elastomer to the preparation components, so that the prepared midsole can maintain a high tear resistance. In addition, since the midsole is shaped by hot pressing after foaming, compared with the thermosetting process, the scraps in the preparation process and the midsole after use can be reused, which is more environmentally friendly.

[0037] In addition, the temperature of each zone of the twin-screw machine and the injection molding machine is limited, which can be adapted to the melting point range of the selected thermoplastic elastomer and α-olefin elastomer, so that the mixing effect of the mixed materials is better and more uniform.

[0038] Among them, the first mold used is a mold for preparing a small mold base, which roughly has the shape of a midsole, but is smaller in size; the second mold is a larger mold for preparing a midsole. After the foaming mold base is placed in the second mold, the foaming mold base is molded into the shape of the midsole by hot pressing. In the conventional preparation process, the foaming material in a molten state needs to be fed into the mold and then solidified. The present invention first uses the first mold to form a small mold base, and then foams the small mold base. The formed foaming mold base has roughly the shape of a shoe midsole, and then the second mold is hot-pressed to obtain a midsole with a preset shape. Compared with the conventional preparation method, the process of this process is simpler and has less material waste. At the same time, in the hot pressing step, the foaming mold base can be further extruded, so that the resilience and tear resistance of the obtained midsole are better.

[0039] In addition, the present invention also provides a shoe, which uses the above-mentioned tear-resistant lightweight extremely elastic midsole as a midsole component.

[0040] Since the above-mentioned tear-resistant, lightweight and extremely elastic midsole is used as the midsole component, the shoe can be used in scenarios such as sports shoes that have high requirements for midsole components. Even after high-intensity use, the shoe can maintain good rebound and shock-absorbing performance, and will not cause the midsole of the shoe to rupture due to poor tear resistance, which will then lead to the scrapping of the shoe.

[0041] The present invention also provides the following examples and comparative examples to illustrate various properties of the tear-resistant, lightweight, extremely elastic midsole.

[0042] Example 1

[0043] Weigh the raw materials according to the following mass ratio: 60 parts of thermoplastic elastomer, 10 parts of α-olefin elastomer, 10 parts of ethylene-vinyl acetate copolymer, 1 part of zinc oxide, 0.5 parts of peroxide crosslinking agent, 0.5 parts of stearic acid, and 1 part of titanium dioxide; wherein, the thermoplastic elastomer is a thermoplastic polyester elastomer with a brand name of HYTRER7889; the α-olefin elastomer is POE7467; the ethylene-vinyl acetate copolymer is EVA7470; the zinc oxide is Zn997; the stearic acid is AST1801; the titanium dioxide is R103; and the crosslinking agent is BIBP PERKADOX 14S-FL;

[0044] After weighing the raw materials, a twin-screw machine was used to granulate to obtain seed material; the temperatures of the first, second, third and fourth zones of the twin-screw machine were 190° C., 185° C., 180° C. and 175° C. respectively, and the screw speed was 20 rpm;

[0045] The seed material is heated and melted by an injection molding machine and then injected into the first mold to obtain a small embryo to be foamed; the temperatures of the first, second, third and fourth zones of the injection molding machine are 185°C, 180°C, 175°C and 170°C respectively, and the holding time is 30s;

[0046] The small embryo to be foamed is foamed by a supercritical foaming process to obtain a foaming mold embryo; wherein the foaming temperature is 120° C., the foaming pressure is 25 MPa, and the foaming time is 120 min;

[0047] After the foaming mold is cooled, it is placed in the second mold and subjected to hot pressing and cooling to obtain a tear-resistant, lightweight and elastic midsole; the cooling time of the foaming mold is 36 hours; the hot pressing temperature during the hot pressing and shaping process is 165°C, and the hot pressing time is 500s; the cooling temperature during the cooling and shaping process is 25°C, and the cooling time is 500s.

[0048] Example 2

[0049] Example 2 is based on Example 1, with the difference that the raw materials are prepared in the following proportions by mass: 70 parts of thermoplastic elastomer, 25 parts of α-olefin elastomer, 25 parts of ethylene-vinyl acetate copolymer, 1 part of zinc oxide, 0.5 parts of peroxide crosslinking agent, 0.5 parts of stearic acid, and 1 part of titanium dioxide.

[0050] Example 3

[0051] Example 3 is based on Example 1, with the difference that the raw materials are prepared in the following proportions by mass: 80 parts of thermoplastic elastomer, 40 parts of α-olefin elastomer, 40 parts of ethylene-vinyl acetate copolymer, 2 parts of zinc oxide, 1 part of peroxide crosslinking agent, 1 part of stearic acid, and 2 parts of titanium dioxide.

[0052] Example 4

[0053] Example 4 is based on Example 1, with the difference that the thermoplastic elastomer is a polyether block polyamide elastomer with the brand name UPAET5050.

[0054] Comparative Example 1

[0055] Comparative Example 1 is based on Example 1, except that no α-olefin elastomer is added.

[0056] Comparative Example 2

[0057] Comparative Example 2 is based on Example 1, except that no ethylene-vinyl acetate copolymer is added.

[0058] The above-mentioned Examples 1, 2, 3, 4 and Comparative Examples 1 and 2 were tested for performance, and the data are as follows:

[0059]

[0060] It can be seen from the above performance test data that, compared with Comparative Examples 1 and 2, the tear-resistant lightweight extremely elastic midsole provided by the present invention has greatly improved the tear resistance while maintaining a relatively low density and better rebound performance, thereby ensuring the durability of the midsole. Among them, since no α-olefin elastomer is added to Comparative Example 1, its tear resistance is greatly affected compared with Example 1, which shows that in the tear-resistant lightweight extremely elastic midsole provided by the present invention, the α-olefin elastomer plays a major role in improving the tear resistance of the midsole; in addition, no ethylene-vinyl acetate copolymer is added to Comparative Example 2, and its tear resistance is improved to a certain extent compared with Comparative Example 1, but it is still not comparable to the tear-resistant lightweight extremely elastic midsole provided by the present invention, which shows that the ethylene-vinyl acetate copolymer also plays a certain role in improving the tear resistance.

[0061] The description of the above specification and embodiments is used to explain the protection scope of the present invention, but does not constitute a limitation on the protection scope of the present invention. Through the enlightenment of the present invention or the above embodiments, ordinary technicians in this field can obtain modifications, equivalent substitutions or other improvements to the embodiments of the present invention or part of the technical features thereof through logical analysis, reasoning or limited experiments, which should be included in the protection scope of the present invention.

Claims

1. A tear-resistant, lightweight and extremely elastic midsole, characterized in that: The composition comprises the following components in parts by weight: 60-80 parts of thermoplastic elastomer, 10-40 parts of α-olefin elastomer, 10-40 parts of ethylene-vinyl acetate copolymer, 1-2 parts of zinc oxide, 0.5-1 parts of peroxide crosslinking agent, 0.5-1 parts of stearic acid, 1-2 parts of titanium dioxide; Wherein, the thermoplastic elastomer is a thermoplastic polyester elastomer or a polyether block polyamide elastomer, and its melting point ranges from 150 to 175°C; the melting point range of the a-olefin elastomer is from 50 to 125°C.

2. The tear-resistant, lightweight, extremely elastic midsole according to claim 1, characterized in that: In the ethylene-vinyl acetate copolymer, the content of vinyl acetate is in the range of 10-40 wt %.

3. The tear-resistant, lightweight, extremely elastic midsole according to claim 1, characterized in that: The zinc content of the zinc oxide is higher than 95 wt %.

4. The tear-resistant, lightweight, extremely elastic midsole according to claim 1, characterized in that: The peroxide crosslinking agent is selected from one or more of dicumyl peroxide and 1,4-di-tert-butyl peroxycumene.

5. A method for preparing a tear-resistant, lightweight and extremely elastic midsole, characterized in that: According to the ratio of a tear-resistant, lightweight and extremely elastic midsole as claimed in any one of claims 1 to 4, the midsole is prepared by the following steps: Step 1: Weigh each raw material according to mass, and granulate after mixing to obtain seed material; Step 2, heating and melting the seed material and then injecting it into a first mold to obtain a small embryo to be foamed; Step 3, foaming the small embryo by supercritical foaming process to obtain a foaming mold embryo; Step 4: After the foaming mold is cooled, place it into a second mold and perform hot pressing and cooling to obtain the tear-resistant, lightweight and elastic midsole.

6. The method for preparing a tear-resistant, lightweight, extremely elastic midsole according to claim 5, characterized in that: In step 1, a twin-screw machine is used for granulation, wherein the temperatures of the first, second, third and fourth zones of the twin-screw machine are 185-195° C., 180-190° C., 175-185° C. and 170-180° C. respectively, and the screw speed is 15-20 rpm.

7. The method for preparing a tear-resistant, lightweight, extremely elastic midsole according to claim 5, characterized in that In step 2, an injection molding machine is used for injection molding, and the temperatures of the first, second, third and fourth zones of the injection molding machine are 180-190° C., 175-185° C., 170-180° C. and 165-175° C. respectively, and the holding time is 20-30 seconds.

8. The method for preparing a tear-resistant, lightweight, extremely elastic midsole according to claim 5, characterized in that In step three, the foaming temperature is 115-125° C., the foaming pressure is 20-30 MPa, and the foaming time is 110-130 min.

9. The method for preparing a tear-resistant, lightweight, extremely elastic midsole according to claim 5, characterized in that In step 4, the cooling time of the foaming mold is 24-48h; the hot pressing temperature during the hot pressing and shaping process is 150-170°C, and the hot pressing time is 400-600s; the cooling temperature during the cooling and shaping process is 20-30°C, and the cooling time is 400-600s.

10. A shoe, characterized in that: The tear-resistant, lightweight and extremely elastic midsole as described in any one of claims 1 to 5 is used as the midsole component.