Preparation method of high-strength asphalt material for roads and bridges
By adding nanographene and basalt fibers, modified organic solvent lignin and modified nanomontmorillonite to the asphalt material, the problem of easy cracking of asphalt materials under low temperature conditions is solved, the high temperature stability and crack resistance are improved, and the high temperature stability and crack resistance are extended service life.
Patent Information
- Application Number
- CN202411348279.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing modified asphalt materials for road and bridges are prone to cracking under low temperature conditions, and the use temperature is limited, resulting in insufficient crack resistance.
Nanographene and basalt fibers are used as composite fillers, and the network structure is formed through a high-speed shearing machine to improve the high-temperature stability and deformation resistance of asphalt; the organic solvent lignin is modified to increase the ester bonds to improve the asphalt Hydrophobic properties; nanomontmorillonite is modified to form a vertical double-layer intercalation structure to enhance the thermal aging resistance of asphalt.
It significantly improves the high-temperature stability, low-temperature crack resistance and thermal aging resistance of asphalt materials, extends the service life, and reduces the occurrence of road surface water damage.
Smart Images

Figure CN119019858A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt materials, and in particular to a method for preparing a high-strength asphalt material for roads and bridges. Background Art
[0002] Asphalt is a dark brown complex mixture of hydrocarbons of different molecular weights and their non-metallic derivatives. It is a kind of high-viscosity organic liquid.
[0003] A Chinese patent with publication number CN110564170A discloses a modified asphalt for roads and bridges, comprising the following components in parts by weight: 60-80 parts of base asphalt, 6-8 parts of dispersant, 6-8 parts of plasticizer, 5-7 parts of polymer fiber, 0.5-1 part of cross-linking agent, 0.5-1 part of compatibilizer, 1-2 parts of stabilizer, 50-60 parts of aggregate, 40-50 parts of filler, 1-3 parts of titanium dioxide, 1-1.5 parts of fatty alcohol polyoxyethylene ether ammonium sulfate, 4-6 parts of ultraviolet absorber, 15-20 parts of rubber powder, 1-2 parts of emulsifier and 2-4 parts of accelerator. Compared with the prior art, the invention modifies the base asphalt through a variety of additives. First, titanium dioxide and ultraviolet absorbers have strong ultraviolet absorption capacity and excellent thermal stability, which can significantly reduce the impact of light on asphalt materials and improve the anti-aging performance of asphalt materials. Sodium hexametaphosphate or sodium pyrophosphate not only has excellent dispersion effect and improves the uniformity of asphalt materials, but also has high compressive strength, which can significantly improve the anti-rolling performance and mechanical strength of asphalt materials. However, the asphalt prepared by the above-mentioned prior art solution is limited in use temperature and is prone to cracking under low temperature conditions. For this reason, the present invention provides a method for preparing high-strength asphalt materials for roads and bridges to solve the above problems. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-strength asphalt material for roads and bridges, which solves the problems mentioned in the above background technology.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing a high-strength asphalt material for roads and bridges, comprising the following preparation steps: Step 1: Heat the oven and high-speed shearing machine to 135-150°C. After the temperature stabilizes, place the matrix asphalt and composite filler into the oven and keep them warm for 2-2.3 hours. Step 2: Place the base asphalt in a high-speed shearing machine, slowly add the composite filler into the base asphalt under stirring conditions, and shear at a rate of 4000-5000 r / min for 50-60 minutes. Step 3: Then add the composite emulsion and shear at a rate of 280-300 r / min for 10-15 min; Step 4: Finally, add the modified nano-montmorillonite and the modified organic solvent lignin, and shear at a rate of 1200-1500 r / min for 40-50 minutes to obtain a high-strength asphalt material for roads and bridges.
[0006] Preferably, the weight proportions of the components in the high-strength asphalt material are: 85-100 parts of base asphalt, 4-6 parts of composite filler, 12-18 parts of composite emulsion, 5-7 parts of modified nano-montmorillonite, and 3-5 parts of modified organic solvent lignin.
[0007] Preferably, the composite filler is nanographene and basalt fiber, and the mass ratio thereof is 1:(0.6-0.8).
[0008] Preferably, the preparation method of the composite emulsion is: 20 to 25 parts of polytetrahydrofuran are mixed with 15 to 18 parts of castor oil, and the mixture is heated to 110 to 120° C. in an oil bath, and then the mixture is vacuum dehydrated for 2 to 3 hours and then cooled to 60 to 80° C.; deionized water is added, and emulsification is performed for 30 to 40 minutes, and then 4 to 6 parts of diphenylmethane diisocyanate are added, and the mixture is stirred and reacted at 60 to 80° C. for 2 to 3 hours under nitrogen protection, and then 8 to 10 parts of methyldiethanolamine are added, and the mixture is stirred and reacted at 30 to 50° C. for 2 to 3 hours, and then 5 to 7 parts of a mixed solution of epoxy resin and acetone are added, and the mixture is stirred and reacted at 30 to 50° C. for 1 to 2 hours, and then the mixture is cooled to room temperature, and glacial acetic acid is added for neutralization and stirring for 1 to 1.5 hours.
[0009] Preferably, the mass ratio of the epoxy resin to acetone is (0.3-0.4):1.
[0010] Preferably, the preparation method of the modified nano-montmorillonite is: adding octadecyl dimethyl benzyl ammonium chloride to the nano-montmorillonite suspension and stirring at a speed of 2800-3000 r / min for 5.5-6 hours; after the reaction is completed, centrifugation is performed and the precipitate is rinsed with deionized water for 4-6 times; finally, the precipitate is placed in a vacuum drying oven for drying and then ground into powder.
[0011] Preferably, in the nano-montmorillonite suspension, the mass proportion of nano-montmorillonite is 5%; the mass ratio of the nano-montmorillonite suspension to octadecyldimethylbenzylammonium chloride is 1:(0.2-0.4).
[0012] Preferably, the preparation method of the modified organic solvent lignin is: 1 to 3 g of organic solvent lignin is placed in a drying oven at 100 to 105° C. and dried for 1.8 to 2 hours, then cooled and ground, and then 10 mL of pyridine is added, and then 2.5 to 3 mL of acetic anhydride is added, and the temperature is raised to 80 to 85° C. and reacted for 22 to 24 hours, and then poured into ice water, and filtered, distilled, and filtered in sequence, and the filter residue is placed in a vacuum drying oven at 50 to 55° C. and dried to obtain the modified organic solvent lignin.
[0013] The present invention provides a method for preparing high-strength asphalt material for roads and bridges. Compared with the prior art, it has the following beneficial effects: (1) The preparation method of the high-strength asphalt material for roads and bridges comprises the following steps: adding nano-graphene and basalt fibers; since nano-graphene itself has a large specific surface area and good thermal conductivity, and basalt fibers can enhance the toughness of asphalt mixtures, the two can give full play to their synergistic advantages and comprehensively improve the high-temperature stability of asphalt mixtures; at the same time, the addition of graphene and basalt fibers can form a mesh structure inside the asphalt, thereby limiting the fluidity of the asphalt, synergistically improving the high-temperature deformation resistance of the asphalt, enhancing the bonding strength inside the asphalt, and effectively inhibiting the formation and development of cracks under low temperature conditions, thereby improving the low-temperature crack resistance of the asphalt.
[0014] (2) The method for preparing high-strength asphalt material for roads and bridges reduces hydroxyl groups and increases ester bonds by modifying the organic solvent lignin, which is beneficial to the combination of asphalt and lignin, improves the uniformity of lignin distribution in asphalt, enhances the hydrophobicity of asphalt, and extends the service life of asphalt, so that the asphalt can effectively reduce the occurrence of water damage to the road surface when in use.
[0015] (3) The method for preparing high-strength asphalt material for roads and bridges is as follows: since octadecyl dimethyl benzyl ammonium chloride has a longer carbon chain and a larger branched molecule, montmorillonite is modified so that a vertical double-layer intercalation structure can be formed between the montmorillonite layers, thereby enhancing the internal stability of the asphalt, thereby enhancing the asphalt's resistance to thermal aging. At the same time, the larger interlayer spacing effectively improves the healing performance of the asphalt. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The SEM images of the nano-montmorillonite before and after modification provided by the present invention; Figure 2 The microscopic morphology of the organic solvent lignin before and after modification provided by the present invention; Figure 3 This is a schematic diagram of the water contact angle of the modified lignin provided by the present invention; Figure 4 This is a comparison chart of the low-temperature crack resistance test provided by the present invention. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] In this technical solution, SK90# base asphalt is used.
[0019] Example 1 A method for preparing a high-strength asphalt material for roads and bridges, comprising the following preparation steps: Step 1: Heat the oven and high-speed shearing machine to 135°C. After the temperature stabilizes, put 85g of matrix asphalt and 6g of nanographene and basalt fiber with a mass ratio of 1:0.6 into the oven and keep warm for 2h. Step 2: Place the base asphalt in a high-speed shearing machine, slowly add the composite filler into the base asphalt under stirring conditions, and shear at a rate of 4000r / min for 50min. Step 3: Then add 18g of the composite emulsion and shear at a rate of 280r / min for 10min; The preparation method of the composite emulsion is as follows: 20 g of polytetrahydrofuran is mixed with 18 g of castor oil, and the mixture is heated to 110° C. in an oil bath, and then the mixture is vacuum dehydrated for 2 h and then cooled to 60° C.; deionized water is added, and the mixture is emulsified for 30 min, and then 6 g of diphenylmethane diisocyanate is added, and the mixture is stirred and reacted at 60° C. for 2 h under nitrogen protection, and then 10 g of methyldiethanolamine is added, and the mixture is stirred and reacted at 30° C. for 2 h, and then 7 g of a mixed solution of epoxy resin and acetone with a mass ratio of 0.3:1 is added, and the mixture is stirred and reacted at 30° C. for 1 h, and then the mixture is cooled to room temperature, and glacial acetic acid is added and the mixture is neutralized and stirred for 1 h; Step 4: Finally, add 7g of modified nano-montmorillonite and 5g of modified organic solvent lignin, and shear at a rate of 1200r / min for 40min to obtain a high-strength asphalt material for roads and bridges; The preparation method of the modified nano-montmorillonite is as follows: add 0.2 g of octadecyl dimethyl benzyl ammonium chloride to 1 g of 5% nano-montmorillonite suspension, and stir at a speed of 2800 r / min for 5.5 h; after the reaction is completed, centrifuge and separate, and rinse the precipitate with deionized water for 4 times; finally, dry it in a vacuum drying oven and grind it into powder; The preparation method of modified organic solvent lignin is as follows: 1 g of organic solvent lignin is placed in a drying oven at 100°C for 1.8 hours, then cooled and ground, and then 10 mL of pyridine is added, and then 2.5 mL of acetic anhydride is added, the temperature is raised to 80°C and reacted for 22 hours, and then poured into ice water, and filtered, distilled, and filtered in sequence, and the filter residue is placed in a vacuum drying oven at 50°C for drying to obtain modified organic solvent lignin.
[0020] Example 2 A method for preparing a high-strength asphalt material for roads and bridges, comprising the following preparation steps: Step 1: Heat the oven and high-speed shearing machine to 145°C. After the temperature stabilizes, put 90g of matrix asphalt and 5g of nanographene and basalt fiber with a mass ratio of 1:0.7 into the oven and keep warm for 2.2h. Step 2: Place the base asphalt in a high-speed shearing machine, slowly add the composite filler into the base asphalt under stirring conditions, and shear at a rate of 4500r / min for 55min. Step 3: Then add 12-18g of the composite emulsion and shear at a rate of 290r / min for 12min; The preparation method of the composite emulsion is as follows: 22g of polytetrahydrofuran is mixed with 16g of castor oil, and the mixture is heated to 115°C in an oil bath, and then the mixture is vacuum dehydrated for 3h and then cooled to 70°C; deionized water is added, and emulsification is performed for 35min, and then 5g of diphenylmethane diisocyanate is added, and the mixture is stirred and reacted at 75°C for 3h under nitrogen protection, and then 9g of methyldiethanolamine is added, and the mixture is stirred and reacted at 40°C for 3h, and then 6g of a mixed solution of epoxy resin and acetone with a mass ratio of 0.4:1 is added, and the mixture is stirred and reacted at 40°C for 2h, and then the mixture is cooled to room temperature, and glacial acetic acid is added for neutralization and stirring for 1.5h; Step 4: Finally, add 6g of modified nano-montmorillonite and 4g of modified organic solvent lignin, and shear at a rate of 1300r / min for 45min to obtain a high-strength asphalt material for roads and bridges; The preparation method of the modified nano-montmorillonite is as follows: add 0.3 g of octadecyl dimethyl benzyl ammonium chloride to 1 g of 5% nano-montmorillonite suspension, and stir at a speed of 2900 r / min for 6 hours; after the reaction is completed, centrifuge and separate, and rinse the precipitate with deionized water for 5 times; finally, dry it in a vacuum drying oven and grind it into powder; The preparation method of modified organic solvent lignin is as follows: 2 g of organic solvent lignin is placed in a drying oven at 105°C for 2 hours, then cooled and ground, and then 10 mL of pyridine is added, and then 2 mL of acetic anhydride is added, the temperature is raised to 80°C for reaction for 23 hours, and then poured into ice water, and filtered, distilled, and filtered in sequence, and the filter residue is placed in a vacuum drying oven at 50°C for drying to obtain modified organic solvent lignin.
[0021] Example 3 A method for preparing a high-strength asphalt material for roads and bridges, comprising the following preparation steps: Step 1: Heat the oven and high-speed shearing machine to 150°C. After the temperature stabilizes, put 100g of matrix asphalt and 4g of nanographene and basalt fiber with a mass ratio of 1:0.8 into the oven and keep warm for 2.3h. Step 2: Place the base asphalt in a high-speed shearing machine, slowly add the composite filler into the base asphalt under stirring conditions, and shear at a rate of 5000r / min for 60min. Step 3: Then add 12g of the composite emulsion and shear at a rate of 300r / min for 15min; The preparation method of the composite emulsion is as follows: 25 g of polytetrahydrofuran is mixed with 15 g of castor oil, and the mixture is heated to 120° C. in an oil bath, and then the mixture is vacuum dehydrated for 3 hours and then cooled to 80° C.; deionized water is added, and the mixture is emulsified for 40 minutes, and then 4 g of diphenylmethane diisocyanate is added, and the mixture is stirred and reacted at 80° C. for 3 hours under nitrogen protection, and then 8 g of methyldiethanolamine is added, and the mixture is stirred and reacted at 50° C. for 3 hours, and then 5 g of a mixed solution of epoxy resin and acetone with a mass ratio of 0.4:1 is added, and the mixture is stirred and reacted at 50° C. for 2 hours, and then the mixture is cooled to room temperature, and glacial acetic acid is added for neutralization and stirring for 1.5 hours; Step 4: Finally, add 5g of modified nano-montmorillonite and 3g of modified organic solvent lignin, and shear at a rate of 1500r / min for 50min to obtain a high-strength asphalt material for roads and bridges; The preparation method of the modified nano-montmorillonite is as follows: add 0.4 g of octadecyl dimethyl benzyl ammonium chloride to 1 g of 5% nano-montmorillonite suspension, and stir at a speed of 3000 r / min for 6 hours; after the reaction is completed, centrifuge and separate, and rinse the precipitate with deionized water for 6 times; finally, dry it in a vacuum drying oven and grind it into powder; The preparation method of modified organic solvent lignin is as follows: 3 g of organic solvent lignin is placed in a drying oven at 105°C for 2 hours, then cooled and ground, and then 10 mL of pyridine is added, and then 3 mL of acetic anhydride is added, the temperature is raised to 85°C for reaction for 24 hours, and then poured into ice water, and filtered, distilled, and filtered in sequence, and the filter residue is placed in a vacuum drying oven at 55°C for drying to obtain modified organic solvent lignin.
[0022] Comparative Example 1 Compared with Example 1, the composite filler in Example 1 is replaced by basalt fiber.
[0023] Comparative Example 2 Compared with Example 1, the modified nano-montmorillonite in Example 1 is replaced by nano-montmorillonite.
[0024] Comparative Example 3 Compared with Example 1, the modified organic solvent lignin in Example 1 is replaced by organic solvent lignin.
[0025] Mechanical properties test: According to GB / T 1040.3-2006 standard, the test was carried out at room temperature using an electronic universal testing machine. The average value of 5 samples was taken to calculate the tensile strength and elongation at break of the samples. The results are shown in Table 1.
[0026] Shear performance test: 50mm thick rutting board specimens were used to form AC-13 mixture rutting boards, and 0.8kg / m 2 Asphalt was then used, and a 10 cm thick rutting plate specimen was used. A 5 cm thick AC-16 composite specimen was laid on the original rutting plate specimen. After the production was completed, core sampling was performed to obtain a shear strength specimen with a height of 100 mm for interlaminar shear test. The results are shown in Table 1.
[0027] Table 1
[0028] Low temperature crack resistance test: A rutting plate specimen of 300mm×300mm×50mm was prepared by the rutting test method, and then cut into 250mm×30mm×35mm prismatic beam specimens with a span of 200mm. The test temperature was -10℃, the loading rate was 50mm / min, and the MTS testing machine was used to test. When the beam specimen broke, the maximum tensile strain was recorded; the flexural tensile strength was used as the evaluation index of the low temperature crack resistance of asphalt; the results are as follows Figure 4 As shown; the calculation formula for flexural tensile strength is: ; In the formula, is the flexural tensile strength of the specimen at failure, MPa; is the specimen span, mm; is the maximum load when the specimen is damaged, N; is the width of the test piece across the interruption, mm; is the height of the test piece across the interruption, mm.
[0029] Put the asphalt into the UV aging box at 60℃ for 35 days, and then conduct the following tests: (1) Softening point test: The test was carried out according to the test method of T0606-2011 in JTGE20-2011; the results are shown in Table 1.
[0030] (2) 25°C needle penetration test: The test was carried out according to the test method of T0604-2011 in JTGE20-2011; the results are shown in Table 1.
[0031] (3) Ductility test: The test was carried out according to the test method of T0605-2011 in TGE20-2011. The results are shown in Table 1.
[0032] Table 2
[0033] like Figure 1 As shown, the nano-montmorillonite before modification is completely soluble in water, and the nano-montmorillonite after modification is completely hydrophobic.
[0034] like Figure 2 As shown, before modification, the organic solvent lignin particles are smaller and the surface is rougher; after modification, the organic solvent lignin particles become larger and the surface is smoother.
[0035] like Figure 3 As shown, the water contact angle of the modified organic solvent lignin is 130.87°, because a part of the hydroxyl groups have been replaced, which weakens the ability of lignin to bind to water, making it more hydrophobic and having a larger water contact angle.
[0036] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0037] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0038] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing high-strength asphalt material for roads and bridges, It is characterized in that The method comprises the following preparation steps: Step 1: Heat the oven and high-speed shearing machine to 135-150°C. After the temperature stabilizes, place the matrix asphalt and composite filler into the oven and keep them warm for 2-2.3 hours. Step 2: Place the base asphalt in a high-speed shearing machine, slowly add the composite filler into the base asphalt under stirring conditions, and shear at a rate of 4000-5000 r / min for 50-60 minutes. Step 3: Then add the composite emulsion and shear at a rate of 280-300 r / min for 10-15 min; Step 4: Finally, add the modified nano-montmorillonite and the modified organic solvent lignin, and shear at a rate of 1200-1500 r / min for 40-50 minutes to obtain a high-strength asphalt material for roads and bridges.
2. A method for preparing a high-strength asphalt material for roads and bridges according to claim 1, Features: The weight proportions of the components in the high-strength asphalt material are: 85-100 parts of base asphalt, 4-6 parts of composite filler, 12-18 parts of composite emulsion, 5-7 parts of modified nano-montmorillonite, and 3-5 parts of modified organic solvent lignin.
3. The method for preparing a high-strength asphalt material for roads and bridges according to claim 1, Features: The composite filler is nanographene and basalt fiber, and the mass ratio thereof is 1:(0.6-0.8).
4. The method for preparing a high-strength asphalt material for roads and bridges according to claim 1, Features: The preparation method of the composite emulsion is as follows: 20-25 parts of polytetrahydrofuran and 15-18 parts of castor oil are mixed, and the mixture is heated to 110-120° C. in an oil bath, and then the mixture is vacuum dehydrated for 2-3 hours and then cooled to 60-80° C.; deionized water is added, and emulsification is performed for 30-40 minutes; 4-6 parts of diphenylmethane diisocyanate are added, and the mixture is stirred and reacted at 60-80° C. for 2-3 hours under nitrogen protection; 8-10 parts of methyldiethanolamine are added, and the mixture is stirred and reacted at 30-50° C. for 2-3 hours; 5-7 parts of a mixed solution of epoxy resin and acetone are added, and the mixture is stirred and reacted at 30-50° C. for 1-2 hours, and then the mixture is cooled to room temperature, and glacial acetic acid is added for neutralization and stirring for 1-1.5 hours.
5. A method for preparing a high-strength asphalt material for roads and bridges according to claim 4, Features: The mass ratio of the epoxy resin to acetone is (0.3-0.4):
1.
6. The method for preparing a high-strength asphalt material for roads and bridges according to claim 1, Features: The preparation method of the modified nano-montmorillonite comprises: adding octadecyl dimethyl benzyl ammonium chloride to the nano-montmorillonite suspension, and stirring at a speed of 2800-3000 r / min for 5.5-6 hours; after the reaction is completed, centrifugation is performed, and the precipitate is washed with deionized water for 4-6 times; and finally, the precipitate is placed in a vacuum drying oven for drying and then ground into powder.
7. A method for preparing a high-strength asphalt material for roads and bridges according to claim 6, Features: In the nano-montmorillonite suspension, the mass proportion of nano-montmorillonite is 5%; the mass ratio of the nano-montmorillonite suspension to octadecyl dimethyl benzyl ammonium chloride is 1:(0.2-0.4).
8. The method for preparing a high-strength asphalt material for roads and bridges according to claim 1, Features: The preparation method of the modified organic solvent lignin is as follows: 1-3 g of the organic solvent lignin is placed in a drying oven at 100-105° C. for drying for 1.8-2 hours, then cooled, ground, and then 10 mL of pyridine is added, and then 2.5-3 mL of acetic anhydride is added, the temperature is raised to 80-85° C. for reaction for 22-24 hours, and then poured into ice water, and suction filtered, distilled, and filtered in sequence, and the filter residue is placed in a vacuum drying oven at 50-55° C. for drying to obtain the modified organic solvent lignin.
Citation Information
Patent Citations
Modified asphalt for roads and bridges and preparation method thereof
CN110564170A
Preparation method of anti-aging nano-organic montmorillonite modified asphalt
CN107189456A
Method for interweaving basalt fibers in asphalt mixture
CN113135693A
Asphalt cement with anti-aging performance
CN114958018A
Graphene-basalt fiber composite modified asphalt mixture and preparation method thereof
CN116768530A
Cited By
Self-healing rubber asphalt based on solid waste aggregate and preparation process thereof
CN119797814A
Self-healing rubber asphalt based on solid waste aggregate and preparation process thereof
CN119797814B