Resin-attached aluminum pigments, coatings and inks
By covering the resin with free radical polymerizable double bonds on the aluminum pigment and controlling the surface roughness and thickness of the resin layer, combined with external shear and vibration, the design and chemical resistance of the resin-adhesive aluminum pigment in the prior art are solved. The problem of insufficient results has achieved high design and alkali resistance.
Patent Information
- Application Number
- CN202410637513.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-12
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to adhere to aluminum pigments with a resin that is excellent in maintaining designability and chemical resistance, especially the thickness and surface roughness of the resin layer have little impact on designability and adhesion, and have insufficient alkali resistance.
By covering the surface of the aluminum particles with a resin with a radically polymerizable double bond, the average surface roughness of the resin layer is controlled to be in the range of 0.1 to 5.0 nm and the thickness is in the range of 10 nm to 20 nm, and the mass ratio of the resin adhesion layer to the aluminum particles is adjusted. Combined with shear and vibration external action, a resin-adhering aluminum pigment is formed with high design and chemical resistance.
It achieves excellent design, adhesion and chemical resistance of resin-adhesive aluminum pigments, improves the brightness and hiding properties of paints and inks, and improves the resistance to alkali and other chemicals.
Smart Images

Figure CN119019868A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin-attached aluminum pigment, and a coating and ink containing the resin-attached aluminum pigment. Background Art
[0002] Conventionally, aluminum pigments have been used for metallic paints, printing inks, plastic blending, etc. to achieve cosmetic effects that emphasize metallic texture. By coating these aluminum pigments with resin, alkali resistance tests can be improved. In particular, thin-film aluminum with an average particle size of 20 μm or less and a particle thickness of 0.2 μm or less has excellent design properties.
[0003] As a method for achieving the above-mentioned alkali resistance of the aluminum pigment, a method of subjecting the aluminum pigment to a predetermined surface treatment has been proposed.
[0004] For example, Patent Document 1 states that when the ratio of the resin mass per unit mass of the resin-attached aluminum pigment to the total surface area of the particles of the resin-attached aluminum pigment is within a predetermined range, there is a tendency that the designability and alkali resistance are excellent. However, there is no description that the thickness of the resin layer can contribute to the designability.
[0005] Patent Document 2 describes a method for producing a resin-coated metallic pigment in which 0.1 to 50 parts by weight of resin is attached to the surface of a metallic pigment relative to 100 parts by weight of the metallic pigment, and the desired resin-coated metallic pigment is obtained by promoting physical dispersion by adding an external action such as ultrasonic irradiation to the resin coating process. However, there is no description of whether the thickness of the resin layer can contribute to design properties.
[0006] Patent Document 3 states that a pigment having excellent chemical resistance to chemicals such as alkali can be provided by providing a ratio of the total area of the resin particles having an area equivalent circle diameter of 25 nm or more to the surface of the resin covering the surface of the aluminum particles within a specific range. However, there is no description of whether the thickness of the resin layer can contribute to the design properties.
[0007] Patent Document 4 describes an aluminum pigment and a method for producing the same that can provide a metal coating film having excellent design and adhesion. However, there is no description that the thickness of the resin layer can contribute to the design, and no description about alkali resistance.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-135455
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 2012-162733
[0012] Patent Document 3: International Publication No. 2018 / 047360
[0013] Patent Document 4: Japanese Patent Application Publication No. 2002-226733 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] An object of the present invention is to provide a resin-adhered aluminum pigment which has not always been fully achieved by using the above-mentioned conventional techniques, and to provide a resin-adhered aluminum pigment having excellent design properties, excellent adhesion and chemical resistance.
[0016] Solutions for solving problems
[0017] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by setting the average surface roughness of the resin layer surface of the resin-attached aluminum pigment and / or the thickness of the resin-attached layer within a predetermined range, a resin-attached aluminum pigment having excellent design properties, excellent adhesion and excellent chemical resistance to chemicals such as alkali can be obtained, thereby completing the present invention.
[0018] That is, the gist of the present invention is as follows.
[0019] [1] A resin-attached aluminum pigment, wherein the surface of aluminum particles is covered with a resin containing a polymer of a monomer and / or an oligomer having one or more free radical polymerizable double bonds, wherein the average surface roughness Ra of the resin layer surface of the resin-attached aluminum pigment is 0.1 to 5.0 nm.
[0020] [2] The resin-adhered aluminum pigment according to [1] above, wherein a thickness τ of the resin-adhered layer measured by cross-sectional observation is 10 nm to 20 nm.
[0021] [3] A resin-attached aluminum pigment, wherein the surface of aluminum particles is covered with a resin containing a polymer of a monomer and / or an oligomer having one or more free radical polymerizable double bonds, wherein the thickness τ of the resin-attached layer measured by cross-sectional observation is 10 nm to 20 nm.
[0022] [4] The resin-attached aluminum pigment according to [1], wherein the mass of the resin per unit mass of the resin-attached aluminum pigment (A (g / g)) and the total surface area per unit mass of the aluminum particles (SSA (m 2 The ratio of (A) / (SSA) is 0.0077 g / m 2 ~0.025g / m 2 .
[0023] [5] The resin-adhered aluminum pigment according to [1] above, wherein the average cross-sectional thickness τ' of the aluminum particles is 0.03 μm to 0.2 μm.
[0024] [6] The resin-adhered aluminum pigment according to [5] above, wherein the average particle size d50 of the aluminum particles is 5 μm to 15 μm.
[0025] [7] A coating material comprising the resin-adherent aluminum pigment according to any one of [1] to [6] above.
[0026] [8] An ink comprising the resin-adhered aluminum pigment according to any one of [1] to [6] above.
[0027] Effects of the Invention
[0028] According to the present invention, it is possible to provide a resin-adhered aluminum pigment which has not been sufficiently achieved by conventional techniques, and it is possible to provide a resin-adhered aluminum pigment having excellent design properties, excellent adhesion and excellent chemical resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is an example of a TEM photograph of the resin-coated metallic pigment of Example 1.
[0030] Figure 2 This is an example of a TEM photograph of the resin-coated metallic pigment of Comparative Example 1. DETAILED DESCRIPTION
[0031] Hereinafter, an example of a preferred mode for carrying out the present invention will be described. However, the following embodiment is an example for explaining the present invention, and the present invention is not limited to the following embodiment at all.
[0032] The resin-adhered aluminum pigment of the present invention has excellent adhesion and chemical resistance while maintaining excellent design properties.
[0033] The resin-adhered aluminum pigment of the present invention has a structure in which the surfaces of aluminum particles are covered with a resin containing a polymer of a monomer and / or an oligomer having one or more radically polymerizable double bonds.
[0034] The specific shape of the aluminum particles serving as a raw material of the resin-adhered aluminum pigment of the present invention will be described below.
[0035] The aluminum particles used in the present invention are not limited in type, and may be aluminum particles commonly used as aluminum pigments, and may be flat in shape such as scales, horns, or circles. If high design properties (such as brightness, glossiness, angular color change, and hiding properties) are maintained, the effects of the present invention are further exerted when aluminum particles of a high design grade (grade for vapor deposition-style metallic paint or ink) are used (hereinafter sometimes referred to as flaky aluminum powder).
[0036] The method for producing aluminum particles is not particularly limited, and the aluminum particles can be obtained by pulverizing granular powder or fragments of metallic aluminum with a few percent of a pulverizing aid using a mechanical method such as a stamp mill method, a dry ball mill method, a wet ball mill method, an attritor method, a vibration ball mill method, etc.
[0037] As a method for producing highly designed aluminum particles, for example, there is the method described in International Publication No. 99 / 54074. The flaky aluminum powder having a smooth surface and uniform thickness obtained by this production method can be particularly preferably used as a raw material for the aluminum pigment of the present invention.
[0038] The particle size of the aluminum particles that serve as the raw material of the resin-attached aluminum pigment of the present invention varies depending on the application. When the resin-attached aluminum pigment of the present invention is used for coatings and printing inks, aluminum particles having an average particle size d50 (μm) of about 1 to 100 μm can be suitably used. In addition, recently, as applications that particularly require high design properties of metallic pigments, there are listed automotive applications, general home appliances, and information appliances represented by mobile phones. In these applications, metallic pigments are used for coating metals such as iron and magnesium alloys, or plastics. In order to ensure high design properties, the preferred average particle size (d50) of the aluminum particles of the resin-attached aluminum pigment of the present invention used in these applications is 5 to 35 μm, and more preferably 5 to 15 μm.
[0039] The average particle size d50 (μm) of the aluminum particles of the present invention can be measured using a common laser diffraction / scattering particle size distribution measuring device, and can be measured, for example, as follows.
[0040] The average particle size (d50) of the flaky aluminum powder was measured using a laser diffraction / scattering particle size distribution analyzer (LA-300 / Horiba Ltd.). Mineral spirits were used as a measurement solvent.
[0041] It is preferred that the resin-adhering aluminum pigment serving as a sample is subjected to ultrasonic dispersion for 2 minutes as a pretreatment, and then placed in a dispersion tank, and measurement is started after confirming that an appropriate concentration has been achieved.
[0042] The average cross-sectional thickness τ' (μm) of the aluminum particles can be determined by measuring the cross-sectional FE-SEM image of the coating film using image analysis software.
[0043] Specifically, it can be determined by randomly selecting 100 particles in a FE-SEM image of a coating cross section, automatically measuring the cross-sectional thickness of the particles, and calculating the arithmetic mean of the 100 particles.
[0044] The average cross-sectional thickness τ′ (μm) of the aluminum particles of the present embodiment is preferably 0.03 μm to 0.2 μm.
[0045] The specific composition and shape of the resin adhered to the surface of the resin-adhering aluminum pigment of the present invention will be described below.
[0046] The resin to be attached to the resin-adhered aluminum pigment of the present embodiment is not particularly limited, but preferably, a resin containing a polymer of a monomer and / or an oligomer having one or more radically polymerizable double bonds is used.
[0047] As the aforementioned monomer having more than one free radical polymerizable double bond, there is no particular limitation, and a monomer having more than one free radical polymerizable double bond known in the past can be used. As a specific example of the aforementioned monomer having more than one free radical polymerizable double bond, it is not limited to the following, and unsaturated carboxylic acids (such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, citraconic acid, crotonic acid, maleic acid or maleic anhydride), mono- or diesters of phosphoric acid or phosphonic acid (such as 2-methacryloyloxyethyl phosphate, di-2-methacryloyloxyethyl phosphate, tri-2-methacryloyloxyethyl phosphate, 2-acryloyloxyethyl phosphate, di-2-acryloyloxyethyl phosphate, tri-2-acryloyloxyethyl phosphate, diphenyl-2-acryloyloxyethyl phosphate, dibutyl-2-methacryloyloxyethyl phosphate) can be suitably used. esters (e.g., dioctyl-2-acryloyloxyethyl phosphate, 2-methacryloyloxypropyl phosphate, bis(2-chloroethyl)vinylphosphonate, diallyl dibutylphosphonosuccinate, 2-methacryloyloxyethyl phosphate, 2-acryloyloxyethyl phosphate), coupling agents (e.g., γ-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, isopropyl isostearyldiacryl titanate, acetoalkoxy diisopropyl aluminum, zirconium aluminate), nitriles of unsaturated carboxylic acids (e.g., acrylonitrile, methacrylonitrile), or an ester of an unsaturated carboxylic acid (e.g., methyl acrylate, ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, stearyl acrylate, hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methoxyethyl acrylate, butoxyethyl acrylate, glycidyl acrylate, cyclohexyl acrylate, 1,6-hexanediol diacrylate, 1,4-butanediol diacrylate, triethylene glycol diacrylate, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, neopentyl glycol dimethacrylate, trimethylolpropane triacrylate, tetramethylolpropane tetraacrylate, tetramethylolpropane methane triacrylate Ester, trimethylolpropane trimethacrylate, tetramethylolmethane trimethacrylate, di-trimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, di-pentaerythritol hexaacrylate, di-pentaerythritol pentaacrylate, di-pentaerythritol pentaacrylate monopropionate, triacryloyl formal, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, stearyl methacrylate, hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, methoxyethyl methacrylate, butoxyethyl methacrylate, glycidyl methacrylate, cyclohexyl methacrylate) and the like.
[0048] Furthermore, cyclic unsaturated compounds (e.g., cyclohexene) and aromatic unsaturated compounds (e.g., styrene, α-methylstyrene, vinyltoluene, divinylbenzene, cyclohexene vinyl monoxide, divinylbenzene monoxide, vinyl acetate, vinyl propionate, allylbenzene, or diallylbenzene) may also be used. The aforementioned oligomer having one or more free radical polymerizable double bonds may be a polymer of these monomers.
[0049] In the method for producing the resin-adhering aluminum pigment according to the present embodiment described below, it is preferred to use a polymerization initiator.
[0050] The polymerization initiator is generally known as a radical generator, and the type thereof is not particularly limited.
[0051] Examples of the polymerization initiator include, but are not limited to, peroxides such as benzoyl peroxide, lauroyl peroxide, and bis-(4-tert-butylcyclohexyl)peroxydicarbonate; and azo compounds such as 2,2'-azobis-isobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, and 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile.
[0052] The amount of the polymerization initiator used is not particularly limited because it is adjusted according to the reaction rate of the radical polymerizable monomer, but is preferably 0.1 to 25 parts by mass based on 100 parts by mass of the aluminum pigment.
[0053] When the resin of the resin-attached aluminum pigment of the present embodiment described later is polymerized, it is preferred to add a polymerization initiator and a reversible addition-fragmentation chain transfer agent (hereinafter referred to as RAFT agent) to control the molecular weight of the reaction product, thereby performing living radical polymerization. This polymerization is superior in productivity compared to other living radical polymerizations from the viewpoints of (1) being applicable to a wide variety of monomers and (2) being applicable to a wide range of reaction conditions. Examples of the RAFT agent used to obtain the resin layer of the resin-adhered aluminum pigment of the present invention include, but are not limited to, dithiocarbonates such as O-ethyl-S-(1-phenylethyl)dithiocarbonate, O-ethyl-S-(2-propoxyethyl)dithiocarbonate, and O-ethyl-S-(1-cyano-1-methylethyl)dithiocarbonate; dithioesters such as cyanoethyl dithiopropionate, benzyl dithiopropionate, benzyl dithiobenzoate, and acetoxyethyl dithiobenzoate; dithiocarbamates such as S-benzyl-N,N-dimethyldithiocarbamate and benzyl-1-pyrrole dithiocarbamate; and trithiocarbonates such as dibenzyl trithiocarbonate and S-cyanomethyl-S-dodecyl trithiocarbonate. The RAFT agent used is preferably the most suitable RAFT agent according to the reactivity of the monomer. In particular, for the polymerization of acrylates, dithiocarbamates and dithiocarbonates are suitable, and for the polymerization of methacrylates, dithioesters are suitable. The RAFT agent is preferably used in an amount of 0.1 to 30 parts by weight, more preferably 1.0 to 10 parts by weight, relative to 100 parts by weight of the total amount of the resin. By setting it to 0.1 parts by weight or more, the tendency of the average molecular weight of the reaction product to increase can be suppressed, and by setting it to 30 parts by weight or less, the tendency of the average molecular weight of the reaction product to decrease can be suppressed.
[0054] As the solvent, it is not limited to the following examples. The organic solvent used for dispersing the metal pigment in the organic solvent can be inactive for the metal pigment, and examples thereof include aliphatic hydrocarbons such as hexane, heptane, octane, mineral spirits, aromatic hydrocarbons such as benzene, toluene, xylene, solvent naphtha, ethers such as tetrahydrofuran, diethyl ether, alcohols such as ethanol, 2-propanol, butanol, esters such as ethyl acetate, butyl acetate, glycols such as propylene glycol, ethylene glycol, glycol ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and glycol esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and ethylene glycol monomethyl ether acetate. These organic solvents can be used alone or in combination of two or more.
[0055] The amount used is preferably such that the solid content concentration of the metallic pigment becomes 1 to 40 wt%. It should be noted that in the present invention, the organic solvent is also used as a reaction solvent when the monomer and / or oligomer having one or more double bonds in the molecule is polymerized to form a resin.
[0056] When manufacturing resin-attached aluminum pigments, as external effects, the external effects of shear and vibration can be used in combination. The external effect of shear refers to the effect of adding high shear force to promote physical dispersion when the metal pigment is dispersed in an organic solvent and when the monomer is added to the dispersion. As a method for this, there is a method of dispersing the metal pigment and the monomer using a stirrer, a disperser, a vibration generator, and an ultrasonic generator. When a vibration generator or an ultrasonic generator is used, the above-mentioned dispersion or the slurry liquid in the polymerization reaction is mechanically vibrated strongly to produce an effect of promoting physical dispersion. In particular, high-speed dispersion using a stirrer is more preferred because it does not damage the surface of the vapor-deposited aluminum pigment.
[0057] The resin-coated aluminum pigment of the present invention is characterized in that, compared with conventional thin-film aluminum pigments, the resin-coated layer has high smoothness and thin-film formation, thereby maintaining high designability. It is believed that this is because the thin-film aluminum pigment forms a monodispersed state under high-speed stirring, and the molecular weight can be controlled in a low-molecular-weight state by RAFT polymerization, so that high smoothness and thin-film formation can be achieved. The uniformity can be evaluated by measuring the thickness τ and average surface roughness Ra of the resin layer of the resin-coated pigment.
[0058] The average surface roughness Ra of the resin layer surface of the resin-attached aluminum pigment of the present invention is preferably 0.1 to 5.0 nm, more preferably 0.1 to 4.5 nm, further preferably 0.1 to 2.6 nm, and most preferably 0.1 to 2.5 nm. Among them, the upper limit of the average surface roughness Ra is preferably the above-mentioned upper limit, more preferably 2.5 nm, further preferably 2.2 nm, and most preferably 2.0 nm. In addition, the lower limit of the average surface roughness Ra may be 0.3 nm, 0.5 nm, 0.7 nm, or 0.9 nm depending on the circumstances. When the average surface roughness Ra is below the above-mentioned upper limit, the regular reflectance of light on the surface of the coating film using the resin-attached aluminum pigment is large, so that extremely excellent brightness is exhibited and the angular heterochromaticity is also good.
[0059] The average surface roughness Ra referred to in the present invention can be calculated by a common surface morphology observation method using an atomic force microscope. Specifically, for example, it can be calculated by the following method.
[0060] As a method for observing the surface morphology of metallic pigments, an atomic force microscope (hereinafter referred to as AFM) (for example, Dimension Icon (manufactured by Bruker)) can be used. As a pretreatment, for example, the resin-attached aluminum pigment of the sample is ultrasonically cleaned with excess methanol and chloroform, vacuum dried, dispersed in acetone again, dripped onto a Si wafer, and naturally dried. For the quantification of surface roughness using AFM, for the case where the resin-coated metallic pigment does not overlap with other resin-coated metallic pigments, the measurement field of view is set to 2 μm and 512 pixels (pixel), and the measurement field of view is divided into 16 partitions. Each partition is subjected to three times of tilt correction (Plane Fit), and the value obtained by calculating the average is defined as the "average surface roughness Ra (nm)". The terminology for surface roughness is based on JIS-B-0601:2013.
[0061] In the resin-adhered aluminum pigment of the present invention, the thickness τ of the resin-adhered aluminum pigment measured by cross-sectional observation is preferably 5 to 30 nm, more preferably 10 nm to 20 nm. The upper limit of the thickness τ of the resin-adhered aluminum pigment is more preferably 18 nm, most preferably 16 nm. When the thickness τ of the resin-adhered aluminum pigment is within the above range, the pigment exhibits extremely excellent design properties, and the adhesion and chemical resistance also become good.
[0062] The average film thickness τ of the resin layer referred to in the present invention is calculated, for example, as follows. First, as a pretreatment, the resin-attached aluminum pigment is ultrasonically cleaned using excess methanol and chloroform, then vacuum dried, dispersed in acetone again for cleaning, and then naturally dried. It is then embedded with epoxy resin, and after complete curing, trimmed and sliced, and its cross section is observed using a transmission electron microscope (hereinafter referred to as TEM) to observe the interface between the resin covering layer and the aluminum pigment. Four fields of view are observed at 200,000 times for one field of view. For the area of the covering layer, the area is measured from the outline of the entire resin layer using known image analysis software (such as Image-ProPLUS ver.7.0 (manufactured by Media Cybernetics)). The arithmetic mean of these four fields of view is defined as [arithmetic mean film thickness τ].
[0063] (I) The mass of the resin per unit mass of the resin-attached aluminum pigment (A (g / g)) and the total surface area of the aluminum particles per unit mass of the resin-attached aluminum pigment (SSA (m 2 / g)) ratio ((A) / (SSA))
[0064] (1) Resin mass (A (g / g))
[0065] The mass of resin per unit mass of the resin-adhered aluminum pigment (A (g / g)) refers to a value obtained by calculating the mass (g) of the resin adhering to 1 g of the resin-adhered aluminum pigment.
[0066] The total surface area (SSA (m 2 / g) refers to the total area of 1g of aluminum particles (m 2 ).
[0067] The ratio (A) / (SSA) of the resin-attached aluminum pigment of the present invention is preferably 0.0077 g / m 2 ~0.025g / m 2 When the ratio (A) / (SSA) is within the above numerical range, the amount of resin relative to the aluminum particles becomes appropriate. When the ratio (A) / (SSA) is above the lower limit of the above numerical range, the decrease in alkali resistance is suppressed, and when it is below the upper limit of the above numerical range, the resin layer is easily controlled and the decrease in color tone is suppressed.
[0068] In the present invention, A (g / g) and SSA (m 2 / g) can be measured, for example, by the following method.
[0069] Weigh 1 g of the resin-attached aluminum pigment of the present invention in a 100 ml beaker, add 50 ml of petroleum benzene and fully disperse it, then heat it in a 40°C constant temperature water bath for 1 hour. Filter the heated dispersion and fully use acetone to wash it before recycling. Dry the solid sample obtained after filtration in a dryer for more than 90 minutes. Analyze a portion of the dried sample using thermogravimetric / differential thermal TG-DTA to determine the resin mass (A (g / g)) per unit mass of the resin-attached aluminum pigment.
[0070] SSA of aluminum particles (m 2 / g) is the total surface area per 1g of aluminum particles and is a value calculated by the following formula.
[0071] SSA(m 2 / g) = 2 × (0.4 / τ' (μm))
[0072] The above SSA(m 2 A method for calculating the molecular weight (MW) of the carbonyl group (g) is described in, for example, Aluminum Paint and Powder, JD Edwards & R.I. Wray, 3rd edition, Reinhold Publishing Corp. New York (1955), pages 16 to 22.
[0073] In addition, the resin-attached aluminum pigment of the present invention has improved chemical resistance in the coating film because the surface of the aluminum particles is more densely and uniformly covered with resin than the conventional aluminum pigment. When the color difference ΔE is obtained according to 6.3.19 of JIS-Z-8781 (2017), it is preferred that ΔE is less than 1.0 as the evaluation of chemical resistance.
[0074] The resin-bonded aluminum pigment of the present invention can be used in coatings and inks.
[0075] The coating containing the resin-attached aluminum pigment of the present invention can be suitably used for automobiles, general household appliances, information appliances represented by mobile phones, printing, and coating of metals such as iron and magnesium alloys, or plastics and the like, and can exhibit high design properties. The ink containing the resin-attached aluminum pigment of the present invention can be suitably used for metal coatings, printing inks, plastic kneading coatings, and the like, and can exhibit high design properties.
[0076] In addition, additives such as pigments, dyes, wetting agents, dispersants, anti-color difference agents, leveling agents, slip agents, rheology control agents, viscosity modifiers, anti-skinning agents, gelation inhibitors, defoamers, thickeners, anti-sagging agents, mildew inhibitors, ultraviolet absorbers, film-forming aids, surfactants, etc. commonly used in the coating industry can be appropriately added to the coating or ink containing the novel resin-attached aluminum pigment of the present invention.
[0077] Example
[0078] The following examples of the present invention are given to explain in detail. It should be noted that "%" in the following descriptions means weight %.
[0079] [Example 1]
[0080] Into a 1-liter four-necked flask, 100 g of a commercially available aluminum paste (SB-10 "average particle size 10 μm, nonvolatile content 74% by mass" manufactured by Asahi Kasei Corporation; aluminum particles of the present invention) was added, and 500 g of mineral spirits were added, and the mixture was stirred for 3 hours while bubbling nitrogen gas, and the temperature in the system was raised to 70°C. Then, 1.11 g of acrylic acid was added, and stirring was continued at 70°C for 30 minutes. Then, 7.83 g of trimethylolpropane trimethacrylate, 0.87 g of di-trimethylolpropane tetraacrylate, 2.0 g of 2,2'-azobis-2,4-dimethylvaleronitrile (polymerization initiator), 0.5 g of bis(dodecylsulfonylthiocarbonyl) disulfide (RAFT agent), and 50 g of mineral spirits were added dropwise over 1 hour (i.e., dropwise addition was adopted as the addition method, and the dropping time was set to 1 hour), and polymerization was carried out for a total of 8 hours while the temperature in the system was maintained at 70°C. The unreacted amount of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate in the filtrate sampled at this time was analyzed by gas chromatography, and the result showed that more than 99% of the added amount reacted. After the polymerization was completed, the treated slurry was filtered to obtain a resin-attached aluminum pigment. The heating residual component of the aluminum pigment (according to JIS-K-5910) was 56.1% by weight.
[0081] [Example 2]
[0082] In Example 1, a resin-adhering aluminum pigment was obtained in the same manner as in Example 1 except that 12.6 g of trimethylolpropane trimethacrylate and 0.14 g of di-trimethylolpropane tetraacrylate were used.
[0083] [Example 3]
[0084] In Example 1, a resin-adhering aluminum pigment was obtained in the same manner as in Example 1 except that the amount of mineral spirits was changed to 150 g.
[0085] [Example 4]
[0086] The method was changed to attach an ultrasonic disperser directly to the outside of the 1-liter four-necked flask used in Example 1 to apply ultrasonic waves to the slurry liquid inside. The ultrasonic disperser was used to irradiate ultrasonic waves with a frequency of 40 kHz and an output of 12 W during polymerization, and a resin-coated aluminum paste was obtained in the same manner as in Example 1. The nonvolatile content of the paste obtained in accordance with JIS-K-5910 was 50.1% by weight.
[0087] [Example 5]
[0088] In Example 1, the resin-attached aluminum pigment was obtained in the same manner as in Example 1 except that the content was changed to 100 g of aluminum paste (manufactured by Asahi Kasei Corporation, FD-5060 "average particle size 6 μm, non-volatile component 72% by mass"; aluminum particles of the present invention), 5.31 g of trimethylolpropane trimethacrylate, and 0.59 g of di-trimethylolpropane tetraacrylate.
[0089] [Example 6]
[0090] In Example 3, a resin-adhering aluminum pigment was obtained in the same manner as in Example 1 except that 10.62 g of trimethylolpropane trimethacrylate and 1.18 g of di-trimethylolpropane tetraacrylate were used.
[0091] [Example 7]
[0092] In Example 1, the resin-attached aluminum pigment was obtained in the same manner as in Example 1 except that the aluminum paste was changed to 100 g (BS-120 "average particle size 13 μm, non-volatile component 65 mass %" manufactured by Asahi Kasei Corporation; aluminum particles of the present invention), 4.95 g of trimethylolpropane trimethacrylate and 0.55 g of di-trimethylolpropane tetraacrylate.
[0093] [Example 8]
[0094] In Example 5, a resin-adhering aluminum pigment was obtained in the same manner as in Example 5 except that the amounts of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate were changed to 7.2 g.
[0095] [Example 9]
[0096] In Example 1, a resin-adhering aluminum pigment was obtained in the same manner as in Example 1 except that 6.83 g of trimethylolpropane trimethacrylate, 0.87 g of di-trimethylolpropane tetraacrylate, and 1.0 g of divinylbenzene were used.
[0097] [Example 10]
[0098] In Example 2, a resin-adhering aluminum pigment was obtained in the same manner as in Example 2 except that the dropping time was changed to 0.5 hours.
[0099] [Example 11]
[0100] In Example 2, a resin-adhering aluminum pigment was obtained in the same manner as in Example 2 except that the addition method was changed to all-at-once addition instead of dropwise addition.
[0101] [Comparative Example 1]
[0102] Into a 1-liter four-necked flask, 100 g of a commercially available aluminum paste (SB-10 "average particle size 10 μm, non-volatile component 74% by mass" manufactured by Asahi Kasei Corporation) was added, and 500 g of mineral spirits were added, and the mixture was stirred for 1 hour while bubbling nitrogen gas, and the temperature in the system was raised to 70°C. Then, 1.11 g of acrylic acid was added, and stirring was continued at 70°C for 30 minutes. Then, 12.6 g of trimethylolpropane trimethacrylate, 0.14 g of di-trimethylolpropane tetraacrylate, 2.0 g of 2,2'-azobis-2,4-dimethylvaleronitrile (polymerization initiator), and 50 g of mineral spirits were added dropwise over 1 hour using a metering pump (i.e., dropwise addition was adopted as the addition method, and the dropping time was set to 1 hour), and the temperature in the system was maintained at 70°C while polymerization was carried out for a total of 8 hours. During the polymerization reaction, a commercially available ultrasonic cleaning machine was used to indirectly irradiate the mixture in the four-necked flask with ultrasonic waves at a frequency of 42kHz and an output power of 180W for about 3 minutes every 15 minutes. The unreacted amount of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate in the filtrate sampled at this time was analyzed by gas chromatography, and the result showed that more than 99% of the added amount reacted. After the polymerization was completed, the treated slurry was filtered to obtain a resin-attached aluminum pigment. The heating residual component of the aluminum pigment (according to JIS-K-5910) was 55.6% by weight.
[0103] [Comparative Example 2]
[0104] In Comparative Example 1, a resin-adhering aluminum pigment was obtained in the same manner as in Comparative Example 1 except that the amounts of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate were changed to 7.83 g.
[0105] [Comparative Example 3]
[0106] In Comparative Example 1, a resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1 except that 100 g of aluminum paste (manufactured by Asahi Kasei Corporation, FD-5060 "average particle size 6 μm, nonvolatile content 72 mass %), 7.20 g of trimethylolpropane trimethacrylate, and 0.80 g of di-trimethylolpropane tetraacrylate were used.
[0107] [Comparative Example 4]
[0108] In Comparative Example 1, a resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1 except that 100 g of aluminum paste (BS-120 "average particle size 13 μm, nonvolatile content 65% by mass, manufactured by Asahi Kasei Corporation"), 4.95 g of trimethylolpropane trimethacrylate, and 0.55 g of di-trimethylolpropane tetraacrylate were used.
[0109] [Comparative Example 5]
[0110] In Comparative Example 1, a resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1 except that the dropping time was changed to 0.5 hours.
[0111] [Comparative Example 6]
[0112] In Comparative Example 1, a resin-adhering aluminum pigment was obtained in the same manner as in Comparative Example 5 except that the addition method was changed to all-at-once addition instead of dropwise addition.
[0113] [Evaluation 1 (resin mass (A (g / g)) and total surface area (SSA (m 2 / g)) ratio ((A) / (SSA)))]
[0114] (1) Resin mass (A (g / g))
[0115] Weigh 1 g of the resin-attached aluminum pigment obtained in the examples and comparative examples in a 100 ml beaker, add 50 ml of petroleum benzene and disperse thoroughly, then heat in a 40°C constant temperature water bath for 1 hour. Filter the heated dispersion and fully wash it with acetone before recycling. Dry the solid sample obtained after filtration in a dryer for more than 90 minutes. Analyze a portion of the dried sample using thermogravimetric / differential thermal TG-DTA to determine the resin mass (A (g / g)) per unit mass of the resin-attached aluminum pigment.
[0116] (2) Total surface area of aluminum particles (SSA (m 2 / g))
[0117] Defined as (the total surface area of aluminum particles SSA (m 2 / g) = 2 × (0.4 / τ' (μm))
[0118] The average thickness τ' (μm) can be determined by measuring using an FE-SEM image of a coating film cross section described later and using image analysis software.
[0119] [Evaluation 2 (Measurement of Average Particle Size d50 of Aluminum Particles)]
[0120] The average particle size (d50) of the aluminum particles was measured using a laser diffraction / scattering particle size distribution analyzer (LA-300 / Horiba, Ltd.).
[0121] Mineral spirits were used as a measurement solvent.
[0122] The measurement was carried out according to the operating manual of the machine. As a precaution, the aluminum particles used as the sample were subjected to ultrasonic dispersion for 2 minutes as a pretreatment, then placed in a dispersion tank, and the measurement was started after confirming that an appropriate concentration was reached.
[0123] After the measurement is completed, d50 is automatically displayed.
[0124] [Evaluation 3 (Measurement of Average Cross-Section Thickness τ' of Aluminum Particles)]
[0125] (1) Production of coated panels
[0126] Using the aluminum pigments obtained in Examples and Comparative Examples, metallic base paints were prepared with the following composition.
[0127] Aluminum pigment: 2g
[0128] Thinner (Musashi Paint Co., Ltd., trade name "PLA-ACE Thinner No. 2726"): 50 g
[0129] Acrylic resin (manufactured by Musashi Paint Co., Ltd., trade name "PLA-ACE No. 7160"): 33 g
[0130] The above-mentioned coating material was applied to an ABS resin plate using an air spray device so as to have a dry film thickness of 20 μm, and dried in an oven at 60° C. for 30 minutes to obtain a metal-based coated plate.
[0131] A topcoat paint having the following composition was applied to the above-mentioned metal base coated plate using an air spray device.
[0132] Hitaloid Varnish 3685S (made by Hitachi Chemical): 25g
[0133] Mixed diluent (solvent mixing ratio / toluene: 45 mass%, butyl acetate: 30 mass%, ethyl acetate: 20 mass%, 2-acetoxy-1-methoxypropane: 5 mass%): 20 g
[0134] ·Duranate TPA100 (manufactured by Asahi Kasei Chemicals Corporation): 5g
[0135] After the above-mentioned painting, the panels were dried in an oven at 60° C. for 30 minutes to obtain painted panels for evaluation.
[0136] (2) Cross-section preparation of coating film
[0137] Using the coated plate for evaluation produced as described above, a coating film cross section was prepared by the following procedure.
[0138] The above-mentioned evaluation coated plate was cut into 2 cm squares using scissors.
[0139] The cross section of the coating film was repeatedly cut with a large rotary slicer (RV-240 manufactured by Yamato Koki Kogyo) to remove the minute aluminum and acrylic resin protruding from the cross section.
[0140] The coating cross section obtained in the above was subjected to ion milling treatment using an ion milling device (IB-09010CP manufactured by JEOL Ltd.) set so that the ion beam could be irradiated to a portion 20 μm away from the coating cross section, thereby preparing a coating cross section for obtaining a FE-SEM image described below.
[0141] (3) Obtaining particle cross-section (FE-SEM image)
[0142] The coating film cross section (coated plate) obtained in ((2) Preparation of coating film cross section) was bonded to the SEM sample stage in a parallel manner, and a FE-SEM image of the coating film cross section was obtained using a field emission FE-SEM (manufactured by HITACHI / S-4700).
[0143] Regarding the conditions for FE-SEM observation / acquisition, the acceleration voltage was set to 5.0 kV, and the measurement was performed at an image magnification of 10,000 times.
[0144] In addition, before obtaining (capturing) the FE-SEM image, an electronic axis alignment process is performed so that no deformation occurs at the boundary line between the aluminum particles and the acrylic resin in the FE-SEM image.
[0145] (4) Analysis (measurement of average thickness of particles in particle cross section)
[0146] Using the FE-SEM image (magnification 10,000) obtained by the above-mentioned particle cross-section (FE-SEM image) acquisition steps ((1) to (3)) and image analysis software Win Roof version 5.5 (manufactured by MITANI CORPORATION), the thickness of the particles in the cross-section of the aluminum particles was measured and the average thickness was calculated.
[0147] The FE-SEM image of the aluminum particle thickness measurement in the cross section is displayed, and the ROI line is selected so that the ROI line matches the 5 μm scale of the image and is set by registering / changing the input length / unit.
[0148] Next, an image of the cross section of the aluminum particle to be measured for thickness is displayed, a rectangular ROI is selected, and binary processing is performed so that the rectangular ROI fits the cross section of the particle.
[0149] Next, after selecting the measurement item of the vertical chord length to be measured, the measurement is performed, and the automatically measured value (vertical chord length value) obtained by the image analysis software is displayed on the image.
[0150] Thus, using the aforementioned image analysis software Win Roof version 5.5, 100 particles within ±50% of the average particle size: d50 described later [(IV) Average particle size: d50] are selected, and the thickness in the cross section of the aluminum particles is automatically measured. The arithmetic mean of the 100 particles is calculated to find the average cross-sectional thickness τ' of the particles.
[0151] [Evaluation 4 (Measurement of Average Film Thickness τ on the Surface of Resin-Adhered Aluminum Pigment)]
[0152] First, as a pretreatment, the resin-coated metal pigment is ultrasonically cleaned with excess methanol and chloroform, then vacuum dried, dispersed in acetone again for cleaning, and then dried naturally. Then, it is embedded with epoxy resin, and after complete curing, it is trimmed and sliced, and its cross section is observed using a transmission electron microscope (hereinafter referred to as TEM) to observe the surface unevenness of the resin coating layer. Four fields of view are observed with a field of view of 1 μm wide. For the area of the coating layer, the image analysis software Image-ProPLUS ver.7.0 (manufactured by Media Cybernetics) is used to detect the overall outline of the resin layer, measure the area, and find the arithmetic mean of these four fields of view as τ.
[0153] [Evaluation 5 (Measurement of Average Surface Roughness Ra of Resin-Adhered Aluminum Pigment Surface)]
[0154] The line profile (300 scans) of a 4 μm square in one field of view of the resin-coated metallic pigment was obtained using an atomic force microscope (AFM). The area was divided into 16 sections, and tilt correction was performed three times to obtain the arithmetic mean surface roughness. The same operation was performed for a total of 4 or more fields of view, and their arithmetic mean was obtained and set as Ra.
[0155] [Evaluation 6 (Evaluation of Adhesion and Chemical Resistance of Coating Film)]
[0156] Using the resin-adhered aluminum pigments obtained in Examples 1 to 9 and Comparative Examples 1 to 6, metallic coatings were prepared with the following compositions.
[0157] Resin-attached aluminum pigment: 1.3 g (solid content mass)
[0158] Diluent (a mixture of 30 parts of butyl acetate, 45 parts of toluene, 20 parts of isopropyl alcohol, and 5 parts of ethyl cellosolve): (D) g (here, the total amount of the resin-adhered aluminum pigment and (D) was adjusted to 33 g.)
[0159] · Transparent resin (ACRYDIC A-166 (DIC): 29 parts, nitrocellulose (industrial nitrocellulose 1 / 2AS, Companhia Nitro Qumica Brasileira): 3 parts, the above diluent: 68 parts) (binder resin component): 42 g
[0160] The obtained coating composition was sprayed and applied to an ABS resin plate so as to have a film thickness of 15 μm, and then dried at 55° C. for 30 minutes to prepare a coated plate for evaluation.
[0161] Adhesion, chemical resistance, and gloss retention were evaluated using the above-mentioned coated panels for evaluation.
[0162] (Adhesion of coating film)
[0163] Using the coated plate prepared above, Sellotape (registered trademark: CT405AP-18 manufactured by Nichiban Co., Ltd.) was placed in close contact with the coating film and pulled at an angle of 45 degrees to visually observe the degree of peeling of the metal pigment particles. The results of the observation were evaluated as follows.
[0164] ○(Good): No peeling
[0165] △ (Pass): Slight peeling
[0166] × (Unqualified): Peeling occurs
[0167] (Chemical resistance of coating film)
[0168] The lower half of the coated plate prepared above was immersed in a beaker containing a 2.5N NaOH aqueous solution and placed at 23°C for 24 hours. After the coated plate was washed and dried, the color of the immersed and unimmersed parts was measured according to condition d (8-d method) of JIS-Z-8722 (1982), and the color difference ΔE was obtained according to 6.3.2 of JIS-Z-8730 (1980). The evaluation was performed as follows based on the value of the color difference ΔE. (The smaller the value, the better.)
[0169] ○(Good): Less than 1.0
[0170] △(Pass): 1.0 or more and less than 2.0
[0171] ×(Unqualified): 2.0 or above
[0172] [Evaluation 7: FF properties (brightness, glossiness) and hiding power of coating film]
[0173] (1) Production of coated panels
[0174] Using the resin-adhered aluminum pigments obtained in Examples 1 to 11 and Comparative Examples 1 to 6, metallic coatings were prepared with the following compositions.
[0175] Resin-attached aluminum pigment: 5.0g
[0176] · Thinner (manufactured by Kansai Paint Co., Ltd., trade name "ACRYDIC 2000GL"): 13.0 g
[0177] Acrylic resin (manufactured by Kansai Paint Co., Ltd., trade name "ACRYDIC 2000"): 97.0 g
[0178] Next, the metal base coating was applied to the PET film using a 3 mil applicator and dried at room temperature for 30 minutes to obtain a metal base coating plate.
[0179] (2) Determination of ΔF / F property (brightness, brilliance)
[0180] The coating film formed by applying the above-mentioned coating to a PET sheet was evaluated using an angle colorimeter (manufactured by Suga Test Instruments Co., Ltd.). The incident angle was set to 45 degrees, and the light receiving angle of 15 degrees (L15) close to the regular reflection light and the light receiving angle of 60 degrees (L60) close to the base color, except for the light reflected in the mirror reflection area on the coating film surface of the above-mentioned evaluation plate, were measured. The ratio (L15 / L60) was taken as the FF property.
[0181] (3) Determination of covering properties
[0182] Covering
[0183] Specifically, the prepared coatings were prepared using a reference aluminum paste and a resin-coated aluminum paste, and two coated plates were pulled on a PET sheet and irradiated with light from the uncoated surface to evaluate the hiding power.
[0184] (Baseline aluminum paste pigment is the aluminum pigment before resin coating)
[0185] ◎: Has hiding power equivalent to that of the standard aluminum paste pigment.
[0186] ○: The hiding power is slightly lower than that of the standard aluminum paste pigment.
[0187] △: The hiding power is low compared to the standard aluminum paste pigment.
[0188] ×: The hiding power is significantly reduced compared to the standard aluminum paste pigment.
[0189] The results of evaluations 1 to 7 are shown in Table 1.
[0190] [Table 1]
[0191]
[0192] a) Raw aluminum paste ①, raw aluminum paste ②, and raw aluminum paste are "Asahi Kasei Corporation aluminum paste, SB-10" (used in Examples 1 to 4, 6, 9 to 11, and Comparative Examples 1, 2, 5, and 6), "Asahi Kasei Corporation aluminum paste, FD-5060" (used in Examples 5, 8, and Comparative Example 3), and "Asahi Kasei Corporation aluminum paste, BS-120" (used in Example 7 and Comparative Example 4), respectively.
Claims
1. A resin-attached aluminum pigment, wherein the surface of aluminum particles is covered with a resin containing a polymer of a monomer and / or an oligomer having one or more free radical polymerizable double bonds, and the average surface roughness Ra of the resin layer surface of the resin-attached aluminum pigment is 0.1 to 5.0 nm.
2. The resin-adhered aluminum pigment according to claim 1, wherein The thickness τ of the resin adhesion layer measured by cross-sectional observation is 10 nm to 20 nm.
3. A resin-attached aluminum pigment, wherein the surface of aluminum particles is covered with a resin containing a polymer of a monomer and / or oligomer having one or more free radical polymerizable double bonds, and the thickness τ of the resin attachment layer measured by cross-sectional observation is 10 nm to 20 nm.
4. The resin-adhered aluminum pigment according to claim 1, wherein The ratio of the resin mass A per unit mass of the resin-attached aluminum pigment to the total surface area SSA per unit mass of the aluminum particles, i.e., (A) / (SSA) is 0.0077 g / m 2 ~0.025g / m 2 , wherein the unit of the resin mass A per unit mass of the resin-attached aluminum pigment is g / g, and the unit of the total surface area SSA per unit mass of the aluminum particles is m 2 / g.
5. The resin-adhered aluminum pigment according to claim 1, wherein The average cross-sectional thickness τ' of the aluminum particles is 0.03 μm to 0.2 μm.
6. The resin-adhered aluminum pigment according to claim 5, wherein The average particle size d50 of the aluminum particles is 5 μm to 15 μm. 7 . A coating material comprising the resin-adherent aluminum pigment according to claim 1 . 8 . An ink comprising the resin-adherent aluminum pigment according to claim 1 .
Citation Information
Patent Citations
Novel aluminum pigment
JP2002226733A
Aluminum pigment
WO1999054074A1
Resin coated aluminum pigment
WO2018047360A1