Metal horn cover cap coating for automotive trim and preparation method of metal horn cover cap coating

By using a combination of high solid content and moderate hydroxyl acrylic resin with high solid content and low viscosity resin in automotive interior metal horn cover coatings, combined with specific solvents and stirring steps, the paint is solved in the surface area of ​​aluminum alloy paint and spreading of aluminum alloys. The problem of poor performance achieves excellent adhesion and weather resistance, and meets the humidity and heat resistance needs of the metal horn cover of the car interior.

CN119019898AInactive Publication Date: 2024-11-26HUIZHOU BESTER CHEM CO LTD

Patent Information

Application Number
CN202411071769.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When used on the surface of aluminum alloy, existing automotive interior metal horn cover paint is prone to paint accumulation problems and poor corrosion resistance, and poor spreadability on the porous substrate, which cannot meet the needs of weather resistance and humidity resistance.

Method used

Using a combination of hydroxyacrylic resin with a solid content of 48-52 wt%, a hydroxyl value of 25-30 KOHmg/g and a high solid content low viscosity resin, combined with ethyl acetate and butyl acetate as solvent, through specific stirring steps and components The proportion is to adjust the viscosity and adhesion of the coating to ensure excellent adhesion after spraying, weather resistance and moisture and heat resistance.

Benefits of technology

Solve the problem of no gap collection after spraying the horn cover paint on the metal horn mesh cover, improve the spreadability and leveling of the paint, significantly improve adhesion and weather resistance, and have good moisture resistance and water vapor resistance. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981069620000061
    Figure BDA0004981069620000061
  • Figure BDA0004981069620000071
    Figure BDA0004981069620000071
Patent Text Reader

Abstract

The invention discloses a metal horn cover cap coating for automotive trim. The metal horn cover cap coating is prepared from the following raw materials in parts by weight: 45-65 parts of hydroxy acrylic resin, 1-10 parts of matting powder, 1-5 parts of a light stabilizer, 0.1-0.5 part of a flatting agent, 0.1-0.5 part of a wetting agent and 25-45 parts of a solvent. The hydroxy acrylic resin with the solid content of 48-52 wt% and the hydroxyl value of 25-30 KOHmg / g and the hydroxy acrylic resin with the high solid content and low viscosity are mixed and matched, the prepared coating can be applied to the metal horn mesh enclosure, the problem that paint is collected in gaps of the mesh enclosure after spraying is avoided, and the scraping resistance is good. And the spraying effect on the metal horn cover is excellent, the adhesive force is good, and good weather resistance, heat and humidity resistance and water vapor resistance are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a metal horn cover coating for automobile interior and a preparation method thereof, and relates to C09D, and in particular to the field of coating combinations of polymer compounds. Background Art

[0002] As people's living standards improve, the number of family cars is increasing. In order to reduce the boredom of drivers and passengers during the journey, audio devices are increasingly used in cars. As people's requirements become higher and higher, in order to improve the use effect of audio devices, improving the timbre, operation and shockproof functions of audio devices are the goals that technical R&D personnel are constantly pursuing. In order to make the audio devices in cars have the advantages of weather resistance, water vapor resistance, and humidity and heat resistance, audio devices are generally made of plastic materials, but the horn of plastic parts has a certain influence on the timbre and cannot play the timbre effect of normal audio. Therefore, replacing the material of the audio device with aluminum alloy can significantly improve the timbre effect of the device, but metal audio devices are easily corroded, and the use of conventional anti-corrosion coatings will cause paint accumulation problems on the speaker cover, and the brushing effect is not good. Therefore, it is very important to develop a weather-resistant coating suitable for mobile speaker covers.

[0003] Chinese invention patent CN201710183691.7 discloses a UV-curing coating for aluminum alloy surface and its preparation method. By comprehensively utilizing UV resin, photoinitiator, dispersant, defoamer, leveling agent, adhesion promoter, anti-settling agent, active monomer, matting powder and filler and other ingredients, the prepared UV-curing coating has good adhesion and excellent curing performance when used on aluminum alloy surface. However, it is not resistant to shock and weathering. Chinese invention patent CN201911391893.6 discloses a bottom-to-top color matching coating and its preparation method. It is a composite color masterbatch component, a light-reducing resin component, a high-gloss resin component and a curing agent component. It has excellent adhesion on a variety of substrates and also has the functions of sealing, isolation, moisture-proof and mildew-proof of the primer, but the leveling and spreading properties on the substrate with holes are not good. Summary of the invention

[0004] In order to develop a coating for metal horn cover with excellent weather resistance, water vapor resistance, and heat and humidity resistance, the first aspect of the present invention provides a metal horn cover coating for automobile interior. The raw materials for preparation include, by weight: 45-65 parts of hydroxyl acrylic resin, 1-10 parts of matting powder, 1-5 parts of light stabilizer, 0.1-0.5 parts of leveling agent, 0.1-0.5 parts of wetting agent, and 25-45 parts of solvent.

[0005] As a preferred embodiment, the raw materials for preparation include, by weight: 50-60 parts of hydroxy acrylic resin, 3-8 parts of matting powder, 1-3 parts of light stabilizer, 0.2-0.4 parts of leveling agent, 0.1-0.3 parts of wetting agent, and 30-40 parts of solvent.

[0006] As a preferred embodiment, the raw materials for preparation include, by weight: 55 parts of hydroxy acrylic resin, 5 parts of matting powder, 1.5 parts of light stabilizer, 0.3 parts of leveling agent, 0.2 parts of wetting agent, and 38 parts of solvent.

[0007] As a preferred embodiment, the hydroxy acrylic resin includes hydroxy acrylic resin A and hydroxy acrylic resin B, and the weight ratio of the hydroxy acrylic resin A to the hydroxy acrylic resin B is (20-30): (20-30).

[0008] As a preferred embodiment, the weight ratio of the hydroxy acrylic resin A to the hydroxy acrylic resin B is (27-29): (26-28).

[0009] As a preferred embodiment, the weight ratio of the hydroxy acrylic resin A to the hydroxy acrylic resin B is 28:27.

[0010] As a preferred embodiment, the solid content of the hydroxy acrylic resin B is 43-58 wt %, and the hydroxy value is 20-35 KOH mg / g.

[0011] As a preferred embodiment, the solid content of the hydroxy acrylic resin B is 48-52 wt %, and the hydroxy value is 25-30 KOH mg / g.

[0012] As a preferred implementation, the model of the hydroxy acrylic resin A is Japan Mitsubishi LR-7721; the model of the hydroxy acrylic resin B is Japan Mitsui OLESTER Q850.

[0013] As a preferred embodiment, the average particle size of the matting powder is 1-5 μm, and the specific surface area of ​​the matting powder is 100-200 m 2 / g.

[0014] As a preferred embodiment, the average particle size of the matting powder is 1.5 μm, and the specific surface area of ​​the matting powder is 150 m 2 / g.

[0015] As a preferred embodiment, the light stabilizer is selected from one or a combination of benzotriazole stabilizers, benzophenone stabilizers, triazine stabilizers, and hindered amine stabilizers.

[0016] As a preferred embodiment, the light stabilizer is a combination of a benzotriazole stabilizer and a hindered amine stabilizer, and the weight ratio of the benzotriazole stabilizer to the hindered amine stabilizer is (1-3): (0.1-0.8).

[0017] As a preferred embodiment, the model of the benzotriazole stabilizer is Tinuvin1130; the model of the hindered amine stabilizer is Tinuvin292.

[0018] As a preferred embodiment, the weight ratio of the benzotriazole stabilizer to the hindered amine stabilizer is (1-2): (0.3-0.7).

[0019] As a preferred embodiment, the weight ratio of the benzotriazole stabilizer to the hindered amine stabilizer is 1:0.5.

[0020] As a preferred embodiment, the solvent is selected from one or a combination of ethyl acetate, butyl acetate, methyl acetate, ethyl formate, isobutyl acetate, isoamyl formate, and methyl propionate.

[0021] As a preferred embodiment, the solvent is a combination of ethyl acetate and butyl acetate, and the weight ratio of ethyl acetate to butyl acetate is (10-20): (20-30).

[0022] As a preferred embodiment, the weight ratio of ethyl acetate to butyl acetate is (13-18):(21-25).

[0023] As a preferred embodiment, the weight ratio of ethyl acetate to butyl acetate is 15:23.

[0024] The applicant found in the experiment that the coating prepared by mixing a hydroxyl acrylic resin with a solid content of 48-52wt% and a hydroxyl value of 25-30KOHmg / g with a high solid content and low viscosity hydroxyl acrylic resin can be applied to metal speaker meshes. After spraying, there will be no problem of paint gathering in the mesh gaps, and the coating has good spreadability and leveling properties on the mesh. The resulting coating has good weather resistance, resistance to moisture, heat and water vapor. The possible reason is that there are many holes on the metal speaker mesh. If the coating is sprayed on the mesh with holes, the surface tension of the coating will cause paint gathering at the edges of the holes, and the edges of the holes will be protruding, and the mesh will have an uneven appearance after spraying. By adjusting the solid content to 48-52wt%, the hydroxyl acrylic resin with a hydroxyl value of 25-30KOHmg / g and the high solid content, low viscosity hydroxyl acrylic resin Japan Mitsubishi LR-7721 to (25-30): (25-30), a balance between spreadability and leveling can be achieved, and there will be no paint collection problem during spraying, and the coating has excellent adhesion to the metal mesh, and has good weather resistance and resistance to moisture and hot water vapor.

[0025] A second aspect of the present invention provides a method for preparing a metal horn cover coating for automobile interior, comprising the following steps:

[0026] S1: 5-15 parts by weight of butyl acetate and hydroxy acrylic resin are mixed, stirred at 500-600 rpm for 10-15 min until uniform, matting powder is added, and stirred at 800-1000 rpm for 45-60 min to obtain mixture A;

[0027] S2: Mix the light stabilizer and part of the solvent, and stir at 500-600 rpm for 10-15 min until the mixture is uniform, to obtain a mixture B;

[0028] S3: Add mixture B into mixture A, add leveling agent and wetting agent in sequence at a speed of 800-1000 rpm, stir for 10-15 minutes, adjust the viscosity to 8.5-9.5s with the remaining solvent, and filter through a 400-mesh filter.

[0029] The viscosity of 8.5-9.5s is the viscosity obtained by Iwata No. 2 cup test at 25°C.

[0030] As a preferred embodiment, part of the solvent in step S2 is a combination of 1-3 parts by weight of butyl acetate and 0.5-1 parts by weight of ethyl acetate, and the remaining solvent in step S3 is a combination of 15-20 parts by weight of butyl acetate and 13-15 parts by weight of ethyl acetate.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The metal horn cover coating for automobile interior of the present invention is a mixture of a hydroxyl acrylic resin having a solid content of 48-52wt% and a hydroxyl value of 25-30KOHmg / g and a hydroxyl acrylic resin having a high solid content and a low viscosity. The prepared coating can be applied to a metal horn grille without the problem of paint accumulation in the gaps of the grille after spraying, and has good scratch resistance.

[0033] (2) In the coating for the metal horn cover for automobile interior of the present invention, the weight ratio of hydroxyl acrylic resin A and hydroxyl acrylic resin B is (27-29): (26-28), which can balance the spreadability and leveling properties of the coating, has excellent spraying effect on the metal horn cover, good adhesion, and good weather resistance, moisture and heat resistance, and water vapor resistance.

[0034] (3) The metal horn cover coating for automobile interior of the present invention adopts a solvent combination of ethyl acetate and butyl acetate, and uses part of the solvent to first dissolve part of the raw materials, and then uses the remaining solvent to adjust the viscosity. The obtained coating has good shear force and can be dispersed at a high speed. The coating has excellent dispersibility and compatibility. DETAILED DESCRIPTION

[0035] Example 1

[0036] A metal horn cover coating for automobile interior decoration, wherein the raw materials for preparation include, by weight, 55 parts of hydroxy acrylic resin, 5 parts of matting powder, 1.5 parts of light stabilizer, 0.3 parts of leveling agent, 0.2 parts of wetting agent and 38 parts of solvent.

[0037] The hydroxy acrylic resin includes hydroxy acrylic resin A and hydroxy acrylic resin B, with a weight ratio of 28:27.

[0038] The model of the hydroxyl acrylic resin A is Japanese Mitsubishi LR-7721; the solid content of the hydroxyl acrylic resin B is 48-52wt%, the hydroxyl value is 25-30KOHmg / g, and the model is Japanese Mitsui OLESTER Q850.

[0039] The average particle size of the matting powder is 1.5 μm, and the specific surface area of ​​the matting powder is 150 m 2 / g, purchased from Tosoh E-1011.

[0040] The light stabilizer is a combination of a benzotriazole stabilizer and a hindered amine stabilizer, with a weight ratio of 1:0.5.

[0041] The model of the benzotriazole stabilizer is Tinuvin1130; the model of the hindered amine stabilizer is Tinuvin292.

[0042] The model of the leveling agent is BYK333, and the model of the wetting agent is EFKA3777.

[0043] The solvent is a combination of ethyl acetate and butyl acetate in a weight ratio of 15:23.

[0044] A method for preparing a metal horn cover coating for automobile interior, comprising the following steps:

[0045] S1: 2.3 parts by weight of butyl acetate and hydroxy acrylic resin were mixed, stirred at 550 rpm for 15 min until uniform, matting powder was added, and stirred at 900 rpm for 60 min to obtain mixture A;

[0046] S2: Mix the light stabilizer and part of the solvent, and stir at 550 rpm for 15 min until uniform, to obtain a mixture B;

[0047] S3: Add mixture B into mixture A, add leveling agent and wetting agent in sequence at 900 rpm, stir for 15 minutes, adjust the viscosity to 8.5-9.5s with the remaining solvent, and filter through a 400-mesh filter.

[0048] The viscosity of 8.5-9.5s is the viscosity obtained by Iwata No. 2 cup test at 25°C.

[0049] The partial solvent in step S2 is a combination of 1.15 parts by weight of butyl acetate and 0.75 parts by weight of ethyl acetate, and the remaining solvent in step S3 is a combination of 19.55 parts by weight of butyl acetate and 14.25 parts by weight of ethyl acetate.

[0050] Comparative Example 1

[0051] A metal horn cover coating for automobile interior and a preparation method thereof, the specific implementation method is the same as that of Example 1, except that the Japanese Mitsui OLESTER Q850 in Example 1 is replaced with an equivalent amount of DSM (DSM) 7120S-60.

[0052] Comparative Example 2

[0053] A metal horn cover coating for automobile interior and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that the Japanese Mitsubishi LR-7721 in Example 1 is replaced by DIC's ACRYDIC AU-7206 in equal amounts.

[0054] Performance Testing

[0055] The spraying process of the coating of Example 1 and Comparative Examples 1 and 2 comprises the following steps:

[0056] An aluminum alloy speaker cover is prepared, phosphated, dusted, and spray-painted (film thickness 15-20 μm, curing temperature 75-80° C., curing time 100 min).

[0057] The following method was used to test the results after spray painting. The test results are shown in Table 1.

[0058] Table 1

[0059]

[0060]

Claims

1. A metal horn cover coating for automobile interior, characterized in that: The raw materials for preparation include, by weight: 45-65 parts of hydroxy acrylic resin, 1-10 parts of matting powder, 1-5 parts of light stabilizer, 0.1-0.5 parts of leveling agent, 0.1-0.5 parts of wetting agent and 25-45 parts of solvent.

2. The metal horn cover coating for automobile interior according to claim 1, characterized in that: The hydroxy acrylic resin includes hydroxy acrylic resin A and hydroxy acrylic resin B, and the weight ratio of the hydroxy acrylic resin A to the hydroxy acrylic resin B is (20-30): (20-30).

3. The metal horn cover coating for automobile interior according to claim 2, characterized in that: The solid content of the hydroxy acrylic resin B is 43-58 wt %, and the hydroxy value is 20-35 KOH mg / g.

4. The metal horn cover coating for automobile interior according to claim 2, characterized in that: The average particle size of the matting powder is 1-5 μm, and the specific surface area of ​​the matting powder is 100-200 m 2 / g.

5. The metal horn cover coating for automobile interior according to claim 2, characterized in that: The light stabilizer is selected from one or a combination of benzotriazole stabilizers, benzophenone stabilizers, triazine stabilizers, and hindered amine stabilizers.

6. The metal horn cover coating for automobile interior according to claim 5, characterized in that: The light stabilizer is a combination of a benzotriazole stabilizer and a hindered amine stabilizer, and the weight ratio of the benzotriazole stabilizer to the hindered amine stabilizer is (1-3): (0.1-0.8).

7. The metal horn cover coating for automobile interior according to claim 2, characterized in that: The solvent is selected from one or a combination of ethyl acetate, butyl acetate, methyl acetate, ethyl formate, isobutyl acetate, isoamyl formate, and methyl propionate.

8. The metal horn cover coating for automobile interior according to claim 7, characterized in that: The solvent is a combination of ethyl acetate and butyl acetate, and the weight ratio of ethyl acetate to butyl acetate is (10-20):(20-30).

9. A method for preparing a metal horn cover coating for automobile interior decoration according to any one of claims 7-8, characterized in that: The following steps are involved: S1: 1-5 parts by weight of butyl acetate and hydroxy acrylic resin are mixed, stirred at 500-600 rpm for 10-15 min until uniform, matting powder is added, and stirred at 800-1000 rpm for 45-60 min to obtain mixture A; S2: Mix the light stabilizer and part of the solvent, and stir at 500-600 rpm for 10-15 min until the mixture is uniform, to obtain a mixture B; S3: Add mixture B into mixture A, add leveling agent and wetting agent in sequence at a speed of 800-1000 rpm, stir for 10-15 minutes, adjust the viscosity to 8.5-9.5s with the remaining solvent, and filter through a 400-mesh filter.

10. The method for preparing the metal horn cover coating for automobile interior according to claim 9, characterized in that: Part of the solvent in step S2 is a combination of 1-3 parts by weight of butyl acetate and 0.5-1 parts by weight of ethyl acetate, and the remaining solvent in step S3 is a combination of 15-20 parts by weight of butyl acetate and 13-15 parts by weight of ethyl acetate.

Citation Information

Patent Citations

  • Double-component ground coating matched with ultraviolet (UV) coating for coating notebook computer plastic case

    CN102977756A

Cited By

  • Preparation method of anti-ultraviolet weather-resistant water-based paint

    CN120536034A

  • Loudspeaker mesh local shielding paint spraying system and paint spraying process thereof

    CN121820085A