Organosilicon pressure-sensitive adhesive suitable for hardened coating film protection, and preparation method and application thereof

By combining silicone modified boric acid ester and vinyl silicone oil and other components, silicon pressure-sensitive adhesive suitable for hardened coating film protection was prepared, which solved the film tearing force and silicon transfer problems of hardened coating film, realizing the Improve stability and smoothness.

CN119019979AActive Publication Date: 2024-11-26WANHUA CHEM GRP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310580436.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

The tearing force of the existing hardened coating film is easy to climb and the silicon transfers more, which affects the experience of end customers and cannot meet the needs of flexible screen protectors.

Method used

Using silicone modified boric acid ester combined with vinyl silicone oil, crosslinking agent, anchoring agent and catalyst, a silicone pressure-sensitive adhesive suitable for hardened coating film protection is prepared, through crosslinking reaction and intermolecular action Force, achieve stable film tearing force and low silicon transfer.

Benefits of technology

The stability of the tearing force in the range of 1 to 4g/inch is achieved, with low silicon transfer, and does not affect the smoothness of the hardened coating film, improving the experience of end customers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004241467510000131
    Figure BDA0004241467510000131
  • Figure BDA0004241467510000132
    Figure BDA0004241467510000132
  • Figure BDA0004241467510000141
    Figure BDA0004241467510000141
Patent Text Reader

Abstract

The invention discloses an organic silicon pressure-sensitive adhesive suitable for protecting a hardened coating film, and a preparation method and application thereof, and belongs to the technical field of organic silicon pressure-sensitive adhesive materials.According to the organic silicon pressure-sensitive adhesive, organic silicon modified boric acid ester is adopted and matched with vinyl silicone oil, a cross-linking agent, an anchoring agent and a catalyst to achieve protection of the hardened coating film; the film tearing force is stable and does not climb, the silicon transfer degree is low, and the smoothness of the hardened coating film is not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic silicon pressure-sensitive adhesive protective films, and in particular to an organic silicon pressure-sensitive adhesive suitable for protecting a hardened coating film, a preparation method and an application thereof. Background Art

[0002] 3D curved screen and folding screen mobile phones are increasingly favored by the market. Screen protectors for their flexible displays are indispensable, and the protection of bare screens is extremely important. Conventional screen protector substrates are usually based on polyethylene terephthalate (PET), thermoplastic polyurethane (TPU) and polyimide (PI), which have poor surface scratch resistance and no anti-fingerprint effect. At present, the mainstream choice on the market is to coat a layer of colorless transparent hardened coating (HC) film of about 1 to 3 um on the surface of the conventional base film to meet the application requirements of flexible screen protectors.

[0003] The main body of the conventional hard coating is a polyurethane-modified acrylic system, and a fluorine-containing additive is added to improve the anti-scratch and smoothness performance of the HC liquid, and then it is coated on the conventional base film and cured by UV light to form an HC film. This type of hard coating film has good hardness and can provide adequate protection for the underlying conventional base film, optical transparent adhesive and flexible bare screen.

[0004] Before the above-mentioned 3D screen mobile phone is shipped to the terminal market, a layer of protective film is required to protect the upper layer of the HC film. This protective film is mainly a layer of acrylic or silicone pressure-sensitive adhesive coated on the PET film, which can have a certain peeling force on the HC film (generally 1 to 4 g / inch) and cannot affect the smoothness of the HC film itself. Conventional acrylic pressure-sensitive adhesives have increased peeling force when attached to HC films, and noise occurs when the film is torn off, which affects the experience of end customers; while silicone pressure-sensitive adhesives have stable peeling force, but they themselves have certain silicon transfer, which will reduce the smoothness of the HC film itself and also cannot meet the needs of end customers. Therefore, there is an urgent need for a silicone pressure-sensitive adhesive suitable for the protection of hardened coating films to solve the problems existing in the above-mentioned prior art. Summary of the invention

[0005] The purpose of the present invention is to provide a silicone pressure-sensitive adhesive suitable for protecting a hardened coating film. By synthesizing a silicone-modified borate ester and combining it with vinyl silicone oil, the hardened coating film can be protected. The film tearing force is stable and does not increase, the degree of silicon transfer is low, and the smoothness of the hardened coating film itself is not affected.

[0006] Another object of the present invention is to provide a method for preparing the organic silicone pressure-sensitive adhesive suitable for protecting the hardened coating film.

[0007] Another object of the present invention is to provide an application of the organic silicone pressure-sensitive adhesive suitable for protecting a hardened coating film.

[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:

[0009] A silicone pressure-sensitive adhesive suitable for protecting a hardened coating film comprises vinyl silicone oil, silicone-modified boric acid ester, a crosslinking agent, an anchoring agent and a catalyst.

[0010] In the present invention, the vinyl silicone oil component is obtained by uniformly stirring the following raw materials in a reaction kettle:

[0011] 40-60 parts by weight of vinyl silicone oil A, 15-25 parts by weight of vinyl silicone oil B, 20-40 parts by weight of vinyl silicone oil C and 0.1-0.3 parts by weight of ethynyl cyclohexanol.

[0012] Among them, the viscosity of vinyl silicone oil A is 9000-11000 mPa·s, and the vinyl content is 0.12-0.16 wt%; the viscosity of vinyl silicone oil B is 54000-66000 mPa·s, and the vinyl content is 0.08-0.10 wt%; the viscosity of vinyl silicone oil C is 1000-1100 mPa·s, and the vinyl content is 0.21-0.25 wt%.

[0013] In the present invention, the organosilicon-modified borate component is obtained by reacting the following raw materials in a vacuum distillation reactor:

[0014] 5 to 10 parts by weight of triallyl borate, 4 to 8 parts by weight of tri(methacrylateethyl) borate and 5 to 9 parts by weight of tri(acrylateethyl) borate; and 40 to 80 parts by weight of dimethylisopropylsilane.

[0015] In the present invention, the crosslinking agent component is a hydrogen polysiloxane having a hydrogen content of 0.95-1.05%; preferably, the structure of the hydrogen polysiloxane as the crosslinking agent component is (CH 3 ) 3 SiO[(CH 3 ) 2 SiO] m [(CH 3 )(H)SiO] n Si(CH 3 ) 3 , where m is a natural number greater than or equal to 0 and less than 3, and n is a natural number greater than or equal to 0.

[0016] In the present invention, the anchoring agent component is a hydrogen polysiloxane containing one or more of an epoxy group, an ether group, and an acyl group; preferably, the hydrogen polysiloxane as the anchoring agent component has a specific structure of (R 1 )(CH 3 ) 2SiO[(CH 3 )(H)SiO] k [(CH 3 )(X)SiO] j Si(CH 3 ) 2 (R 2 ), where R 1 and R 2 is an alkyl group or H, X is an epoxy group, an ether group or an acyloxy group, k and j are both natural numbers, and 1≤k≤7, 1≤j≤4.

[0017] In the present invention, the catalyst component is a platinum catalyst formed by coordination of platinum and divinyltetramethyldisiloxane, wherein the platinum content is 4000-6000ppm.

[0018] In the present invention, the dosage of each component is as follows: 100 parts of vinyl silicone oil component, 6-12 parts of organosilicon-modified borate component, 1.4-1.6 parts of crosslinking agent component, 0.8-1.2 parts of anchoring agent component, and -1.2-1.4 parts of catalyst component, calculated by weight.

[0019] On the other hand, the present invention also provides a method for preparing the aforementioned organic silicone pressure-sensitive adhesive suitable for hardening coating film protection, comprising the following steps:

[0020] 1) preparing an organosilicon-modified borate component: adding 5 to 10 parts by weight of triallyl borate, 4 to 8 parts by weight of tri(methacrylate-ethyl) borate and 5 to 9 parts by weight of tri(acrylate-ethyl) borate to a vacuum distillation reactor, stirring evenly, and then mixing in 40 to 80 parts by weight of dimethylisopropylsilane, stirring, and obtaining an organosilicon-modified borate component;

[0021] 2) preparing a vinyl silicone oil component: adding 40 to 60 parts by weight of vinyl silicone oil A, 15 to 25 parts by weight of vinyl silicone oil B, 20 to 40 parts by weight of vinyl silicone oil C and 0.1 to 0.3 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature, to obtain a vinyl silicone oil component;

[0022] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 9-12 minutes, then add 6-12 parts of organosilicon-modified borate component, 1.4-1.6 parts of crosslinking agent component, 0.8-1.2 parts of anchoring agent component while stirring, stir for 10 minutes, finally add 1.2-1.4 parts of catalyst component, stir after all are added to obtain the final pressure-sensitive adhesive bath;

[0023] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution is coated on the PET film, and then placed in an oven for curing to obtain a silicone pressure-sensitive adhesive film suitable for hardening the coating film protection.

[0024] In the present invention, the stirring temperature in step 1) is 80-120° C., and the stirring time is 4-6 hours; the stirring time at room temperature in step 2) is 4-6 hours; the stirring time in step 3) is 14-16 minutes; the temperature of the oven in step 4) is 145-155° C., and the curing time is 1.5-2 minutes.

[0025] On the other hand, the aforementioned organosilicon pressure-sensitive adhesive suitable for hardening coating film protection or the organosilicon pressure-sensitive adhesive prepared by the aforementioned method is preferably used in the field of electronic protective films for hardening coating film protection applications.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) The tearing force of the silicone pressure-sensitive adhesive of the present invention on the colorless transparent hardened coating (HC) film is controllable. By changing the addition amount of the silicone-modified borate component, the tearing force is stabilized in the range of 1 to 4 g / inch. Generally, if the tearing force is less than 1 g / inch, there is a risk of the silicone pressure-sensitive adhesive film and the HC film falling off. If the tearing force is greater than 4 g / inch, the film tearing feels heavy, which affects the end customer's experience of film tearing.

[0028] 2) The silicone pressure-sensitive adhesive of the present invention has a low degree of silicon transfer to the colorless transparent hardened coating (HC) film, so that the smoothness of the HC film itself will not be affected; conventional silicone pressure-sensitive adhesives use MQ resin as a tackifier. MQ resin is an inert mixture with a wide molecular weight distribution range. It is inevitable that small molecular siloxane molecules will migrate to the surface of the HC film, thereby reducing the smoothness of the HC film.

[0029] 3) In the present invention, three vinyl silicone oils with different vinyl structures are used in combination with a crosslinking agent (hydrogen-containing silicone oil) component to achieve stable peeling force; the vinyl positions and vinyl contents of the three vinyl silicone rubbers are different, providing active sites for multiple crosslinking reactions in space, thereby achieving a higher crosslinking density. After adding the silicone tackifier, the peeling force will tend to be stable, and the peeling force will not increase due to high-temperature baking and room temperature storage time.

[0030] 5) In the present invention, a special organosilicon-modified borate component is synthesized as a tackifier for the organosilicon pressure-sensitive adhesive to increase the peeling force, while at the same time avoiding the silicon transfer caused by the conventional MQ resin as a tackifier; the aforementioned organosilicon-modified borate component has a vinyl functional group, which reacts with the cross-linking agent (hydrogen-containing silicone oil) to avoid silicon transfer as much as possible; the borate structure forms an intermolecular force with the polar groups on the surface of the HC film to achieve a certain range of tackification effect. DETAILED DESCRIPTION

[0031] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0032] The present invention is further explained below by more specific examples, but does not constitute any limitation.

[0033] In each example, unless otherwise specified, all parts are by weight; for the convenience of expression, the sources of the main raw materials used in each example and comparative example are as follows:

[0034] Vinyl silicone oil A: Hesheng HS-10000, viscosity 9000-11000mPa·s, vinyl mass fraction 0.12-0.16%, volatile matter ≤1.5%;

[0035] Vinyl silicone oil B: Hesheng HS-60000, viscosity 54000-66000mPa·s, vinyl mass fraction 0.08-0.10%, volatile matter ≤1.5%;

[0036] Vinyl silicone oil C: Runhe RH-Vi305B, viscosity 1000mPa·s, vinyl mass fraction 0.21-0.25%, volatile matter ≤1%;

[0037] Triallyl borate: Aladdin, analytical grade;

[0038] Tri(methacrylateethyl) borate: Aladdin, analytical grade

[0039] Tri(acrylated ethyl) borate: Aladdin, analytical grade

[0040] Dimethylisopropylsilane: Aladdin, analytical grade

[0041] Ethynyl cyclohexanol: Aladdin, analytical grade;

[0042] Ethyl acetate: Aladdin, analytical grade;

[0043] Cross-linking agent: Runhe, RH510;

[0044] Anchoring agent: Tianqi New Materials, SK-M02 or SK-M03;

[0045] Catalyst: Heraeus, platinum content 5000ppm.

[0046] Embodiment 1:

[0047] 1) Preparation of organosilicon-modified borate component:

[0048] 5 parts by weight of triallyl borate, 8 parts by weight of tri(methacrylateethyl) borate and 7 parts by weight of tri(acrylateethyl) borate were added to a vacuum distillation reactor, stirred evenly, and then 80 parts by weight of dimethylisopropylsilane was added and stirred at 80° C. for 6 hours to obtain an organosilicon-modified borate component;

[0049] 2) preparing a vinyl silicone oil component: adding 40 parts by weight of vinyl silicone oil A, 20 parts by weight of vinyl silicone oil B, 40 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 4 hours, to obtain a vinyl silicone oil component;

[0050] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 6 parts of organosilicon-modified borate component, 1.5 parts of cross-linking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0051] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 1.

[0052] Embodiment 2:

[0053] 1) Preparation of organosilicon-modified borate component:

[0054] 10 parts by weight of triallyl borate, 4 parts by weight of tri(methacrylateethyl) borate and 6 parts by weight of tri(acrylateethyl) borate were added to a vacuum distillation reactor, stirred evenly, and then 80 parts by weight of dimethylisopropylsilane was added and stirred at 100° C. for 5 hours to obtain an organosilicon-modified borate component;

[0055] 2) preparing a vinyl silicone oil component: adding 60 parts by weight of vinyl silicone oil A, 15 parts by weight of vinyl silicone oil B, 25 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 6 hours, to obtain a vinyl silicone oil component;

[0056] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, 120 parts of ethyl acetate are added and stirred for 10 minutes, then 8 parts of organosilicon-modified borate component, 1.5 parts of cross-linking agent component, 1.0 part of anchoring agent component are added while stirring, and stirred for 10 minutes, and finally 1.3 parts of catalyst component are added, and stirred for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath solution;

[0057] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 1.

[0058] Embodiment 3:

[0059] 1) Preparation of organosilicon-modified borate component:

[0060] 7 parts by weight of triallyl borate, 8 parts by weight of tri(methacrylateethyl) borate and 5 parts by weight of tri(acrylateethyl) borate were added to a vacuum distillation reactor, stirred evenly, and then 80 parts by weight of dimethylisopropylsilane was added and stirred at 120° C. for 4 hours to obtain an organosilicon-modified borate component;

[0061] 2) preparing a vinyl silicone oil component: adding 55 parts by weight of vinyl silicone oil A, 25 parts by weight of vinyl silicone oil B, 20 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 6 hours, to obtain a vinyl silicone oil component;

[0062] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 10 parts of organosilicon-modified borate component, 1.5 parts of cross-linking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0063] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 1.

[0064] Embodiment 4:

[0065] 1) Preparation of organosilicon-modified borate component:

[0066] 5 parts by weight of triallyl borate, 6 parts by weight of tri(methacrylateethyl) borate and 9 parts by weight of tri(acrylateethyl) borate were added to a vacuum distillation reactor, stirred evenly, and then 80 parts by weight of dimethylisopropylsilane was added and stirred at 120° C. for 5 hours to obtain an organosilicon-modified borate component;

[0067] 2) preparing a vinyl silicone oil component: adding 50 parts by weight of vinyl silicone oil A, 20 parts by weight of vinyl silicone oil B, 30 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 5 hours, to obtain a vinyl silicone oil component;

[0068] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 12 parts of organosilicon-modified borate component, 1.5 parts of cross-linking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0069] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 1.

[0070] Comparative Example 1:

[0071] 1) Silicone MQ resin (similar to the above-mentioned silicone-modified borate component):

[0072] The methyl MQ organosilicon tackifier has a solid content of 75%, and the structural formula of the methyl MQ organosilicon tackifier is [(CH 3 ) 3 SiO 1 / 2 ] a [SiO 4 / 2 ] c ; where [(CH 3 ) 3 SiO 1 / 2 ] a is the M unit, [SiO 4 / 2 ] c The ratio of M unit to Q unit is a / c value of 0.6-0.8; the bulk density of the powder is 0.2-0.3g / cm 3 ; Molecular weight is 4000-6000; Average particle size is 90-110μm; Hydroxyl content ≤0.5;

[0073] 2) preparing a vinyl silicone oil component: adding 40 parts by weight of vinyl silicone oil A, 20 parts by weight of vinyl silicone oil B, 40 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 5 hours, to obtain a vinyl silicone oil component;

[0074] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 6 parts of silicone MQ resin, 1.5 parts of crosslinking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0075] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 2.

[0076] Comparative Example 2:

[0077] 1) Silicone MQ resin (similar to the above-mentioned silicone-modified borate component):

[0078] The methyl MQ organosilicon tackifier has a solid content of 75%, and the structural formula of the methyl MQ organosilicon tackifier is [(CH 3 ) 3 SiO 1 / 2 ] a [SiO 4 / 2 ] c ; where [(CH 3 ) 3 SiO 1 / 2 ] a is the M unit, [SiO 4 / 2 ] c The ratio of M unit to Q unit is a / c value of 0.6-0.8; the bulk density of the powder is 0.2-0.3g / cm 3 ; Molecular weight is 4000-6000; Average particle size is 90-110μm; Hydroxyl content ≤0.5;

[0079] 2) preparing a vinyl silicone oil component: adding 50 parts by weight of vinyl silicone oil A, 20 parts by weight of vinyl silicone oil B, 30 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 6 hours, to obtain a vinyl silicone oil component;

[0080] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 12 parts of organosilicon MQ resin, 1.5 parts of crosslinking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0081] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 2.

[0082] Comparative Example 3

[0083] 1) Preparation of organosilicon-modified borate component:

[0084] 7 parts by weight of triallyl borate, 8 parts by weight of tri(methacrylateethyl) borate and 5 parts by weight of tri(acrylateethyl) borate were added to a vacuum distillation reactor, stirred evenly, and then 80 parts by weight of dimethylisopropylsilane was added and stirred at 120° C. for 4 hours to obtain an organosilicon-modified borate component;

[0085] 2) preparing a vinyl silicone oil component: adding 60 parts by weight of vinyl silicone oil A, 40 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 6 hours, to obtain a vinyl silicone oil component;

[0086] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 10 parts of tributyl borate, 1.5 parts of cross-linking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0087] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 2.

[0088] Comparative Example 4

[0089] 1) Directly use tributyl borate;

[0090] 2) preparing a vinyl silicone oil component: adding 55 parts by weight of vinyl silicone oil A, 25 parts by weight of vinyl silicone oil B, 20 parts by weight of vinyl silicone oil C and 0.22 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature for 6 hours, to obtain a vinyl silicone oil component;

[0091] 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 10 minutes, then add 10 parts of tributyl borate, 1.5 parts of cross-linking agent component, 1.0 part of anchoring agent component while stirring, stir for 10 minutes, finally add 1.3 parts of catalyst component, stir for 15 minutes after all are added to obtain the final pressure-sensitive adhesive bath;

[0092] 4) Curing of the pressure-sensitive adhesive: The prepared bath solution was coated on a 50 um PET film, and then placed in a 150°C oven for curing for 1.5 minutes to obtain a final pressure-sensitive adhesive protective film; the HC film was attached for performance testing, and its performance parameters are shown in Table 2.

[0093] The performances tested in the above Examples 1-4 and Comparative Examples 1-4 are:

[0094] 1. Film tearing force test: The pressure-sensitive adhesive tape (pressure-sensitive adhesive thickness of 10um) coated on the PET film and fully cured is laminated with the HC film, and then cut into a standard test piece with a width of 25.4mm and a length of 300mm. The test piece is aged at room temperature for 1 day / 7 days and at 70℃ for 1 day / 7 days. During the test, the pressure-sensitive adhesive tape is peeled 180° upward (peeling speed is 300mm / min). The test result is the film tearing force. The test environment is 23±2℃ and 50±5% RH.

[0095] 2. Low silicon transfer test: The smoothness of the HC film surface is tested by a friction coefficient tester (equipment model: YH-9819, test standard: GB 10006-88). The test results are expressed as dynamic friction coefficient U d It is presented to characterize the degree of silicon transfer of the pressure-sensitive adhesive tape to the HC film; where: U d The smaller the value, the smoother the HC film surface is, indicating that the degree of silicon transfer is lower. Generally, the initial U d The value is about 0.10. After the pressure-sensitive tape is attached, the U d A value of ≤0.3 indicates a low degree of silicon transfer, which meets the technical requirements for HC film protection).

[0096] The performance test results of Examples 1-4 in Table 1 are as follows:

[0097]

[0098] Table 2 Performance test results of Comparative Examples 1-4 are as follows:

[0099]

[0100]

[0101] In summary:

[0102] It can be seen from Examples 1, 2, 3, and 4 that the silicone pressure-sensitive adhesive of the present invention combined with three vinyl silicone oils with different vinyl contents and positions can achieve controllable tearing force for HC films, and by changing the addition amount of the silicone-modified borate component, the tearing force can be stabilized at 1 to 2 g / inch (Examples 1 and 2) and 2 to 4 g / inch (Examples 3 and 4), and the peeling force of room temperature time tracking and high temperature aging tracking has almost no increase or attenuation.

[0103] It can be seen from Examples 1, 2, 3, and 4 that the degree of silicon transfer of the silicone pressure-sensitive adhesive of the present invention to the colorless transparent hardened coating (HC) film is low, which is much lower than the dynamic friction U d The upper limit of the value (≤0.3) will not affect the smoothness of the HC film itself.

[0104] It can be seen from Comparative Examples 1 and 2 that the tearing force of the conventional organosilicon pressure-sensitive adhesive tackifier (MQ resin) increases more significantly at room temperature and high temperature than the organosilicon-modified borate component shown herein, and more importantly, the dynamic friction coefficient is much higher than the dynamic friction coefficient U d The upper limit of the value (≤0.3) directly affects the smoothness of the HC film.

[0105] It can be seen from Comparative Examples 3 and 4 that: when only two vinyl silicone oils are stirred into a vinyl silicone oil component and n-butyl borate is used as a viscosity-increasing component, the degree of increase in the tearing force under room temperature aging and high temperature aging is much higher than that of Examples 1, 2, 3, and 4.

[0106] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A silicone pressure-sensitive adhesive suitable for protecting a hardened coating film, comprising vinyl silicone oil, a silicone-modified boric acid ester, a crosslinking agent, an anchoring agent and a catalyst; the silicone-modified boric acid ester component is obtained by reacting the following raw materials in a vacuum distillation reactor: 5 to 10 parts by weight of triallyl borate, 4 to 8 parts by weight of tri(methacrylateethyl) borate and 5 to 9 parts by weight of tri(acrylateethyl) borate; and 40 to 80 parts by weight of dimethylisopropylsilane.

2. The organic silicone pressure-sensitive adhesive according to claim 1, characterized in that: The vinyl silicone oil component is obtained by uniformly stirring the following raw materials in a reaction kettle: 40-60 parts by weight of vinyl silicone oil A, 15-25 parts by weight of vinyl silicone oil B, 20-40 parts by weight of vinyl silicone oil C and 0.1-0.3 parts by weight of ethynyl cyclohexanol; Preferably, the viscosity of vinyl silicone oil A is 9000-11000 mPa·s, and the vinyl content is 0.12-0.16 wt%; the viscosity of vinyl silicone oil B is 54000-66000 mPa·s, and the vinyl content is 0.08-0.10 wt%; the viscosity of vinyl silicone oil C is 1000-1100 mPa·s, and the vinyl content is 0.21-0.25 wt%.

3. The organic silicone pressure-sensitive adhesive according to claim 1 or 2, characterized in that: The crosslinking agent component is a hydrogen polysiloxane having a hydrogen content of 0.95-1.05%; preferably, the structure of the hydrogen polysiloxane as the crosslinking agent component is (CH3)3SiO[(CH3)2SiO] m [(CH3)(H)SiO] n Si(CH3)3, wherein m is a natural number greater than or equal to 0 and less than 3, and n is a natural number greater than or equal to 0.

4. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The anchoring agent component is a hydrogen polysiloxane containing one or more of an epoxy group, an ether group, and an acyl group; preferably, the hydrogen polysiloxane as the anchoring agent component has a specific structure of (R1)(CH3)2SiO[(CH3)(H)SiO] k [(CH3)(X)SiO] j Si(CH3)2(R2), wherein R1 and R2 are alkyl or H, X is epoxy, ether or acyloxy, k and j are both natural numbers, and 1≤k≤7, 1≤j≤4.

5. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 4, characterized in that: The catalyst component is a platinum catalyst formed by coordination of platinum and divinyltetramethyldisiloxane, wherein the platinum content is 4000-6000ppm.

6. The organic silicone pressure-sensitive adhesive according to any one of claims 1 to 5, characterized in that: In terms of weight, the dosage of each component is: 100 parts of vinyl silicone oil component, 6-12 parts of organosilicon-modified borate component, 1.4-1.6 parts of crosslinking agent component, 0.8-1.2 parts of anchoring agent component, and 1.2-1.4 parts of catalyst component.

7. A method for preparing an organic silicone pressure-sensitive adhesive suitable for hardening coating film protection as claimed in any one of claims 1 to 6, comprising the following steps: 1) preparing an organosilicon-modified borate component: adding 5 to 10 parts by weight of triallyl borate, 4 to 8 parts by weight of tri(methacrylate-ethyl) borate and 5 to 9 parts by weight of tri(acrylate-ethyl) borate to a vacuum distillation reactor, stirring evenly, and then mixing in 40 to 80 parts by weight of dimethylisopropylsilane, stirring, and obtaining an organosilicon-modified borate component; 2) preparing a vinyl silicone oil component: adding 40 to 60 parts by weight of vinyl silicone oil A, 15 to 25 parts by weight of vinyl silicone oil B, 20 to 40 parts by weight of vinyl silicone oil C and 0.1 to 0.3 parts by weight of ethynyl cyclohexanol to a reaction kettle in sequence, stirring at room temperature, to obtain a vinyl silicone oil component; 3) Preparation of pressure-sensitive adhesive: 100 parts of vinyl silicone oil component, add 120 parts of ethyl acetate and stir for 9-12 minutes, then add 6-12 parts of organosilicon-modified borate component, 1.4-1.6 parts of crosslinking agent component, 0.8-1.2 parts of anchoring agent component while stirring, stir for 10 minutes, finally add 1.2-1.4 parts of catalyst component, stir after all are added to obtain the final pressure-sensitive adhesive bath; 4) Curing of the pressure-sensitive adhesive: The prepared bath solution is coated on the PET film, and then placed in an oven for curing to obtain a silicone pressure-sensitive adhesive film suitable for hardening the coating film protection.

8. The preparation method according to claim 7, characterized in that: The stirring temperature in step 1) is 80-120° C. and the stirring time is 4-6 hours; and / or, the stirring time at room temperature in step 2) is 4-6 hours; and / or, the stirring time in step 3) is 14-16 minutes; and / or, the temperature of the oven in step 4) is 145-155° C. and the curing time is 1.5-2 minutes.

9. Use of the organosilicon pressure-sensitive adhesive suitable for hardening coating film protection as described in any one of claims 1 to 6 or the organosilicon pressure-sensitive adhesive suitable for hardening coating film protection prepared by the preparation method as described in any one of claims 7 to 8 in the field of electronic protective films, preferably suitable for hardening coating film protection applications.

Citation Information

Patent Citations

  • Boron silane modified silicon resin, addition type resin composition and application

    CN105524281A

  • Organic silicon pressure sensitive adhesive and pressure sensitive adhesive tape or film

    CN106753195A

  • Boron-containing organosilicone tackifier in linear structure and preparation method thereof

    CN109824899A

  • High-AF screen adhesive force organosilicon pressure-sensitive adhesive suitable for TPU film general curing, preparation method and application of high-AF screen adhesive force organosilicon pressure-sensitive adhesive

    CN114196374A

  • Anti-fingerprint glass organic silicon pressure-sensitive adhesive as well as preparation method and application thereof

    CN114854367A