High-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material and preparation method thereof

By regulating the components and process of TiNbAlCr high-entropy alloys, high-strength plastic TiNbAlCr materials with high intensity and excellent gamma ray shielding performance were prepared, which solved the shortcomings of existing gamma ray shielding materials in terms of mechanical properties and achieved high efficiency gamma ray shielding and structural stability.

CN119020656APending Publication Date: 2024-11-26XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136899.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing gamma-ray shielding materials have shortcomings in mechanical properties, especially plasticity, and their heat resistance and structural properties are poor, which limits their promotion and use.

Method used

By regulating the component elements and molar ratio of TiNbAlCr high-entropy alloys, the element mixing effect and lattice distortion effect are enhanced, and combined with specific smelting processes and homogenization treatment, a body-center cubic structure with room temperature yield strength is prepared with a room temperature of no less than 800MPa, high-strength plastic TiNbAlCr high-entropy alloy gamma shielding material with plasticity of no less than 14%.

Benefits of technology

It significantly improves the strong plasticity and gamma-ray shielding performance of the alloy, ensures the high strength of the material, excellent gamma-shielding performance and structural stability, and solves the problem of insufficient mechanical properties of existing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020656A_ABST
    Figure CN119020656A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material and a preparation method thereof, the material is recorded as TiaNbbAlcCrd according to the molar ratio of each component element, a is more than or equal to 20 and less than or equal to 60, b is more than or equal to 20 and less than or equal to 50, c is more than or equal to 1 and less than or equal to 30, d is more than or equal to 1 and less than or equal to 30, and a + b + c + d is equal to 100; the method comprises the following steps: 1, removing impurities from raw material elemental metal, cleaning, proportioning and weighing; 2, smelting the weighed raw materials; and 3, carrying out homogenization treatment. According to the high-entropy alloy and the preparation method thereof, the element mixing effect and the lattice distortion effect of the high-entropy alloy are enhanced by regulating and controlling the composition elements and the molar ratio of the high-entropy alloy, and the high plasticity and the gamma ray shielding performance of the high-entropy alloy material are improved; by optimizing a raw material smelting process and combining a high-temperature homogenization treatment process, volatilization of elements is avoided, the component stability and the element uniformity of the material are improved, and the gamma ray shielding performance and the high-strength plastic performance of the material are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high entropy alloy processing, and specifically relates to a high-strength and plastic TiNbAlCr high entropy alloy gamma shielding material and a preparation method thereof. Background Art

[0002] With the development of aerospace, nuclear technology and other fields and the widespread use of nuclear energy, higher requirements are placed on the performance of nuclear radiation shielding materials. Neutrons and gamma rays produced in nuclear reactions have strong penetrating power and are more harmful, so the research on neutron and gamma radiation shielding materials has become the focus of radiation protection research. Materials composed of high atomic numbers have good shielding effects, so tungsten (W), lead and rare earth elements are often used as shielding materials.

[0003] With the development of nuclear energy, the performance requirements of gamma-ray shielding materials are getting higher and higher. The materials should not only have excellent shielding performance, but also have good mechanical properties, heat resistance and radiation resistance. Although the addition of W and rare earth elements can improve the shielding performance of alloy materials, the presence of a large number of low-plasticity intermetallic compounds in the material reduces its plastic processing and forming performance, and its heat resistance and structural properties are not good, which seriously limits the promotion and use of the shielding material. As a new type of multi-principal alloy material, high entropy alloy has high strength, high plasticity, excellent corrosion resistance, high temperature softening resistance and unique radiation resistance of the matrix, making it a potential gamma-ray irradiation shielding material.

[0004] Therefore, a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material and a preparation method thereof are needed. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material in view of the deficiencies of the above-mentioned prior art. The material enhances the element mixing effect and lattice distortion effect of the high-entropy alloy, strengthens the solid solution strengthening effect of the alloy, improves the strength and plasticity and gamma-ray shielding performance of the TiVCrNb high-entropy alloy, and solves the problem of poor mechanical properties, especially plasticity, of existing gamma-ray shielding materials by regulating the constituent elements and molar ratio of the TiVCrNb high-entropy alloy.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material, characterized in that the high-entropy alloy gamma-ray shielding material is recorded as follows according to the molar ratio of each component element: Ti a Nb b Al c Cr d, wherein 20≤a≤60, 20≤b≤50, 1≤c≤30, 1≤d≤30, and a+b+c+d=100; the physical phase of the high entropy alloy gamma shielding material is a body-centered cubic structure, the yield strength at room temperature is not less than 800MPa, and the plasticity is not less than 14%.

[0007] The present invention significantly reduces the activation performance of the high entropy alloy by adding low-activation elements Ti and Cr, and the presence of the Ti element makes the alloy have excellent plasticity; at the same time, the addition of the brittle Cr element improves the strength of the alloy, ensuring that the alloy has excellent strong-plastic matching performance, and the addition of the high-density refractory metal Nb element significantly improves the gamma-ray shielding performance of the alloy; in addition, the addition of the Al element, which has a large difference in atomic radius from other elements, further strengthens the lattice distortion effect and solid solution strengthening effect of the high entropy alloy, so that the alloy has excellent strong-plasticity and gamma-ray shielding performance.

[0008] The above-mentioned high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material is characterized in that the high-entropy alloy gamma-ray shielding material is recorded as follows according to the molar ratio of each component element: Ti a Nb b Al c Cr d , where 22≤a≤58, 22≤b≤48, 2≤c≤28, 2≤d≤28, and a+b+c+d=100.

[0009] The above-mentioned high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material is characterized in that the high-entropy alloy gamma-ray shielding material is recorded as follows according to the molar ratio of each component element: Ti a Nb b Al c Cr d , where a=45, b=45, c=5, d=5.

[0010] In the preferred composition molar ratio of the material of the present invention, the plastic Ti element ensures the ductility of the high entropy alloy, the Cr element significantly enhances the strength of the high entropy alloy, the Al element strengthens the strong plasticity of the alloy, and the Nb element improves the gamma shielding effect of the alloy, thereby ensuring the high strength-plasticity and excellent gamma shielding performance of the high entropy alloy.

[0011] At the same time, the present invention also discloses a method for preparing the high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material as described above, characterized in that the method comprises the following steps:

[0012] Step 1: remove surface impurities from the single metals of Ti, Nb, Al and Cr and wash them in anhydrous ethanol, then weigh the washed raw materials according to the component design of the target product;

[0013] Step 2: placing the raw materials weighed in step 1 into a vacuum arc melting furnace for melting to obtain an alloy ingot;

[0014] Step 3: Place the alloy ingot obtained in step 2 into a vacuum annealing furnace for homogenization to obtain a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material.

[0015] In the preparation process of the high entropy alloy gamma shielding material of the present invention, the single metal surfaces of the raw materials Ti, Nb, Al and Cr are firstly removed from impurities and cleaned, and then placed in a vacuum arc melting furnace in order for melting, and then subjected to homogenization treatment to obtain the TiNbAlCr high entropy alloy gamma shielding material. In this process, firstly, the impurities on the surface of the raw materials are removed to purify the impurity gas in the vacuum arc melting furnace, thereby improving the purity of the alloy; then, by controlling the placement order of each raw material, the volatilization of low melting point elements is avoided, the stability of the alloy components is ensured, and the diffusion effect of the alloy elements is accelerated in combination with the homogenization treatment, the element uniformity of the alloy is improved, the structural stability of the alloy is ensured, and the strong plasticity and gamma shielding properties of the TiVCrNb high entropy alloy material are further enhanced.

[0016] The above method is characterized in that the mass purity of the single metals of Ti, Nb, Al and Cr in step 1 is not less than 99.8%, and the single metals of Ti, Nb, Al and Cr are all in block or granular form; the surface impurities are removed by sandpaper or a grinder. The present invention reduces the influence of gaseous element impurities such as C, N, and O on the structure and performance of the alloy by controlling the purity of the metal raw materials and the surface impurity removal process of the raw materials, ensures the purity of the alloy, and is conducive to improving the structure and performance stability of the high entropy alloy.

[0017] The above method is characterized in that the weighed raw materials in step 2 are placed in the following order: firstly, the Al single metal is placed at the bottom of the crucible in the vacuum arc melting furnace, and then the Ti, Nb and Cr single metals are mixed and placed on top of the Al single metal. The present invention places the Al raw material with a low melting point under the crucible, avoids direct contact between the arc and the Al raw material during melting, prevents the volatilization of the Al element, and ensures the stability of the alloy composition.

[0018] The above method is characterized in that, during the smelting in step 2, a small current of 70A to 110A is first used to melt the single metal mixture of Ti, Nb, and Cr at the top of the crucible and wrap the single metal of Al at the bottom, and then the current is increased to 140A to 200A for overturning smelting. The present invention first uses a small current to melt the single metal mixture of Ti, Nb, and Cr, thereby avoiding the arc gas flow caused by the initial current being too large to roughly splash the single metal mixture of Ti, Nb, and Cr out of the crucible, and melts the single metal mixture of Ti, Nb, and Cr and wraps the single metal of Al at the bottom, thereby preventing the loss of low-melting-point Al raw materials caused by the subsequent current increase, and further ensuring the stability of the alloy composition.

[0019] The above method is characterized in that the homogenization process in step 3 is: heating to 900°C to 1300°C under vacuum conditions for 2h to 48h of heat treatment, and then cooling with the furnace. The homogenization treatment in the present invention can accelerate the migration and diffusion between atoms of each element in the alloy, enhance the distribution uniformity of the high entropy alloy components, and improve the structural stability and mechanical properties of the high entropy alloy.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. The present invention enhances the element mixing effect and lattice distortion effect of the high entropy alloy, strengthens the solid solution strengthening effect of the alloy, and improves the strength and plasticity and gamma-ray shielding performance of the TiVCrNb high entropy alloy by regulating the constituent elements and molar ratio of the TiVCrNb high entropy alloy.

[0022] 2. The present invention avoids the volatilization of low-melting-point elements and protects the stability of alloy components by controlling the placement order of alloy raw materials and optimizing the smelting process, thereby ensuring the stability of the alloy's organizational structure and performance, and enhancing the strength and plasticity and gamma shielding properties of the TiVCrNb high-entropy alloy material.

[0023] 3. The present invention improves the distribution uniformity of each element in the high entropy alloy, stabilizes the phase structure of the high entropy alloy, and improves the strength, plasticity and gamma shielding performance of the high entropy alloy by performing homogenization heat treatment on the high entropy alloy ingot.

[0024] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a comparison diagram of the half-value layers of the TiNbAlCr high entropy alloy gamma shielding material prepared in Example 1 of the present invention and Ti, TiAl, TiAlCr without adding Nb element and TiNbAl system without adding Cr element.

[0026] Figure 2 This is an X-ray diffraction pattern of the TiNbAlCr high entropy alloy gamma shielding material prepared in Example 1 of the present invention.

[0027] Figure 3 This is a room temperature tensile stress-strain curve of the TiNbAlCr high entropy alloy gamma-ray shielding material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0028] Example 1

[0029] The strong plastic TiNbAlCr high entropy alloy gamma shielding material of this embodiment is recorded as follows according to the molar ratio of each component element: Ti 45 Nb 45 Al5Cr5.

[0030] The preparation method of the high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material of this embodiment comprises the following steps:

[0031] Step 1: using sandpaper to remove surface impurities from single metal blocks of Ti, Nb, Al and Cr with a raw material purity of not less than 99.8%, and then washing them in anhydrous ethanol, and then weighing the washed raw material ratio according to the component design of the target product;

[0032] Step 2: Place the Al single metal weighed in step 1 at the bottom of the crucible in a vacuum arc melting furnace, then mix the Ti, Nb, and Cr single metals and place them on top of the Al single metal, then evacuate and fill with argon, first use a small current of 70A to melt the Ti, Nb, and Cr single metal mixture on the top of the crucible and wrap the Al single metal at the bottom, then increase the current to 160A for flip melting to obtain an alloy ingot;

[0033] Step 3: Place the alloy ingot obtained in step 2 into a vacuum annealing furnace, evacuate the vacuum, heat to 1200°C, and then heat treat for 24 hours, cool it in the furnace, and obtain a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material.

[0034] After testing, it was found that the physical phase of the high entropy alloy gamma shielding material prepared in this embodiment was a body-centered cubic (BCC) structure, the yield strength at room temperature was 823 MPa, and the tensile plasticity was 14.7%.

[0035] Figure 1 The half-value layer comparison diagram of the TiNbAlCr high entropy alloy gamma shielding material prepared in this embodiment and the Ti, TiAl, TiAlCr without adding Nb element and the TiNbAl system without adding Cr element is shown in FIG. Figure 1It can be seen that after adding Nb and Cr elements, the half-value layer value of TiNbAlCr high entropy alloy at different incident photon energies is the lowest, indicating that the addition of Nb and Cr elements improves the gamma-ray shielding performance of the high entropy alloy of the system of the present invention.

[0036] Figure 2 This is the X-ray diffraction pattern of the TiNbAlCr high entropy alloy gamma shielding material prepared in this embodiment. Figure 2 It can be seen that the phase structure of the TiNbAlCr high entropy alloy gamma shielding material is a body-centered cubic structure (BCC), and no diffraction peaks of other metal compounds are generated, indicating that the TiNbAlCr high entropy alloy prepared in this embodiment has a stable phase structure.

[0037] Figure 3 This is a room temperature tensile stress-strain curve of the TiNbAlCr high entropy alloy gamma shielding material prepared in Example 1 of the present invention. Figure 3 It can be seen that the yield strength of the TiNbAlCr high entropy alloy gamma shielding material reaches 823 MPa, and the tensile plasticity reaches 14.7%, indicating that the TiNbAlCr high entropy alloy prepared in this embodiment has excellent high-strength and high-plasticity properties.

[0038] The raw material in step 1 of this embodiment can also be replaced with granular material, and a grinder can be used to remove surface impurities.

[0039] Example 2

[0040] The strong plastic TiNbAlCr high entropy alloy gamma shielding material of this embodiment is recorded as follows according to the molar ratio of each component element: Ti 60 V 20 Cr1Nb 19 .

[0041] The preparation method of the high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material of this embodiment comprises the following steps:

[0042] Step 1: using sandpaper to remove surface impurities from single metal blocks of Ti, Nb, Al and Cr with a raw material purity of not less than 99.8%, and then washing them in anhydrous ethanol, and then weighing the washed raw material ratio according to the component design of the target product;

[0043] Step 2: Place the Al single metal weighed in step 1 at the bottom of the crucible in a vacuum arc melting furnace, then mix the Ti, Nb, and Cr single metals and place them on top of the Al single metal, then evacuate and fill with argon, first use a small current of 70A to melt the Ti, Nb, and Cr single metal mixture on the top of the crucible and wrap the Al single metal at the bottom, then increase the current to 140A for flip melting to obtain an alloy ingot;

[0044] Step 3: Place the alloy ingot obtained in step 2 into a vacuum annealing furnace, evacuate the vacuum, heat to 900°C, and then heat treat for 48 hours. Cool the furnace to obtain a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material.

[0045] According to tests, the high entropy alloy gamma shielding material prepared in this embodiment has a body-centered cubic (BCC) structure, a yield strength of 810 MPa at room temperature, and a tensile plasticity of 20.5%.

[0046] Example 3

[0047] The strong plastic TiNbAlCr high entropy alloy gamma shielding material of this embodiment is recorded as follows according to the molar ratio of each component element: Ti 20 V 50 Cr 29 Nb1.

[0048] The preparation method of the high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material of this embodiment comprises the following steps:

[0049] Step 1: using sandpaper to remove surface impurities from single metal blocks of Ti, Nb, Al and Cr with a raw material purity of not less than 99.8%, and then washing them in anhydrous ethanol, and then weighing the washed raw material ratio according to the component design of the target product;

[0050] Step 2: Place the Al single metal weighed in step 1 at the bottom of the crucible in a vacuum arc melting furnace, then mix the Ti, Nb, and Cr single metals and place them on top of the Al single metal, then evacuate and fill with argon, first use a small current of 110A to melt the Ti, Nb, and Cr single metal mixture on the top of the crucible and wrap the Al single metal at the bottom, then increase the current to 200A for flip melting to obtain an alloy ingot;

[0051] Step 3: Place the alloy ingot obtained in step 2 into a vacuum annealing furnace, evacuate the vacuum, heat to 1300°C, and then heat treat for 2 hours, and cool it in the furnace to obtain a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material.

[0052] After testing, it was found that the high entropy alloy gamma shielding material prepared in this embodiment had a body-centered cubic (BCC) structure, a yield strength of 834 MPa at room temperature, and a tensile plasticity of 18.6%.

[0053] Example 4

[0054] The strong plastic TiNbAlCr high entropy alloy gamma shielding material of this embodiment is recorded as follows according to the molar ratio of each component element: Ti 20 Nb 20 Al30 Cr 30 .

[0055] The preparation method of the high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material of this embodiment comprises the following steps:

[0056] Step 1: using sandpaper to remove surface impurities from single metal blocks of Ti, Nb, Al and Cr with a raw material purity of not less than 99.8%, and then washing them in anhydrous ethanol, and then weighing the washed raw material ratio according to the component design of the target product;

[0057] Step 2: Place the Al single metal weighed in step 1 at the bottom of the crucible in a vacuum arc melting furnace, then mix the Ti, Nb, and Cr single metals and place them on top of the Al single metal, then evacuate and fill with argon, first use a small current of 90A to melt the Ti, Nb, and Cr single metal mixture on the top of the crucible and wrap the Al single metal at the bottom, then increase the current to 180A for flip melting to obtain an alloy ingot;

[0058] Step 3: Place the alloy ingot obtained in step 2 into a vacuum annealing furnace, evacuate the vacuum, heat to 1100°C, and then heat treat for 36 hours, and cool it in the furnace to obtain a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material.

[0059] After testing, it was found that the physical phase of the high entropy alloy gamma shielding material prepared in this embodiment was a body-centered cubic (BCC) structure, the yield strength at room temperature was 843 MPa, and the tensile plasticity was 16.1%.

[0060] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A high-strength and high-plastic TiNbAlCr high-entropy alloy gamma-ray shielding material, characterized in that: The high entropy alloy gamma shielding material is recorded as follows according to the molar ratio of each component element: Ti a Nb b Al c Cr d , wherein 20≤a≤60, 20≤b≤50, 1≤c≤30, 1≤d≤30, and a+b+c+d=100; the physical phase of the high entropy alloy gamma shielding material is a body-centered cubic structure, the yield strength at room temperature is not less than 800MPa, and the plasticity is not less than 14%.

2. A high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material according to claim 1, characterized in that: The high entropy alloy gamma shielding material is recorded as follows according to the molar ratio of each component element: Ti a Nb b Al c Cr d , where 22≤a≤58, 22≤b≤48, 2≤c≤28, 2≤d≤28, and a+b+c+d=100.

3. A high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material according to claim 2, characterized in that: The high entropy alloy gamma shielding material is recorded as follows according to the molar ratio of each component element: Ti a Nb b Al c Cr d , where a=45, b=45, c=5, d=5.

4. A method for preparing the high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma-ray shielding material as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: Step 1: remove surface impurities from the single metals of Ti, Nb, Al and Cr and wash them in anhydrous ethanol, then weigh the washed raw materials according to the component design of the target product; Step 2: placing the raw materials weighed in step 1 into a vacuum arc melting furnace for melting to obtain an alloy ingot; Step 3: Place the alloy ingot obtained in step 2 into a vacuum annealing furnace for homogenization treatment to obtain a high-strength and high-plasticity TiNbAlCr high-entropy alloy gamma shielding material.

5. The method according to claim 4, characterized in that In step 1, the mass purity of the single metals of Ti, Nb, Al and Cr is not less than 99.8%, and the single metals of Ti, Nb, Al and Cr are all in block or granular form; the removal of surface impurities is carried out using sandpaper or a grinder.

6. The method according to claim 4, characterized in that The weighed raw materials in step 2 are placed in the following order: firstly, the Al single metal is placed at the bottom of the crucible in the vacuum arc melting furnace, and then the Ti, Nb and Cr single metals are mixed and placed on top of the Al single metal.

7. The method according to claim 6, characterized in that During the smelting in step 2, a small current of 70A to 110A is first used to melt the single metal mixture of Ti, Nb, and Cr at the top of the crucible and wrap the single metal of Al at the bottom, and then the current is increased to 140A to 200A for flip melting.

8. The method according to claim 4, characterized in that The homogenization process in step three is: heating to 900° C. to 1300° C. under vacuum conditions for heat treatment for 2 h to 48 h, and then cooling with the furnace.