Corrosion-resistant galvanized steel strand and preparation process thereof

By optimizing the composition of zinc liquid and the selection of plating agents, the corrosion resistance and white rust resistance of galvanized steel strands are improved, and the corrosion resistance and white rust resistance of galvanized steel strands are solved. The corrosion resistance and insufficient white rust resistance of galvanized steel strands are used in the external environment. Problem, significantly extending its service life.

CN119020712APending Publication Date: 2024-11-26HEJIAN CHANGHONG COMM EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153571.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When existing galvanized steel strands are exposed to external environment for a long time, their corrosion resistance and white rust resistance are poor, and they cannot guarantee their long-term effective operation.

Method used

By optimizing the composition of zinc liquid, Ni, Bi and Sr are added, and zinc acetate and L-carnitine tartrate are used as plating agents during the plating process to improve the galvanized quality of galvanized steel wires, thereby improving the galvanized steel strand wires corrosion resistance and white rust resistance. Specific processes include wire pretreatment, auxiliary plating, hot-dip galvanizing and stranding treatment.

Benefits of technology

It significantly improves the corrosion resistance and white rust resistance of galvanized steel strands, extends its service life, and reduces mass loss in different environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of steel strands, and provides a corrosion-resistant galvanized steel strand and a preparation technology thereof.The galvanized steel strand is formed by stranding galvanized steel wires, the galvanized steel wires are obtained by conducting assistant plating and hot galvanizing on the steel wires, and during hot galvanizing, zinc liquid is composed of, by weight, 0.15%-0.20% of Al, 0.12%-0.22% of Ni, 0.30%-0.50% of Sn, 0.05%-0.50% of Sr, 0.12%-0.25% of Bi, 0.02%-0.03% of Pb, 0.04%-0.06% of Sb, 0.10%-0.18% of Fe and the balance Zn and inevitable impurities. According to the technical scheme, the problems of poor corrosion resistance and poor white rust resistance of the galvanized steel strand in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel strands, and in particular to a corrosion-resistant galvanized steel strand and a preparation process thereof. Background Art

[0002] Steel strands are twisted from multiple steel wires and usually have high toughness and good fatigue resistance. They are an important engineering material and play a key role in ensuring the safety and stability of various buildings and infrastructure. Galvanized steel strands are formed by galvanizing the surface of ordinary steel strands to form a solid galvanized layer, thereby isolating the steel strands from direct contact with the external environment and reducing the erosion of oxygen, moisture and other media on the steel strands. Therefore, they can be widely used in hydropower, railways, post and telecommunications engineering overhead power lines, communication cables, hangers, suspensions, and tension tower tie-downs. Galvanized steel strands are usually directly exposed to the atmosphere and are in constant vibration. Some of them will also be subjected to a certain current carrying capacity, so there are high requirements for their anti-corrosion performance. In the existing technology, although galvanized steel strands have certain corrosion resistance, they are exposed to the external environment for a long time, and their corrosion resistance and white rust resistance are poor, and their long-term effective operation cannot be guaranteed. Therefore, improving the corrosion resistance and white rust resistance of galvanized steel strands is a technical problem that needs to be solved urgently. Summary of the invention

[0003] The invention provides a corrosion-resistant galvanized steel strand and a preparation process thereof, which solves the problem of poor corrosion resistance and poor white rust resistance of the galvanized steel strand in the related art.

[0004] The technical solution of the present invention is as follows: A corrosion-resistant galvanized steel strand is formed by twisting galvanized steel wires. The galvanized steel wires are obtained by assisted plating and hot-dip galvanizing. During the hot-dip galvanizing, the zinc liquid consists of the following components in percentage by weight: Al 0.15%~0.20%, Ni 0.12%~0.22%, Sn 0.30%~0.50%, Sr 0.05%~0.50%, Bi 0.12%~0.25%, Pb 0.02%~0.03%, Sb 0.04%~0.06%, Fe 0.1%~0.18%, and the rest are Zn and unavoidable impurities.

[0005] As a further technical solution, the weight ratio of the sum of the Ni and Bi to the weight ratio of the Sr is 1-2:1.

[0006] When the weight ratio of Ni and Bi to Sr is 1~2:1, the corrosion resistance of galvanized steel strand can be further improved.

[0007] As a further technical solution, the weight ratio of Ni to Bi is 1:1.

[0008] As a further technical solution, during the plating aid, the plating aid comprises the following components in parts by weight: 25-30 parts of zinc chloride, 2-14 parts of zinc acetate, 3-15 parts of L-carnitine tartrate, 10-25 parts of ammonium chloride, and 100 parts of water.

[0009] When the steel wire is galvanized, the plating aid includes zinc acetate and L-carnitine tartrate. Through the synergistic effect of zinc acetate and L-carnitine tartrate, the surface activity of the steel wire can be effectively improved, and the surface tension of the zinc liquid can be reduced, so that the steel wire and the zinc liquid can be quickly immersed, thereby improving the galvanizing quality, and further improving the corrosion resistance of the galvanized steel strand.

[0010] As a further technical solution, the weight ratio of the zinc acetate to L-carnitine tartrate is 1-3:1.

[0011] When the weight ratio of zinc acetate to L-carnitine tartrate is 1-3:1, the corrosion resistance of the galvanized steel strand can be further improved.

[0012] The present invention also provides a preparation process of the corrosion-resistant galvanized steel strand, comprising the following steps: S1, subjecting the steel wire to a first water washing, an acid washing, and a second water washing to obtain a pretreated steel wire; S2, the pretreated steel wire is subjected to assisted plating to obtain assisted plating steel wire; S3, immersing the steel wire after the plating assistance into a zinc solution for hot-dip galvanizing to obtain a galvanized steel wire; S4, twisting the galvanized steel wires, twisting them into strands, and performing stabilization treatment to obtain galvanized steel stranded wires.

[0013] As a further technical solution, in step S1, during the pickling, a hydrochloric acid solution with a mass fraction of 15% to 20% is used.

[0014] As a further technical solution, the steel wire is 70# steel wire with a diameter of 0.5~8mm.

[0015] As a further technical solution, in step S1, the temperature of the first water washing and the second water washing is independently 70-80°C.

[0016] As a further technical solution, in step S2, during the plating aid, the weight ratio of the plating aid to the pretreated steel wire is 0.5~1:100.

[0017] As a further technical solution, in step S2, the assist plating time is 6 to 10 minutes.

[0018] As a further technical solution, in step S3, during the hot-dip galvanizing treatment, the temperature of the zinc solution is 440-460°C.

[0019] As a further technical solution, in step S3, the weight of the zinc layer of the galvanized steel wire is 250-350 g / m 2 .

[0020] As a further technical solution, in step S4, when twisting the strands, the twisting distance is 220-240 mm and the twisting angle is 8-10°.

[0021] As a further technical solution, in step S4, during the stabilization treatment, the temperature is 350-370° C. and the time is 15-30 seconds.

[0022] As a further technical solution, the number of wires of the galvanized steel strand is 7 to 19.

[0023] The working principle and beneficial effects of the present invention are: In the present invention, the steel wire is hot-dip galvanized to obtain the galvanized steel wire. By optimizing the component composition of the zinc solution, the galvanizing quality of the steel wire is improved, so that the galvanized steel strand has higher corrosion resistance and white rust resistance. Among them, by adding Ni, Bi and Sr, the complementary combination of the three is utilized to significantly improve the corrosion resistance and white rust resistance of the galvanized steel strand. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In the following embodiments and comparative examples, unless otherwise specified, the steel wire is 70# steel wire with a diameter of 3.8 mm; the number of wires of the galvanized steel strand is 7.

[0026] Example 1 A corrosion-resistant galvanized steel strand is formed by twisting galvanized steel wires. The galvanized steel wires are obtained by assisted plating and hot-dip galvanizing. During hot-dip galvanizing, the zinc liquid consists of the following components in percentage by weight: Al 0.15%, Ni 0.12%, Sn 0.30%, Sr 0.05%, Bi 0.12%, Pb 0.02%, Sb 0.04%, Fe0.10%, the rest is Zn and unavoidable impurities; When assisting plating, the plating agent includes the following components in parts by weight: 25 parts zinc chloride, 2 parts zinc acetate, 3 parts L-carnitine tartrate, 10 parts ammonium chloride, 100 parts water; The preparation process of galvanized steel strand includes the following steps: S1, performing a first water washing of the steel wire at 70° C., performing an acid wash in a hydrochloric acid solution having a mass fraction of 18%, and performing a second water washing at 70° C. to obtain a pretreated steel wire; S2, the pretreated steel wire is subjected to auxiliary plating to obtain an auxiliary plating steel wire (the weight ratio of the auxiliary plating agent to the pretreated steel wire is 0.5:100); S3, immerse the galvanized steel wire in a zinc solution at a temperature of 440°C for hot-dip galvanizing, and obtain a zinc layer with a weight of 275g / m 2 Galvanized steel wire; S4, 7 zinc layers with a weight of 275g / m 2 The galvanized steel wires are twisted into strands with a lay length of 220 mm and a lay angle of 8°. After stabilization treatment at 350°C for 15 seconds, galvanized steel stranded wire is obtained.

[0027] Example 2 A corrosion-resistant galvanized steel strand is formed by twisting galvanized steel wires. The galvanized steel wires are obtained by assisted plating and hot-dip galvanizing. During hot-dip galvanizing, the zinc liquid consists of the following components in percentage by weight: Al 0.18%, Ni 0.14%, Sn 0.40%, Sr 0.32%, Bi 0.14%, Pb 0.025%, Sb 0.05%, Fe0.15%, the rest is Zn and unavoidable impurities; When assisting plating, the plating agent includes the following components in parts by weight: 28 parts of zinc chloride, 7 parts of zinc acetate, 9 parts of L-carnitine tartrate, 18 parts of ammonium chloride, 100 parts of water; The preparation process of galvanized steel strand includes the following steps: S1, performing a first water washing of the steel wire at 75° C., performing an acid wash in a hydrochloric acid solution having a mass fraction of 18%, and performing a second water washing at 75° C. to obtain a pretreated steel wire; S2, the pretreated steel wire is subjected to auxiliary plating to obtain an auxiliary plating steel wire (the weight ratio of the auxiliary plating agent to the pretreated steel wire is 0.8:100); S3, immerse the galvanized steel wire in a zinc solution at a temperature of 450°C for hot-dip galvanizing to obtain a zinc layer with a weight of 275g / m 2 Galvanized steel wire; S4, 7 zinc layers with a weight of 275g / m 2 The galvanized steel wires are twisted into strands with a lay length of 230 mm and a lay angle of 9°. After stabilization treatment at 360°C for 25 seconds, galvanized steel stranded wire is obtained.

[0028] Example 3 A corrosion-resistant galvanized steel strand is formed by twisting galvanized steel wires. The galvanized steel wires are obtained by assisted plating and hot-dip galvanizing. During hot-dip galvanizing, the zinc liquid consists of the following components in percentage by weight: Al 0.20%, Ni 0.22%, Sn 0.50%, Sr 0.50%, Bi 0.25%, Pb 0.03%, Sb 0.06%, Fe0.18%, the rest is Zn and unavoidable impurities; When assisting plating, the plating agent includes the following components in parts by weight: 30 parts of zinc chloride, 14 parts of zinc acetate, 15 parts of L-carnitine tartrate, 25 parts of ammonium chloride, 100 parts of water; The preparation process of galvanized steel strand includes the following steps: S1, performing a first water washing of the steel wire at 80° C., performing an acid wash in a hydrochloric acid solution having a mass fraction of 18%, and performing a second water washing at 80° C. to obtain a pretreated steel wire; S2, the pretreated steel wire is subjected to auxiliary plating to obtain an auxiliary plating steel wire (the weight ratio of the auxiliary plating agent to the pretreated steel wire is 1:100); S3, immerse the galvanized steel wire in a zinc solution at a temperature of 460°C for hot-dip galvanizing to obtain a zinc layer with a weight of 275g / m 2 Galvanized steel wire; S4, 7 zinc layers with a weight of 275g / m 2 The galvanized steel wires are twisted into strands with a lay length of 240 mm and a lay angle of 10°. After stabilization treatment at 370°C for 30 seconds, galvanized steel stranded wire is obtained.

[0029] Example 4 The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight percentage of Ni added to the zinc liquid is 0.22%, the weight percentage of Bi added is 0.22%, and the weight percentage of Sr added is 0.16%.

[0030] Example 5 The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight percentage of Ni added to the zinc liquid is 0.15%, the weight percentage of Bi added is 0.15%, and the weight percentage of Sr added is 0.30%.

[0031] Example 6 The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight percentage of Ni added to the zinc liquid is 0.20%, the weight percentage of Bi added is 0.20%, and the weight percentage of Sr added is 0.20%.

[0032] Example 7 The only difference between this embodiment and embodiment 6 is that in this embodiment, 13 parts of zinc acetate and 3 parts of L-carnitine tartrate are added to the plating assistant.

[0033] Example 8 The only difference between this embodiment and embodiment 6 is that in this embodiment, 8 parts of zinc acetate and 8 parts of L-carnitine tartrate are added to the plating assistant.

[0034] Example 9 The only difference between this embodiment and embodiment 6 is that in this embodiment, 12 parts of zinc acetate and 4 parts of L-carnitine tartrate are added to the plating assistant.

[0035] Comparative Example 1 The difference between this comparative example and Example 1 is that in this comparative example, Sr is not added to the zinc solution, the weight percentage of Ni added is 0.145%, and the weight percentage of Bi added is 0.145%.

[0036] Comparative Example 2 The only difference between this comparative example and Example 1 is that in this comparative example, no Ni is added to the zinc solution, the weight percentage of Bi added is 0.24%, and the weight percentage of Sr added is 0.05%.

[0037] Comparative Example 3 The only difference between this comparative example and Example 1 is that in this comparative example, Bi is not added to the zinc solution, the weight percentage of Ni added is 0.24%, and the weight percentage of Sr added is 0.05%.

[0038] Comparative Example 4 The difference between this comparative example and Example 1 is that in this comparative example, no Ni and no Bi are added to the zinc liquid, and the weight percentage of Sr added is 0.29%.

[0039] Comparative Example 5 The only difference between this comparative example and Example 1 is that in this comparative example, Ni, Bi and Sr are not added to the zinc solution.

[0040] The galvanized steel wires prepared in Examples 1 to 9 and Comparative Examples 1 to 5 were subjected to the following performance tests: Corrosion resistance: According to the neutral salt spray test in GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", prepare a salt spray box, measure the mass loss of the galvanized steel wire sample, and calculate the mass reduction percentage according to the following formula, mass reduction percentage = (mass of galvanized steel strand sample before neutral salt spray test - mass of galvanized steel strand sample after test) / mass of galvanized steel strand sample before neutral salt spray test × 100%; among which, the concentration of the spray liquid prepared by sodium chloride is 55g / L, the pH value is 6.8, the spray pressure is 98kPa, the saturated tower hot water temperature is 48°C, and the test period is 168h; the temperature in the salt spray box is 35°C.

[0041] Anti-white rust performance: The galvanized steel wire sample was placed in an environment of 35℃, 95%RH for 24 hours and then subjected to a simulated rain scouring test. During the rain scouring test, a nozzle was set 2.5m above the sample, and the rainfall of the nozzle was 40mm. The simulated rain scouring was continued for 5 hours as one test. Before the next test, the sample was placed in an environment of 25℃, 40%RH for 9 hours. Observe and record whether white rust appears on the surface of the sample after 5 and 10 times. If white rust appears after 5 tests, there is no need to conduct 10 tests.

[0042] The test results are shown in Table 1 below: Table 1 Test results

[0043] Compared with Comparative Examples 1 to 5, after simultaneously adding Ni, Sr and Bi in Example 1, the mass reduction percentage of the galvanized steel wire is significantly reduced, and after 5 and 10 simulated rainwater scouring tests, no white rust appears on the surface of the galvanized steel wire, indicating that by adding Ni, Sr and Bi and utilizing the complementary combination of the three, the corrosion resistance and white rust resistance of the galvanized steel strand can be significantly improved.

[0044] Compared with Examples 2 and 4, the mass reduction percentage of the galvanized steel wire of Examples 5-6 is reduced, indicating that when the weight ratio of Ni and Bi to Sr is 1-2:1, the corrosion resistance of the galvanized steel strand can be further improved. Compared with Examples 6-7, the mass reduction percentage of the galvanized steel wire of Examples 8-9 is reduced, indicating that when the weight ratio of zinc acetate and L-carnitine tartrate in the plating agent is 1-3:1, the corrosion resistance of the galvanized steel strand can be further improved.

[0045] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A corrosion-resistant galvanized steel strand, which is made of galvanized steel wires twisted together, characterized in that: The galvanized steel wire is obtained by assisted plating and hot-dip galvanizing of the steel wire. During the hot-dip galvanizing, the zinc liquid is composed of the following components in weight percentage: Al 0.15%~0.20%, Ni 0.12%~0.22%, Sn 0.30%~0.50%, Sr 0.05%~0.50%, Bi 0.12%~0.25%, Pb 0.02%~0.03%, Sb 0.04%~0.06%, Fe 0.10%~0.18%, and the rest are Zn and unavoidable impurities.

2. The corrosion-resistant galvanized steel strand according to claim 1, characterized in that: The weight ratio of the Ni and Bi to the Sr is 1-2:

1.

3. The corrosion-resistant galvanized steel strand according to claim 1, characterized in that: When assisting plating, the plating assistant comprises the following components in parts by weight: 25-30 parts of zinc chloride, 2-14 parts of zinc acetate, 3-15 parts of L-carnitine tartrate, 10-25 parts of ammonium chloride, and 100 parts of water.

4. The corrosion-resistant galvanized steel strand according to claim 3, characterized in that: The weight ratio of the zinc acetate to L-carnitine tartrate is 1-3:

1.

5. A process for preparing a corrosion-resistant galvanized steel strand according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, subjecting the steel wire to a first water washing, a pickling, and a second water washing to obtain a pretreated steel wire; S2, the pretreated steel wire is subjected to assisted plating to obtain assisted plating steel wire; S3, immersing the steel wire after the plating assistance into a zinc solution for hot-dip galvanizing to obtain a galvanized steel wire; S4, twisting the galvanized steel wires, twisting them into strands, and performing stabilization treatment to obtain galvanized steel stranded wires.

6. The process for preparing a corrosion-resistant galvanized steel strand according to claim 5, characterized in that: In step S1, during the pickling, a hydrochloric acid solution with a mass fraction of 15% to 20% is used.

7. The process for preparing a corrosion-resistant galvanized steel strand according to claim 5, characterized in that: In step S1, the temperatures of the first water washing and the second water washing are independently 70-80°C.

8. The process for preparing a corrosion-resistant galvanized steel strand according to claim 5, characterized in that: In step S3, during the hot-dip galvanizing treatment, the temperature of the zinc solution is 440-460°C.

9. The process for preparing a corrosion-resistant galvanized steel strand according to claim 5, characterized in that: In step S4, when twisting the strands, the twisting distance is 220-240 mm and the twisting angle is 8-10°.

10. The process for preparing a corrosion-resistant galvanized steel strand according to claim 5, characterized in that: In step S4, during the stabilization treatment, the temperature is 350-370° C. and the time is 15-30 seconds.