Platinum load-adjustable hydrogen evolution electrode and preparation method and application thereof
By using electrodeposition method on base metal substrates to form a hydrogen evolution electrode with adjustable platinum load, the problems of low hydrolysis activity and high platinum cost of nickel grid electrodes are solved, and the precise control and stability of platinum load is achieved, and the electrolysis is improved The efficiency and economicality of water hydrogen production.
Patent Information
- Application Number
- CN202411013395.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing electrolytic hydrogen production technology, the nickel grid electrode is difficult to match the high hydrogen production needs due to its low hydrolysis activity. The high cost and low reserves of platinum as a high-efficiency hydrogen evolution electrode material limit its large-scale application. How to take into account hydrolysis Activity and cost are a technical challenge.
The hydrogen evolution electrode with adjustable platinum load is formed on the base metal substrate by electrodeposition method. By controlling the pH value of the electrolyte, the concentration of platinum ions and base metal ions, the number of cycles and the heating treatment, the precise control of platinum load is achieved. , ensure stable load and efficient operation of platinum elements.
It realizes the precise controllable load of platinum and load stability, improves hydrogen evolution activity and durability, reduces costs, and meets the needs of efficient electrolyzed hydrogen production.
Smart Images

Figure CN119020799A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hydrogen production by electrolysis of water, and in particular to a hydrogen evolution electrode with adjustable platinum loading, and a preparation method and application thereof. Background Art
[0002] With the rapid development of renewable energy, its intermittent, random and time-space mismatch of loads are becoming increasingly prominent. How to solve the absorption of renewable energy and ensure the safe operation of the power grid system is gradually becoming the focus of attention in the energy field. Hydrogen energy, as a large-scale and long-term energy storage method with great advantages, can effectively solve the problem of renewable energy power generation; at the same time, the application range of hydrogen energy is very wide, and it can be used in transportation, chemical industry, metallurgy and other fields to further reduce carbon emissions. The electrolysis of water to produce hydrogen currently mainly includes alkaline electrolysis cells, proton exchange membrane electrolysis cells and solid oxide electrolysis cells. Alkaline solution electrolysis cells are the most mature commercial water electrolysis hydrogen production method because of their low cost. The electrode is the place where the water decomposition reaction occurs, which determines the speed of the reaction.
[0003] Nickel mesh is the most common electrode material for hydrogen production from alkaline solutions due to its low cost and resistance to alkali corrosion, but its low hydrolysis activity leads to an overall low efficiency of hydrogen production from alkaline solutions, making it difficult to match higher hydrogen production needs. According to DFT (Density Functional Theory) calculations, platinum (Pt) has the highest theoretical hydrogen evolution activity, but its high price (208 yuan / g) and reserves limit its large-scale application as an electrode material. Considering its high cost, nickel mesh electrodes are usually only doped with trace amounts of platinum. However, when trace-doping platinum, how to better balance hydrolysis activity and cost is a technical challenge currently faced by platinum-doped electrodes. Summary of the invention
[0004] Based on this, the present application provides a hydrogen evolution electrode with adjustable platinum loading and a preparation method and application thereof, which can achieve precise control of the platinum loading during the electrode preparation process and enable the platinum element loaded on the base metal substrate to work stably, thereby achieving a good balance between hydrolysis activity and cost.
[0005] The first aspect of the present application provides a method for preparing a hydrogen evolution electrode with adjustable platinum loading, comprising:
[0006] The electrolyte is deposited on a substrate by an electrodeposition method to form a base metal hydroxide loaded on the substrate and platinum partially or completely loaded on the base metal hydroxide, so as to prepare a hydrogen evolution electrode with adjustable platinum loading.
[0007] Wherein, the electrolyte contains platinum ions and base metal ions, the pH value of the electrolyte is >7, and the substrate contains the base metal.
[0008] In some embodiments of the present application, linear voltammetry is used for the electrodeposition, and the linear voltammetry satisfies at least one of the following conditions:
[0009] (1) In the linear voltammetry, the voltage range relative to the reversible hydrogen electrode is 0 to -0.5 V;
[0010] (2) In the linear voltammetry, the number of cycles is: 0 < cycle ≤ 250 cycles, and optionally: 20 ≤ cycle ≤ 250 cycles.
[0011] In some embodiments of the present application, the electrolyte satisfies at least one of the following conditions:
[0012] (1) In the electrolyte, the concentration of platinum ions is 5 mg / L to 50 mg / L;
[0013] (2) In the electrolyte, the concentration of ions of base metals is 0.5 g / L to 1 g / L;
[0014] (3) The electrolyte further contains a pH adjusting reagent;
[0015] Optionally, the pH adjusting reagent includes urea;
[0016] Optionally, in the electrolyte, the concentration of the pH adjusting reagent is 1 g / L to 5 g / L;
[0017] (4) The electrolyte further contains anions;
[0018] Optionally, the anions include at least one of chloride ions, nitrate ions, and sulfate ions, and further optionally chloride ions;
[0019] (5) The pH value of the electrolyte satisfies: 7.5 ≤ pH value ≤ 8.5.
[0020] In some embodiments of the present application, at least one of the following conditions is satisfied:
[0021] (1) The source of the platinum ions includes at least one of platinum chloride and platinum nitrate, and optionally platinum chloride;
[0022] (2) The source of the ions of the base metals includes at least one of chlorides, nitrate compounds, and sulfate compounds of the base metal ions, and optionally chlorides of the base metal ions.
[0023] In some embodiments of the present application, it further includes: heating the hydrogen evolution electrode to decompose the base metal hydroxide into a base metal oxide;
[0024] Optionally, the temperature of the heating treatment is T1, the decomposition temperature of the base metal hydroxide is T2, and T2≤T1≤T2+20°C.
[0025] In some embodiments of the present application, the base metal includes nickel.
[0026] The second aspect of the present application provides a hydrogen evolution electrode with adjustable platinum loading, which is prepared by the preparation method of the first aspect of the present application.
[0027] In some embodiments of the present application, the hydrogen evolution electrode comprises the substrate, an intermediate carrier loaded on the substrate, and platinum loaded on the intermediate carrier, wherein the intermediate carrier comprises the base metal hydroxide or the base metal oxide;
[0028] Optionally, the base metal hydroxide contains a whisker-like structure;
[0029] Optionally, the base metal oxide contains whisker structures;
[0030] Optionally, the platinum comprises a granular structure.
[0031] In some embodiments of the present application, the platinum loading on the hydrogen evolution electrode is 0-0.16 mg / cm 2 , optional 0.01mg / cm 2 ~0.16mg / cm 2 .
[0032] The third aspect of the present application provides an application of the hydrogen evolution electrode with adjustable platinum loading as described in the second aspect of the present application in hydrogen production from alkaline solution.
[0033] The preparation method provided in the present application can achieve precise control of the platinum loading during the electrode preparation process, and can enable the platinum element loaded on the base metal substrate to work stably, thereby obtaining a hydrogen evolution electrode with precisely controllable platinum loading and stable coordination of microscopic particles, while also providing the possibility for efficient hydrogen production by water electrolysis, thereby achieving a good balance between hydrolysis activity and cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of a device for electrodeposition according to one embodiment of the present application.
[0035] Figure 2 1 is a curve showing the relationship between the voltage scanning range and the number of cycles during the electrodeposition process of Examples 1 to 7.
[0036] Figure 3 The XRD diffraction patterns of the hydrogen evolution electrodes of Example 1 and Comparative Example 8 are shown.
[0037] Figure 4(b) and (a) are morphology images of the hydrogen evolution electrodes of Example 1 and Comparative Example 8, respectively.
[0038] Figure 5 This is another morphology picture of the hydrogen evolution electrode of Example 1.
[0039] Description of reference numerals:
[0040] 1 working electrode, 2 reference electrode, 3 counter electrode, 4 electrolyte, 5 nickel mesh. DETAILED DESCRIPTION
[0041] In order to facilitate understanding of the present application, the present application will be described more comprehensively below. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0042] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. It should be noted that, unless otherwise specified, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" are inclusive of the number, and the meaning of "multiple" in "one or more" is more than two.
[0044] Herein, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values within the numerical interval is considered to be continuous and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval only refers to integers within the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.
[0045] In this article, if there are multiple steps involved in the method flow, unless there is a clear different description in this article, there is no strict order restriction for the execution of these steps, and they can be executed in other orders than described. Moreover, any step can include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn, alternating or simultaneously with other steps or parts of sub-steps or stages of other steps.
[0046] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0047] At present, platinum has the highest theoretical hydrogen evolution activity. Therefore, in a platinum-doped nickel mesh electrode, a trace amount of platinum doping can achieve a significant increase in the electrode hydrolysis activity. We usually think that when trace doping is performed, the higher the amount of platinum doping in the electrode, the better its hydrogen evolution activity may be. However, the inventors found that in fact, the hydrogen evolution activity of the electrode is not better with the higher amount of platinum doping; and the higher the amount of platinum doping, the higher the cost. Therefore, we hope to achieve higher hydrogen evolution activity with as little doping as possible and reduce costs as much as possible. In addition, the inventors also found that when the doping amount of platinum is low, platinum is easy to fall off the electrode, and its load stability on the electrode is not high, making it difficult to ensure the stable operation of the platinum element.
[0048] That is to say, the hydrolysis activity of the electrode is mainly related to the amount of platinum doped on the electrode (i.e., platinum loading) and the stability of platinum loading on the electrode; and the stability of platinum loading on the electrode is related to both the platinum loading and the loading method of platinum on the electrode (or the bonding method between platinum and the electrode). Based on this, the inventors found that in the process of preparing platinum-doped hydrogen evolution electrodes, how to achieve more accurate regulation of the doping amount of platinum, so that through this regulation, it is possible to find and determine the appropriate doping amount, so that the doping amount is as small as possible to control the cost, and at the same time, it can effectively improve the hydrogen evolution activity, and ensure the stability of the platinum element loaded on the nickel mesh, so that it can work stably, is a crucial issue. Based on this, the inventors proposed the following technical solution of this application.
[0049] In a first aspect, the present application provides a method for preparing a hydrogen evolution electrode with adjustable platinum loading, which may include the following steps:
[0050] S1. Depositing an electrolyte on a substrate by an electrodeposition method to form a base metal hydroxide loaded on the substrate, and platinum partially or completely loaded on the base metal hydroxide, to prepare a hydrogen evolution electrode with adjustable platinum loading,
[0051] Wherein, the electrolyte contains platinum ions and base metal ions, the pH value of the electrolyte is >7, and the substrate contains the base metal.
[0052] It should be noted that the "platinum loading" or "platinum loading" mentioned in this application refers to the mass of platinum loaded on the substrate per unit area (e.g., per square centimeter). The "base metal" refers to metals other than precious metals (gold, silver, ruthenium, rhodium, palladium, osmium, iridium, platinum).
[0053] It is understood that the base metal in the base metal hydroxide, the base metal in the base metal ions contained in the electrolyte, and the base metal contained in the substrate are all the same.
[0054] In the process of studying how to achieve more precise control of the doping amount of platinum, the inventors also found that traditional electrodes usually load precious metals (such as platinum) directly on a substrate (such as a nickel mesh). When this loading method is used, the binding force between the precious metal and the substrate is not strong, and the precious metal is more likely to fall off the substrate. This possibility of falling off will cause a large difference between the actual loading amount of the precious metal on the substrate and the expected loading amount (or theoretical loading amount), which is one of the main reasons why it is difficult to achieve more accurate control of the (actual) loading amount of the precious metal.
[0055] Accordingly, the preparation method provided in the present application uses an electrodeposition method to deposit an electrolyte with a pH value>7 on a substrate to form a base metal hydroxide and platinum, and the base metal hydroxide is loaded on the substrate, and part or all of the platinum is loaded on the base metal hydroxide. Among them, the base metal in the base metal hydroxide is the same as the base metal contained in the substrate, which can make the base metal hydroxide and the substrate have good bonding force. At the same time, the base metal hydroxide can be used as an intermediate carrier for supporting platinum, so that part or all of the platinum is loaded on the substrate with the base metal hydroxide as a loading medium, and the intermediate carrier is conducive to improving the load stability of platinum thereon. Compared with directly depositing platinum on the substrate (i.e. directly using the substrate as a carrier for supporting platinum), this method can reduce the possibility of the loaded platinum falling off the electrode and effectively improve the load stability of platinum. Thus, the base metal hydroxide loaded on the substrate, and the platinum partially or entirely loaded on the base metal hydroxide, can synergistically improve the load stability of platinum on the hydrogen evolution electrode.
[0056] Based on the good load stability of platinum on the hydrogen evolution electrode, by changing the preparation conditions of electrodeposition (such as the number of cycles), or the concentration of platinum ions in the electrolyte, or other related preparation conditions, the loading amount of platinum can be regulated more accurately. Through this regulation, it is possible to find and determine the appropriate loading amount, so that the loading amount is as small as possible to control the cost, and the stability of the platinum element loaded on the electrode is further improved by adjusting the loading amount, so as to obtain a hydrogen evolution electrode with a precisely controllable platinum loading and stable matching of microscopic particles, and at the same time, it also provides the possibility for efficient hydrogen production by electrolysis of water, thereby greatly improving the electrode activity while ensuring the cost. In addition, compared with hydrogen evolution electrodes loaded with multiple elements, the single element (such as platinum) loading of the present application makes it easier to achieve precise control of the loading amount.
[0057] In the above preparation method, the pH value of the electrolyte is made greater than 7, which can provide an alkaline environment for the electrodeposition process, thereby facilitating the base metal ions in the electrolyte to form base metal hydroxides.
[0058] In some embodiments, the pH value of the electrolyte satisfies: 7.5≤pH≤8.5. For example, the pH value may be 7.5, 7.55, 7.6, 7.65, 7.7, 7.75, 7.8, 7.85, 7.9, 7.95, 8, 8.05, 8.1, 8.15, 8.2, 8.25, 8.3, 8.35, 8.4, 8.45, 8.5 or within the range of any of the above values. In this way, the formation of base metal hydroxides is more promoted.
[0059] In some embodiments, the electrolyte further comprises a pH adjusting agent; optionally, the pH adjusting agent comprises urea.
[0060] When the pH adjusting reagent includes urea, during the electrodeposition process, it can decompose to generate ammonia and carbon dioxide. Among them, ammonia can dissolve in the electrolyte to form ammonia water, providing a weak alkaline environment for the formation of base metal hydroxides, while carbon dioxide can be released and discharged. Compared with using other pH adjusting reagents (such as sodium hydroxide), urea can avoid the introduction of other impurity elements as much as possible, and thereby reduce the adverse effects on the hydrogen evolution electrode activity caused by the introduction of impurity elements.
[0061] In some embodiments, the electrodeposition uses linear sweep voltammetry. In the linear sweep voltammetry, the voltage sweep range relative to the reversible hydrogen electrode is 0~-0.5V, which can be expressed as: 0~-0.5V vs. RHE (RHE, Reversible Hydrogen Electrode, reversible hydrogen electrode).
[0062] In some embodiments, the electrodeposition uses linear sweep voltammetry. In the linear sweep voltammetry, the number of cycles is: 0 < cycle ≤ 250 cycles, and can be selected as: 20 ≤ cycle ≤ 250 cycles.
[0063] Both the voltage sweep range and the number of cycles can control the deposition rate of platinum element and the number of particles deposited per unit time, and thus can achieve precise control of the platinum loading and the particle size of platinum. Therefore, within the above voltage sweep range or number of cycles, the platinum loading can increase with the increase of the absolute value of the voltage sweep range or the number of cycles, so that it is possible to accurately regulate the (actual) loading of platinum. At the same time, within the above voltage sweep range or number of cycles, it is also beneficial to make platinum have a suitable loading amount, which is as small as possible to control costs, and at the same time, platinum can have a high loading stability on the hydrogen evolution electrode, so that the platinum element loaded on the electrode can work stably, and the hydrogen evolution electrode has high hydrogen evolution activity and durability.
[0064] In some embodiments, in the electrolyte, the concentration of the platinum ions is 5mg / L~50mg / L. For example, the concentration of the platinum ions can be 5mg / L, 8mg / L, 10mg / L, 13mg / L, 15mg / L, 17mg / L, 20mg / L, 23mg / L, 25mg / L, 27mg / L, 30mg / L, 32mg / L, 35mg / L, 38mg / L, 40mg / L, 43mg / L, 45mg / L, 47mg / L, 50mg / L or within the range composed of any of the above values. When the concentration of the platinum ions is within this range, it is beneficial to accurately adjust the (actual) loading of platinum.
[0065] In some embodiments, in the electrolyte, the concentration of the base metal ions is 0.5 g / L to 1 g / L. For example, the concentration of the base metal ions can be 0.5 g / L, 0.6 g / L, 0.7 g / L, 0.8 g / L, 0.9 g / L, 1 g / L, or within the range of any of the above values. The concentration of the base metal ions within this range is conducive to the formation of an appropriate amount of hydroxide support carrier, thereby accurately adjusting the (actual) loading amount of platinum.
[0066] In some embodiments, in the electrolyte, the concentration of the pH adjusting agent is 1 g / L to 5 g / L. For example, the concentration of the pH adjusting agent can be 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L, 5 g / L or within the range of any of the above values. In this way, an alkaline environment can be provided for the electrodeposition process, the pH value of the solution can be regulated, and the formation of base metal hydroxides can be promoted.
[0067] In some embodiments, the electrolyte further comprises anions; optionally, the anions include at least one of chloride ions, nitrate ions and sulfate ions.
[0068] In some embodiments, the anion is a chloride ion. The chloride ion can promote the base metal hydroxide to form a whisker structure, which can make the base metal hydroxide have a higher specific surface area, thereby facilitating the surface to load more platinum particles; and the whisker structure is also conducive to increasing the binding force between the base metal hydroxide and the platinum particles, thereby improving the loading stability of platinum.
[0069] In some embodiments, the source of platinum ions includes at least one of platinum chloride and platinum nitrate, and may be platinum chloride.
[0070] In some embodiments, the source of the base metal ion includes at least one of a base metal chloride, a nitric acid compound, and a sulfuric acid compound, and may be a base metal chloride.
[0071] In some embodiments, the base metal includes nickel.
[0072] In some embodiments, the substrate is a mesh of a base metal.
[0073] In some embodiments, the preparation method may further include the following steps:
[0074] S2. Heating the hydrogen evolution electrode to decompose the base metal hydroxide into base metal oxide.
[0075] In some embodiments, the temperature of the heating treatment is T1, the decomposition temperature of the base metal hydroxide is T2, and T2≤T1≤T2+20° C. In this way, the base metal hydroxide can be completely decomposed into base metal oxides, and the adverse effects on the hydrogen evolution electrode caused by excessively high temperature can be reduced.
[0076] In a second aspect, the present application provides a hydrogen evolution electrode with adjustable platinum loading, which can be prepared by the preparation method of the first aspect of the present application.
[0077] In some embodiments, the hydrogen evolution electrode includes a substrate, an intermediate support supported on the substrate, and platinum partially or fully supported on the intermediate support, wherein the intermediate support includes a base metal hydroxide.
[0078] In some embodiments, the hydrogen evolution electrode includes a substrate, an intermediate support supported on the substrate, and platinum partially or fully supported on the intermediate support, wherein the intermediate support includes a base metal oxide.
[0079] Base metal hydroxide or base metal oxide can be used as an intermediate carrier for carrying platinum, so that part or all of the platinum is loaded on the substrate with base metal hydroxide or base metal oxide as a loading medium, and the intermediate carrier is conducive to improving the load stability of platinum thereon. At the same time, the base metal in the base metal hydroxide or base metal oxide is the same as the base metal contained in the substrate, so that the intermediate carrier and the substrate can have good bonding force. Compared with directly using the substrate as a carrier for carrying platinum, the hydrogen evolution electrode provided by the present application can reduce the possibility of the loaded platinum falling off from the electrode, and effectively improve the load stability of platinum. Thus, the base metal hydroxide or base metal oxide loaded on the substrate, and the platinum partially or entirely loaded on the intermediate carrier, can synergistically improve the load stability of platinum on the hydrogen evolution electrode.
[0080] In some embodiments, the base metal hydroxide contains whisker structures (see Figure 5 ).
[0081] In some embodiments, the base metal oxide contains whisker structures.
[0082] The whisker-like structure can make the base metal hydroxide or base metal oxide have a higher specific surface area, which is conducive to loading more platinum particles on its surface; and the whisker-like structure is also conducive to increasing the binding force between the base metal hydroxide and the platinum particles, thereby improving the loading stability of platinum.
[0083] In some embodiments, the platinum has a granular structure. The granular structure is conducive to the loading of platinum on the non-metallic hydroxide or non-metallic oxide, and is conducive to more accurate regulation of the loading amount of platinum.
[0084] In some embodiments, the platinum loading on the hydrogen evolution electrode is 0-0.16 mg / cm 2 , optional 0.01mg / cm 2 ~0.16mg / cm 2 For example, the platinum loading can be 0.001 mg / cm 2 , 0.002mg / cm 2 , 0.004mg / cm 2 , 0.005mg / cm 2 , 0.007mg / cm 2 , 0.009mg / cm 2 , 0.01mg / cm 2 , 0.03mg / cm 2 , 0.04mg / cm 2 , 0.05mg / cm 2 , 0.06mg / cm 2 , 0.08mg / cm 2 , 0.1mg / cm 2 , 0.13mg / cm 2 , 0.15mg / cm 2 , 0.16mg / cm 2 Or within the range formed by any of the above values. When the platinum loading is within this range, the loading amount can be as small as possible, and at the same time, the platinum can have a higher loading stability on the hydrogen evolution electrode, so that the platinum element loaded on the electrode can work stably, and the hydrogen evolution electrode can have higher hydrogen evolution activity and durability.
[0085] In a third aspect, the present application provides an application of a hydrogen evolution electrode with adjustable platinum loading according to the second aspect of the present application in hydrogen production from alkaline solution.
[0086] Example
[0087] The following are specific examples, which more specifically describe the contents disclosed in this application, and these examples are only for illustrative purposes, because it is obvious to those skilled in the art that various modifications and variations are made within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0088] Example 1
[0089] A three-electrode system was built, with nickel mesh (NM) as the working electrode, Hg|HgO electrode as the reference electrode, and carbon rod as the counter electrode. 3.0 mg PtCl3, 0.3 g urea, and 0.07 g NiCl2 were added to 100 mL of deionized water and stirred evenly as the electrolyte. Electrodeposition was performed using the voltammetric curve program (CV), with the CV voltage scanning range selected from 0 to 0.5 V vs. RHE, and 100 cycles. A hydrogen evolution electrode with adjustable platinum loading was prepared and represented as Pt 0.05 -Ni(OH)2 / NM.
[0090] Embodiments 2 to 7
[0091] The preparation method is similar to that of Example 1, except that the number of cycles is adjusted to 1, 20, 50, 150, 200 and 250 respectively, and the prepared hydrogen evolution electrodes are represented as: Pt 0.001 -Ni(OH)2 / NM、Pt 0.01 -Ni(OH)2 / NM、Pt 0.03 -Ni(OH)2 / NM、Pt 0.08 -Ni(OH)2 / NM、Pt 0.11 -Ni(OH)2 / NM and Pt 0.15 -Ni(OH)2 / NM.
[0092] Example 8
[0093] The preparation method is similar to that of Example 1, with the main difference being that the hydrogen evolution electrode is heated at a temperature of 235°C.
[0094] Comparative Examples 1 to 7
[0095] The preparation methods are respectively similar to those of Examples 1 to 7, with the main difference being that the electrolyte does not contain urea and NiCl2.
[0096] Comparative Example 8
[0097] The hydrogen evolution electrode in Example 1 was replaced by a nickel mesh.
[0098] The hydrogen evolution electrodes prepared in Examples 1 to 8 and Comparative Examples 1 to 8 were subjected to relevant performance tests, and the test results are shown in Tables 1 and 2 below.
[0099] Among them, the test conditions or test standards for each performance test item are as follows:
[0100] (1) XRD test
[0101] X-ray diffraction analysis patterns were measured using CuKα1 radiation with reference to JIS K 0131-1996, General Rules for X-ray Diffraction Analysis Methods.
[0102] (2) Morphology test
[0103] A scanning electron microscope (model: JSM-6700F) was used to test the morphology.
[0104] (3) Platinum loading test
[0105] The platinum content was tested using an inductively coupled plasma optical emission spectrometer (ICP-OES, model: Thermo Scientific iCAP6300).
[0106] (4) Hydrogen evolution activity test and durability test
[0107] The hydrogen evolution activity test adopts a three-electrode method, with the embodiment and comparative example as working electrodes, Hg|HgO as reference electrode, and carbon rod as counter electrode, and uses an electrochemical workstation (model: CHI 750E) to perform polarization curve test and iR compensation. The calculated voltage of the electrode relative to the standard hydrogen electrode (vs. RHE) is processed by the Nernst formula:
[0108] E (RHE) = E (Hg|HgO) + 0.0591 × pH + 0.098 (V)
[0109] E (RHE) is the calculated standard hydrogen electrode voltage, E (Hg|HgO) is the test voltage of the electrochemical workstation, 0.098 is the standard hydrogen voltage of Hg|HgO at 25°C. The test current density reaches 10 mA / cm 2 The overpotential at 200 s can be used to characterize the hydrogen evolution activity.
[0110] The durability test was performed using an electrochemical workstation (model: CHI 750E) to perform chronopotentiometry (chronopotentiometry, a curve of potential change over time detected by constant current density). The current density used in this paper is 100 mA / cm 2 The durability can be characterized by the time required for the voltage increase to reach 5%.
[0111] Table 1
[0112]
[0113] Table 2
[0114]
[0115] In Table 1, by comparing the examples with the comparative examples, it can be seen that the hydrogen evolution electrode prepared by the preparation method of the present application still has good hydrogen evolution activity and durability when the platinum loading is low, which is beneficial to the stable operation of the platinum element loaded on the nickel mesh and can better balance the hydrolysis activity and cost.
[0116] In Table 2, by comparing Examples 1 to 7 with Comparative Examples 1 to 7, it can be seen that the platinum loading of the hydrogen evolution electrode containing the intermediate carrier nickel hydroxide in Examples 1 to 7 increases significantly with the continuous increase in the number of cycles. For example, from 100 cycles to 150 cycles, the increase is 0.0308; from 150 cycles to 200 cycles, the increase is 0.0261; and from 200 cycles to 250 cycles, the increase is 0.0441. In Comparative Examples 1 to 7, the platinum loading of the hydrogen evolution electrode directly loaded on the nickel mesh increases less with the continuous increase in the number of cycles. For example, from 100 cycles to 150 cycles, the increase is only 0.0204; from 150 cycles to 200 cycles, the increase is only 0.0085; and from 200 cycles to 250 cycles, the increase is only 0.0047. This shows that when the hydrogen evolution electrode does not contain the intermediate carrier nickel hydroxide, the part of platinum that is deposited on the nickel mesh due to the increase in the number of cycles is easy to fall off the electrode, making the actual measured platinum loading increase smaller and much lower than the platinum loading increase that should theoretically correspond to the increase in the number of cycles, and the higher the number of cycles, the more obvious this phenomenon will be. In the hydrogen evolution electrode of the present application, the intermediate carrier nickel hydroxide can effectively improve the load stability of platinum, so the actual measured platinum loading increase is higher and closer to the platinum loading increase that should theoretically correspond to the increase in the number of cycles, so that more accurate control of the platinum loading can be achieved.
[0117] Also, see Figure 3 In Comparative Example 8, the clean NM without electrodeposition only showed three typical characteristic peaks at 44.5°, 51.8° and 76.4°, corresponding to the standard diffraction card No. 04-0850 of Ni metal. 0.05 -Ni(OH)2 / NM, an obvious characteristic peak appears at the 39.8° position, corresponding to the Pt(111) crystal plane, indicating the successful doping of Pt element. In addition, the characteristic peaks displayed at the 19.3° and 38.5° positions correspond to the standard diffraction card No.14-0117 of Ni(OH)2.
[0118] See also Figure 4 , the surface of the NM fiber in Comparative Example 8 was smooth and pure without electrodeposition. However, after the electrodeposition reaction of Pt and Ni(OH)2 was carried out in Example 1, a large number of particles were formed on the surface of the NM fiber, and the particle size was about 5 μm. Figure 5 , it can be seen that after loading Pt and Ni(OH)2, the particles on the NM surface are stacked by a large number of whisker-like nanowires with a width of about 10 nm.
[0119] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0120] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for preparing a hydrogen evolution electrode with adjustable platinum loading, characterized in that: Comprising: By an electrodeposition method, an electrolyte is deposited on a substrate to form a base metal hydroxide loaded on the substrate, and platinum partially or fully loaded on the base metal hydroxide, thereby preparing a hydrogen evolution electrode with adjustable platinum loading. Wherein, the electrolyte contains platinum ions and ions of a base metal, the pH value of the electrolyte > 7, and the substrate contains the base metal.
2. The preparation method according to claim 1, characterized in that: The electrodeposition uses linear voltammetry, and the linear voltammetry satisfies at least one of the following conditions: (1) In the linear voltammetry, the voltage scanning range relative to the reversible hydrogen electrode is 0~-0.5V; (2) In the linear voltammetry, the number of cycles is: 0 < cycle ≤ 250 cycles, optionally: 20 ≤ cycle ≤ 250 cycles.
3. The preparation method according to claim 1 or 2, characterized in that: The electrolyte satisfies at least one of the following conditions: (1) In the electrolyte, the concentration of the platinum ions is 5mg / L~50mg / L; (2) In the electrolyte, the concentration of the ions of the base metal is 0.5g / L~1g / L; (3) The electrolyte further contains a pH adjusting reagent; Optionally, the pH adjusting reagent includes urea; Optionally, in the electrolyte, the concentration of the pH adjusting reagent is 1g / L~5g / L; (4) The electrolyte further contains anions; Optionally, the anions include at least one of chloride ions, nitrate ions and sulfate ions, and further optionally chloride ions; (5) The pH value of the electrolyte satisfies: 7.5 ≤ pH value ≤ 8.
5.
4. The preparation method according to claim 1 or 2, characterized in that: Satisfying at least one of the following conditions: (1) The source of the platinum ions includes at least one of platinum chloride and platinum nitrate, and optionally platinum chloride; (2) The source of the ions of the base metal includes at least one of chlorides, nitrate compounds and sulfate compounds of the ions of the base metal, and optionally chlorides of the ions of the base metal.
5. The preparation method according to claim 1 or 2, characterized in that: Also comprising: The hydrogen evolution electrode is heat-treated to decompose the base metal hydroxide into a base metal oxide; Optionally, the temperature of the heat treatment is T1, the decomposition temperature of the base metal hydroxide is T2, and T2 ≤ T1 ≤ T2 + 20°C.
6. The preparation method according to any one of claims 1 to 5, characterized in that The base metal includes nickel.
7. A hydrogen evolution electrode with adjustable platinum loading, characterized in that: Obtained by the preparation method according to any one of claims 1~5.
8. The hydrogen evolution electrode according to claim 7, characterized in that The hydrogen evolution electrode includes the substrate, an intermediate carrier loaded on the substrate, and platinum loaded on the intermediate carrier, and the intermediate carrier includes the base metal hydroxide or the base metal oxide; Optionally, the base metal hydroxide contains a whisker structure; Optionally, the base metal oxide contains a whisker structure; Optionally, the platinum contains a granular structure.
9. The hydrogen evolution electrode according to claim 7 or 8, characterized in that The platinum loading on the hydrogen evolution electrode is 0-0.16 mg / cm 2 , optional 0.01mg / cm 2 ~0.16mg / cm 2 .
10. An application of the hydrogen evolution electrode with adjustable platinum loading according to any one of claims 7~9 in hydrogen production from alkaline solution.