Shell, manufacturing method thereof and electronic equipment
By dividing the shielding agent area on the surface of the metal matrix and oxidizing and coloring one by one, the shell with colorful patterns and continuous surfaces is realized, which solves the problems of poor flatness of the oxide layer and difficulty in three-dimensional processing in the anodizing process, and improves the shell Beautifulness and touch.
Patent Information
- Application Number
- CN202310609769.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing anodizing process is difficult to achieve colorful patterns while processing three-dimensional shells, resulting in poor flatness of the oxide layer, affecting the touch and appearance.
The masking agent is applied to the surface of the metal matrix to form different processing areas, and the masking agent is removed one by one and oxidation, coloring and sealing treatment are carried out. Different types of masking agents and oxidation methods are used to achieve colorful patterns and continuous surfaces.
A shell with colorful patterns was obtained, and there was no difference in the surface of each oxide layer, which improved the aesthetics and touch of the shell, and solved the problem that traditional oxidation technology could not process a three-dimensional three-dimensional shell.
Smart Images

Figure CN119020838A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of material processing, and in particular to a housing and a manufacturing method thereof, and an electronic device. Background Art
[0002] Among packaging components, anodized shells are often widely used in various packaging structures, such as the shells of electronic devices, due to their excellent properties such as high hardness, good wear resistance, diverse colors, and high reliability. The anodizing process usually requires oxidation, dyeing, and sealing treatment in the anodizing tank to obtain an anodized layer with a specific color. However, the anodized layer obtained using the existing anodizing process has a relatively single color, and it is difficult to achieve colorful colors. The existing method has an anodized layer of two colors. During the production, the metal substrate is anodized once to form a first oxide layer with a first color on the surface of the metal substrate, and then a part of the first oxide layer is removed by CNC cutting or laser and other processes, and then a second anodization is performed to form a second oxide layer with a second color. There is usually a height difference between the first oxide layer and the second oxide layer, resulting in poor flatness of the entire anodized layer, which affects the touch and appearance when used as a packaging structure. Summary of the invention
[0003] The present application provides a shell, a manufacturing method thereof, and an electronic device. The shell obtained by the manufacturing method of the present application can have at least two colors, and the surface of the oxide layer corresponding to the different colors is a continuous surface without step difference, so as to improve the aesthetics of the shell when used as the shell of an electronic device.
[0004] In a first aspect, the present application provides a method for manufacturing a housing, the method comprising the following steps:
[0005] Step A), coating a shielding agent on the surface of the metal substrate to form a shielding layer, wherein the shielding layer is divided into at least two different processing areas;
[0006] Step B), removing the shielding agent in one of the processing areas, and oxidizing, coloring and sealing the metal substrate corresponding to the processing area;
[0007] Repeat step B until all the shielding layers are removed and all the metal substrates corresponding to the shielding layers are oxidized, colored and sealed.
[0008] The manufacturing method of the shell of the present application is to first apply a shielding agent on the surface of the metal substrate to form a shielding layer, and then divide the shielding layer into regions according to the pattern to be processed, which can be divided into at least two different processing regions. Then the metal substrate is oxidized for each processing region. When oxidizing the metal substrate, the shielding layer of one processing region is first removed, and the metal substrate corresponding to the processing region is oxidized, colored and sealed, and then the shielding layer of another processing region is removed, and the metal substrate of the processing region is oxidized until all the metal substrates corresponding to the processing regions are completely oxidized. Each processing region can correspond to an oxide layer of one color. Therefore, a shell with a colorful pattern can be obtained by using the manufacturing method of the present application, and the surface between each oxide layer can form a continuous surface.
[0009] In one implementation, the oxidation in the manufacturing method of the present application includes but is not limited to one of anodizing, film passivation, and micro-arc oxidation.
[0010] In one implementation, each processing area corresponds to a shielding agent, and different processing areas correspond to different types of shielding agents. By setting different types of shielding agents, the purpose of removing shielding layers of different processing areas one by one can be achieved.
[0011] In one implementation, the shielding agent includes one of a strong acid soluble shielding agent, a strong alkali soluble shielding agent, an organic soluble shielding agent, a photosensitive stripping shielding agent, and a heat-sensitive stripping shielding agent. Different processing areas can be provided with different types of shielding agents and adopt different dissolving methods to protect shielding agents in other processing areas from being affected.
[0012] In one implementation, the type of the shielding agent corresponding to different processing areas is the same, and the shielding agent is one of a photosensitive stripping type shielding agent and a heat-sensitive stripping type shielding agent. In this implementation, different processing areas correspond to the same shielding agent, and the shielding layer on the surface of the metal substrate is formed by the same shielding agent. At this time, the shielding agent needs to be selected from one of a photosensitive stripping type shielding agent and a heat-sensitive stripping type shielding agent. By selecting these two shielding agents, the shielding layer of different processing areas can be removed by using zoned irradiation or heating, thereby achieving oxidation of the metal substrate in different processing areas.
[0013] In one implementation, the removing of the shielding agent in one of the processing areas comprises: irradiating the processing area to be processed with ultraviolet rays or providing heat, shielding the remaining processing areas with a mask, and removing the shielding agent in the corresponding processing area after the shielding agent in the processing area to be processed is photosensitively cured or thermally cured. Using a mask to shield, fine processing of the pattern can be achieved.
[0014] In one implementation, the shielding layer is formed by printing, spraying, pad printing, silk screen printing, lamination, exposure and development, or other similar coating processes. The specific method of forming the shielding layer can be selected according to the type of shielding agent.
[0015] In one implementation, after forming the shielding layer and before removing the shielding agent from one of the processing areas, the oxidation method further includes the step of forming the metal substrate covered with the shielding layer. After the shielding agent is applied to form the shielding layer, the metal substrate may be formed to obtain a three-dimensional shell structure. This method can solve the problem that a three-dimensional shell cannot be processed while obtaining a colorful pattern in a conventional oxidation process.
[0016] In a second aspect, the present application provides a shell, which includes a metal substrate and an oxide layer provided on the surface of the metal substrate, the oxide layer includes at least two color regions, and the surface of the oxide layer corresponding to the different color regions facing away from the metal substrate is a continuous surface.
[0017] The shell of the present application has an oxide layer including at least two colors, which can effectively improve the appearance of the shell, solve the problem of the single appearance of the shell oxide layer, and achieve a colorful effect. In addition, in the oxide layer of the present application, the surface of the oxide layer corresponding to the different color areas is a continuous plane without step difference and boundary line, that is, the surface of the oxide layer corresponding to the different colors does not have the boundary line and drop of multiple surfaces, which can effectively improve the touch of the shell.
[0018] In one implementation, the shell is a three-dimensional shell. The three-dimensional shell can help to improve the diversity and application scope of the packaging structure. The color of the oxide layer can include at least three. Each color corresponds to one oxide layer. The surfaces of different oxide layers are all continuous surfaces. Among them, the oxide layer of the shell of the present application can be an anodic oxide layer, a film oxide layer or a micro-arc oxide layer.
[0019] In one implementation, the shell is a shell obtained using the manufacturing method of the present application.
[0020] In a third aspect, the present application provides an electronic device, which includes the housing of the present application.
[0021] The technical effects that can be achieved in the third aspect can be described with reference to the corresponding effects in the first and second aspects, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a structural schematic diagram of a shell;
[0023] Figure 2 A schematic diagram of a process for manufacturing a shell;
[0024] Figure 3 A schematic diagram of a method for manufacturing a housing according to an embodiment of the present invention;
[0025] Figure 4 This is a schematic diagram of the structure of a metal substrate after forming treatment in one embodiment;
[0026] Figure 5 A schematic diagram of a method for manufacturing a housing according to another embodiment;
[0027] Figure 6 FIG. 4 is a schematic diagram of the appearance of an oxide layer according to an embodiment of the present invention.
[0028] Reference numerals:
[0029] 11-metal substrate; 12-oxide layer; 121-first oxide layer; 122-second oxide layer; 123-third oxide layer;
[0030] 13- shielding layer; 14- processing area; 141- first processing area; 142- second processing area; 143- third processing area. DETAILED DESCRIPTION
[0031] In order to make the objectives, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings.
[0032] The terms used in the following embodiments are only for the purpose of describing specific embodiments and are not intended to be limiting of the present application. As used in the specification and appended claims of the present application, the singular expressions "a", "an", "above", "the" and "this" are intended to also include expressions such as "one or more", unless there is a clear contrary indication in the context.
[0033] References to "one embodiment" or "some embodiments" etc. described in this specification mean that a particular feature, structure or characteristic described in conjunction with the embodiment is included in one or more embodiments of the present application. Thus, the phrases "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear at different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.
[0034] The embodiment of the present application provides a shell. The shell can be used to form a packaging shell of an electronic device. The packaging shell can be an electronic device, such as a back cover of a mobile phone or a tablet computer. The material of the shell in the embodiment of the present application includes but is not limited to aluminum alloy, magnesium alloy or titanium alloy. The structure and processing and manufacturing process of the shell are explained below.
[0035] Figure 1 FIG. 1 is a schematic diagram of the structure of a shell. Figure 1 The shell may include a metal substrate 11 and an oxide layer 12 provided on the surface of the metal substrate 11. The metal substrate 11 includes but is not limited to an aluminum alloy substrate, a magnesium alloy substrate or a titanium alloy substrate. When the metal substrate 11 is an aluminum alloy substrate, the oxide layer 12 may be an aluminum oxide film layer. The oxide layer 12 may include at least two colors. The colors in the oxide layer 12 may be 2, 3 or more. The surface of the oxide layer 12 corresponding to each color may form a continuous surface. There is no misalignment or height difference in the thickness direction of the oxide layer 12 to avoid reducing the user's touch.
[0036] like Figure 1 As shown, the structure of the shell can be a three-dimensional structure, and a bending portion can be provided on the circumference of the plate surface of the shell. The surface of the bending portion can also be provided with an oxide layer 12. Among them, the oxide layer 12 can be an anodic oxide layer, a film oxide layer or a micro-arc oxide layer.
[0037] The structure of the housing is explained above, and the manufacturing process thereof will be explained below.
[0038] Figure 2 FIG. 1 is a schematic diagram of a method for manufacturing a shell. Figure 2 As shown, the manufacturing method of the embodiment of the present application includes the following steps:
[0039] Step S1, coating a shielding agent on the surface of a metal substrate 11 to form a shielding layer 13, wherein the shielding layer 13 can be divided into at least two different processing areas 14;
[0040] Step S2, remove the shielding agent in one of the processing areas 14, and oxidize, color and seal the metal substrate 11 corresponding to the processing area 14; repeat step B until all shielding layers 13 are removed and all metal substrates 11 corresponding to the shielding layers 13 are oxidized, colored and sealed. After all processing areas 14 are oxidized, each processing area 14 corresponds to an oxide layer 12 of a color, and the oxide layers 12 corresponding to each processing area 14 have different colors. The oxidation in the manufacturing method of the embodiment of the present application includes but is not limited to one of anodizing, film passivation or micro-arc oxidation.
[0041] In step S1, the shielding agent includes, but is not limited to, one of a strong acid soluble shielding agent, a strong alkali soluble shielding agent, an organic soluble shielding agent, a photosensitive stripping shielding agent, and a heat-sensitive stripping shielding agent. When the shielding agent is selected from a strong acid soluble shielding agent, a strong alkali soluble shielding agent, or an organic soluble shielding agent, each processing area 14 corresponds to a shielding agent, and different processing areas 14 correspond to different types of shielding agents. When the shielding agent is selected from a photosensitive stripping shielding agent or a heat-sensitive stripping shielding agent, different processing areas 14 may correspond to the same type of shielding agent.
[0042] Among them, strong acid soluble masking agents can remain intact in weak acid, weak alkali environment and strong alkali solvent, and can be dissolved and peeled off in strong acid solvent. Strong alkali soluble masking agents can remain intact in weak acid and weak alkali environment and strong acid solvent, and can be dissolved and peeled off in strong alkali solvent. Organic soluble masking agents can remain intact in strong acid, strong alkali and other organic solvents, and can be dissolved and peeled off in specific organic solvents. For example: alkyd and nitro paint masking agents can be removed by organic solvents such as ketones and benzene, and polyurethane, epoxy polyphthalamide or amino alkyd resin paint masking agents can be removed by chlorinated hydrocarbon paint strippers. Photosensitive stripping masking agents can maintain toughness and viscosity before specific light exposure, and can be cured and peeled off after receiving light of specific wavelength and energy. For example: adding a photoinitiator to the masking agent, UV curing and mercury lamp curing of the masking agent can be used for stripping. Thermosensitive stripping masking agents can remain intact in solvents at room temperature, and heating them to a specific temperature can achieve rapid stripping.
[0043] In the anodizing method of the embodiment of the present application, when different processing areas 14 use different masking agents, different dissolving agents can be used to distribute and dissolve the masking agents in different processing areas 14. When the same masking agent is used in different processing areas 14, the masking agents in different processing areas 14 can be distributed and removed by mask exposure.
[0044] In the embodiment of the present application, the method for forming the shielding layer 13 includes but is not limited to printing, spraying, pad printing or silk screen printing or other similar coating processes. The shielding layer 13 with a specific shape structure can also be formed by film pasting, exposure and development. When the shielding agent forming the shielding layer 13 is a strong acid soluble shielding agent, a strong alkali soluble shielding agent or an organic soluble shielding agent, the shielding layer 13 can be formed by printing, spraying, pad printing or silk screen printing. When the shielding agent is one of a photosensitive stripping shielding agent and a heat-sensitive stripping shielding agent, the shielding layer 13 can be formed by film pasting, exposure and development. Industrial printing, pad printing, and silk screen printing have high precision and can form high-precision graphics. In addition, after the oxide layer 12 is formed, the boundaries of different colors can be subjected to finishing processes such as laser engraving and CNC cutting to further improve the accuracy of the pattern.
[0045] When the shielding layer 13 is divided into different processing areas 14, the processing areas 14 can be divided according to the pattern to be processed. When the pattern to be processed is a complex pattern, the shielding layer 13 with a specific pattern can be formed on the surface of the metal substrate 11 by exposure and development.
[0046] Figure 3 FIG. 1 is a schematic diagram of a method for manufacturing a housing according to an embodiment of the present invention. Figure 3 As shown, the production method comprises the following steps:
[0047] Step S11 , providing a metal substrate 11 , which may be an aluminum alloy substrate, and performing a surface treatment process such as sandblasting, polishing or laser treatment on the metal substrate 11 to remove dirt, scratches, grains and other defects on the surface of the metal substrate 11 .
[0048] Step S12: using partition printing, inkjet printing, pad printing, silk screen printing or film lamination, and combining developing and exposing methods to coat the surface of the metal substrate 11 with a variety of different types of shielding agents, the shielding layer 13 formed by different shielding agents can form a fine and complex pattern. Each shielding layer 13 formed by a shielding agent corresponds to a processing area 14.
[0049] by Figure 3 The three shielding agents shown are used as examples for explanation. In the embodiment of the present application, the three shielding agents correspond to three processing areas 14, and each shielding agent corresponds to one processing area 14; the three shielding agents are shielding agent A, shielding agent B and shielding agent C. Among them, shielding agent A is soluble in solvent A, but insoluble in solvent B and solvent C; shielding agent B is soluble in solvent B, but insoluble in solvent A and solvent C; shielding agent C is soluble in solvent C, but insoluble in solvent A and solvent B.
[0050] Step S13, stamping the metal substrate 11 coated with the shielding layer 13.
[0051] Step S14, using solvent A to remove the shielding agent A corresponding to the first processing area 141, and performing anodizing, coloring and sealing treatment on the metal substrate 11 corresponding to the first processing area 141, so as to form a first oxide layer 121 in the first processing area 141;
[0052] Step S15, using solvent B to remove the shielding agent B corresponding to the second processing area 142, and performing anodizing, coloring and sealing treatment on the metal substrate 11 corresponding to the second processing area 142, so as to form a second oxide layer 122 in the second processing area 142;
[0053] Step S16: using solvent C to remove the shielding agent C corresponding to the third processing area 143, and performing anodizing, coloring and sealing treatment on the metal substrate 11 corresponding to the third processing area 143, so as to form a third oxide layer 123 in the third processing area 143. The first oxide layer 121, the second oxide layer 122 and the third oxide layer 123 are colored differently from each other.
[0054] The anodizing method of the embodiment of the present application is protected by the shielding layer 13 before the forming process, which can prevent the surface after sandblasting from being oxidized. Moreover, since the shielding layer 13 is an elastic layer, under the protection of the shielding layer 13, the metal substrate 11 can be first formed and then anodized to achieve the production of shells of different shapes. Figure 4 FIG. 1 is a schematic diagram of the structure of a metal substrate after forming in an embodiment. Figure 4 As shown, the metal matrix 11 can form a wavy irregular three-dimensional shape. The thickness of the metal matrix 11 can be the same or different at different locations, which is not specifically limited here.
[0055] In addition, the embodiment of the present application uses masking agents with different solubility properties, so that other parts of the metal substrate 11 are not affected during the process of making the oxide layer 12 corresponding to a processing area 14, so that other processing areas 14 of the metal substrate 11 maintain good integrity before anodizing, and a colorful effect is achieved by removing the masking agents at different positions one by one and processing oxide layers 12 of different colors. Therefore, the anodizing method of the present application solves the problem that the existing method cannot achieve unconventional shapes and colorful anode layers, and achieves the effect of three-dimensional processing and colorful oxide layers 12.
[0056] Among them, in step S12, in order to enhance the accuracy of the pattern formed by the shielding layer 13, multiple coating, exposure, development, demoulding and other processes may be performed to finally form a pattern of the shielding layer 13 with higher accuracy. In steps S14 to S16, when the oxidation treatment is anodizing treatment, anodizing can be performed in different types, such as sulfuric acid anodizing, phosphoric acid anodizing, or oxalic acid anodizing. In addition, in the coloring process, by performing dyeing and sealing of different colors in different processing areas, a combination effect of multiple colors and textures can be achieved.
[0057] It is understandable that the above embodiment only uses three shielding agents as examples for illustration, and the types of shielding agents are not limited in the embodiments of the present application. When more types of shielding agents are used to form the shielding layer 13, more colors and more complex patterns can be obtained.
[0058] Figure 5 FIG. 1 is a schematic diagram of a method for manufacturing a housing according to another embodiment. Figure 5 As shown, the production method comprises the following steps:
[0059] Step S11 , providing a metal substrate 11 , which may be an aluminum alloy substrate, and performing a surface treatment process such as sandblasting, polishing or laser treatment on the metal substrate 11 to remove dirt, scratches, grains and other defects on the surface of the metal substrate 11 .
[0060] Step S12, forming a shielding layer 13 on the entire surface of the metal substrate 11 by means of zone printing, spray painting, pad printing, silk screen printing or film laminating, the shielding layer 13 can be formed by the same shielding agent, and the shielding agent is a photosensitive stripping shielding agent or a heat-sensitive stripping shielding agent. The shielding agent selected in the embodiment of the present application is an ultraviolet light-sensitive stripping shielding agent.
[0061] Step S13, using laser engraving, punching half cutting, developing and exposing methods to segment the shielding layer 13 to form a fine and complex pattern. The shielding layer 13 is divided into different processing areas 14 according to the color of the pattern, such as Figure 5 As shown, the shielding layer 13 is divided into three processing areas 14 , which are respectively denoted as a first processing area 141 , a second processing area 142 and a third processing area 143 .
[0062] Step S14, stamping the metal substrate 11 coated with the shielding layer 13.
[0063] Step S15, removing the shielding agent of the first processing area 141: using a mask to cover the shielding layer 13 of the second processing area 142 and the third processing area 143, irradiating the shielding agent of the first processing area 141 with ultraviolet rays to cause a curing reaction and then peeling off, exposing the metal substrate 11 corresponding to the first processing area 141, and performing anodizing, coloring and sealing treatment on the part of the metal substrate 11, so as to form a first oxide layer 121 in the first processing area 141;
[0064] Step S16, removing the shielding agent in the second processing area 142: using a mask to cover the shielding layer 13 of the third processing area 143, irradiating the shielding agent in the second processing area 142 with ultraviolet light to cause a curing reaction and then peel off, exposing the metal substrate 11 corresponding to the second processing area 142, and performing anodizing, coloring and sealing treatment on the part of the metal substrate 11, so as to form a second oxide layer 122 in the second processing area 142;
[0065] Step S17, removing the shielding agent in the third processing area 143: irradiating the shielding agent in the third processing area 143 with ultraviolet light to cause a curing reaction and then peeling it off, exposing the metal substrate 11 corresponding to the third processing area 143, and performing anodizing, coloring and sealing treatment on the part of the metal substrate 11 to form a third oxide layer 123 in the third processing area 143. The colors of the first oxide layer 121, the second oxide layer 122 and the third oxide layer 123 are different from each other.
[0066] use Figure 3 or Figure 5 The process flow method shown can obtain Figure 6 The pattern shown. Figure 6 The pattern of the structure shown is exquisite and multiple color areas can be obtained. Among them, the obtained pattern can be a simple pattern, such as having three oxide layers ( Figure 6 The long strip combination pattern of the first oxide layer 121, the second oxide layer 122 and the third oxide layer 123 in the long strip part can also be an irregular pattern, such as a combination of three oxide layers ( Figure 6 A flower pattern is formed by the first oxide layer 121, the second oxide layer 122 and the third oxide layer 123 in the flower part.
[0067] The same masking agent is used to form a masking layer by coating once, and then laser engraving or stamping half-cut is used. When applying the masking agent, low-cost coating equipment such as brushing, silk screen printing, and lamination can be used. There is no need to use a high-precision industrial printer, which can save equipment costs and improve production efficiency. In addition, this method can easily realize the coating of masking agents on aluminum alloy coils, and then cutting, stamping, forming, anodizing and other processes, which greatly improves production efficiency and reduces costs, and can obtain a three-dimensional structure shell.
[0068] The shell of the embodiment of the present application may have a planar structure or a three-dimensional structure, and its oxide layer may have a pattern of two or more colors. In the process of manufacturing the shell, since the formation of the shielding layer can be achieved by high-precision printing, spray painting, pad printing, silk screen printing or film pasting, the pattern formed by the shielding layer is fine, has clear boundaries, and is highly designable. By removing the shielding layer of different processing areas once or multiple times, the obtained oxide layer also has the characteristics of clear pattern boundaries, and there are no obvious boundaries and step differences between the boundaries of oxide layers of different colors. The oxide layer obtained by anodizing, film passivation or micro-arc oxidation has high hardness and good wear resistance, and its reliability is comparable to the performance of conventional oxide layers.
[0069] Compared with CNC cutting or laser processing, the shell of the embodiment of the present application reduces cutting time and material waste, greatly reduces costs, and can achieve a colorful effect without borders and height differences. In conjunction with the stamping process, a colorful effect of a three-dimensional shape can be achieved. During the anodizing, coloring and sealing process, the formation of multiple color oxide layers can be completed in the equipment by hanging up and down once, and the plane graphics can be reworked multiple times, with high efficiency and yield, shortening the process flow, reducing quality abnormalities, improving yield, and reducing costs.
[0070] The shell of the embodiment of the present application can be used as a packaging shell for consumer electronic products such as tablet computers, laptop computers, and mobile phones, and can also be used as a packaging shell for automobiles, furniture, decorations, etc.
[0071] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for manufacturing a housing, characterized in that: include: Step A), coating a shielding agent on the surface of the metal substrate to form a shielding layer, wherein the shielding layer is divided into at least two different processing areas; Step B), removing the shielding agent in one of the processing areas, and oxidizing, coloring and sealing the metal substrate corresponding to the processing area; Repeat step B until all the shielding layers are removed and all the metal substrates corresponding to the shielding layers are oxidized, colored and sealed; Each of the processed areas corresponds to an oxide layer, and the oxide layers have different colors.
2. The method according to claim 1, characterized in that: Each of the processing areas corresponds to a shielding agent, and different processing areas correspond to different types of shielding agents.
3. The method according to claim 2, characterized in that: The shielding agent includes one of a strong acid soluble shielding agent, a strong alkali soluble shielding agent, an organic soluble shielding agent, a photosensitive stripping shielding agent, and a heat-sensitive stripping shielding agent.
4. The method according to claim 1, characterized in that: The types of the masking agents corresponding to the different processing areas are the same, and the masking agent is one of a photosensitive peeling type masking agent and a heat-sensitive peeling type masking agent.
5. The method according to claim 4, characterized in that: The removing of the masking agent in one of the processing areas comprises: The processing area to be processed is irradiated with ultraviolet rays or provided with heat, and the remaining processing area is shielded by a mask template. After the shielding agent in the processing area to be processed is photosensitively cured or thermally cured, the shielding agent in the corresponding processing area is removed.
6. The production method according to any one of claims 1 to 5, characterized in that: The method for forming the shielding layer includes: one of printing, spray painting, pad printing, silk screen printing, lamination or exposure and development.
7. The production method according to any one of claims 1 to 5, characterized in that: After forming the shielding layer and before removing the shielding agent in one of the processing areas, the manufacturing method further includes the step of performing a molding process on the metal substrate covered with the shielding layer.
8. The production method according to any one of claims 1 to 7, characterized in that: The oxidation includes one of anodic oxidation, film passivation, and micro-arc oxidation.
9. A housing, characterized in that: It comprises a metal substrate and an oxide layer arranged on the surface of the metal substrate, wherein the oxide layer comprises at least two color regions, and the surfaces of the oxide layer corresponding to the different color regions and away from the metal substrate are continuous surfaces.
10. The housing according to claim 9, characterized in that The shell is a three-dimensional shell.
11. The housing according to claim 9 or 10, characterized in that: The shell is obtained by the manufacturing method according to any one of claims 1 to 8.
12. An electronic device, characterized in that: Comprising a housing as described in any one of claims 9 to 11.