Ultrathin conductive glass fiber cloth and preparation method thereof
Through the coordinated structure of silver nanowires and single-wall carbon nanotube graphene, the problems of hole blocking and large resistance of the conductive layer of thin glass fiber cloth are solved, and ultra-thin without hole blocking, low square resistance value, and uniform coating on both sides are achieved. Conductive glass fiber cloth improves adhesion fastness and stability, and is suitable for large-scale production.
Patent Information
- Application Number
- CN202411379978.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the conductive layer of the thin glass fiber cloth is prone to cause hole blockage, has large resistance, and is difficult to apply uniformly on both sides, affecting its application performance.
A synergistic structure of silver nanowires and single-wall carbon nanotube graphene is adopted to form a conductive layer with low resistance and high resistance through impregnation coating, and a packaging layer is formed on it to ensure the uniformity and adhesion fastness of the conductive layer.
It realizes ultra-thin conductive fiber cloth with no plugging holes, low square resistance value, and uniform coating on both sides, which improves adhesion fastness and stability, and is suitable for large-scale production.
Smart Images

Figure HDA0005069655910000011 
Figure HDA0005069655910000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of glass fiber cloth preparation, and in particular relates to an ultra-thin conductive glass fiber cloth and a preparation method thereof. Background Art
[0002] The strength of glass fiber cloth mainly depends on the diameter and weaving density of the fiber. For thin glass fiber cloth, it is more susceptible to deformation due to external forces. In order to give glass fiber cloth efficient conductive and heating functions, a coating method can be used to directly construct a conductive functional structure on the surface of the fabric. This method has the advantages of simple process, easy control of conditions, and multiple conductive phase selectivity. It can also maximize the original structure of the fabric and improve the performance. Patent CN114258167A adheres the glass fiber cloth to the heating plate and uses a wire rod coating method to coat the carbon nanotubes on the glass fiber cloth. This not only makes the conductive glass fiber cloth have conductive properties on only one side and easily causes serious pore blocking problems, but also the prepared conductive layer has a large resistance and requires multiple coatings to reach 100Ω / sq, which brings troubles to the application of thin glass fiber cloth. Summary of the invention
[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide an ultra-thin conductive glass fiber cloth with no pore blockage, small coating thickness, low square resistance and uniform coating on both sides, and excellent coating adhesion, which is suitable for large-scale production.
[0004] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0005] The present invention provides an ultra-thin conductive glass fiber cloth, comprising an ultra-thin glass fiber base cloth, a conductive layer 1 formed on the ultra-thin glass fiber base cloth, a conductive layer 2 formed on the conductive layer 1, and an encapsulation layer formed on the conductive layer 2. The conductive component in the conductive layer 1 is silver nanowire, and the conductive component in the conductive layer 2 is single-walled carbon nanotube and graphene. The conductive layer 1 is formed by dip-coating a silver nanowire conductive ink, and the conductive layer 2 is formed by dip-coating a mixed conductive ink of single-walled carbon nanotube and graphene. Two conductive layers are formed on both the upper and lower surfaces of the glass fiber cloth by the dip-coating method, and the ink is also attached to the inner wall of the mesh of the fiber cloth to connect the upper and lower four conductive layers.
[0006] As a preference: the weight per unit area of the ultra-thin glass fiber base fabric is 20-48 g / m 2 , thickness is 0.02-0.1mm.
[0007] As a preference: the dry weight of the conductive layer 1 is 0.5-2 g / m 2, thickness is 0.8-2μm, resistance range is 5-50Ω / sq. The components of the conductive layer 1 are composed of 2-5 parts of silver nanowires, 0.3-2 parts of hydroxypropyl methylcellulose, 0.2-0.5 parts of polyvinyl pyrrolidone and 0.01-0.02 parts of polyethylene glycol octylphenyl ether in parts by weight. The diameter of the silver nanowire is 50-150nm and the length is 10-30μm. Further preferably, the diameter of the silver nanowire is 100-120nm and the length is 10-30μm.
[0008] As a preference: the coating dry weight of the conductive layer 2 is 0.5-1.5 g / m 2 , thickness is 0.5-2μm, resistance range is 5000-100000Ω. The components of the conductive layer 2 are composed of 1-3 parts of single-walled carbon nanotubes, 1-3 parts of graphene, 0.1-0.2 parts of sodium dodecyl sulfate and 1-5 parts of modified polyurethane by weight. The single-walled carbon nanotube has a diameter of 1-2nm and a length of 10-30μm. The graphene sheet has a diameter of ≤6μm and has 6-10 layers.
[0009] Preferably, the encapsulation layer is formed by dip coating encapsulation ink, and the dry weight of the coating is 0.5-1.5 g / m 2 The thickness is 0.5-1 μm. The components in the encapsulation layer are composed of 1-3 parts of modified polyurethane, 0.08-0.2 parts of aziridine crosslinking agent, and 0.1-0.5 parts of nano silicon dioxide by weight.
[0010] The method for preparing the ultra-thin conductive glass fiber cloth of the present invention comprises the following steps:
[0011] S1, cleaning and drying the ultra-thin glass fiber base cloth to obtain a clean ultra-thin glass fiber base cloth;
[0012] S2, mixing a silver nanowire dispersion containing 2-5 parts of silver nanowires, 0.3-2 parts of hydroxypropyl methylcellulose, 0.2-0.5 parts of polyvinyl pyrrolidone and 0.01-0.02 parts of polyethylene glycol octylphenyl ether in a mixed solvent consisting of 85-95 parts of water and 5-15 parts of ethanol to obtain a silver nanowire conductive ink; using an impregnation device to dip-coat the silver nanowire conductive ink on a clean ultra-thin glass fiber base cloth, and then sequentially performing post-treatment steps including extrusion, drying and cooling to obtain a glass fiber cloth coated with a conductive layer 1;
[0013] S3, mixing a carbon nanotube dispersion containing 1-3 parts of single-walled carbon nanotubes, a graphene dispersion containing 1-3 parts of graphene, 0.1-0.2 parts of sodium dodecyl sulfate and a modified polyurethane emulsion containing 1-5 parts of modified waterborne polyurethane in a mixed solvent consisting of 80-90 parts of water and 10-20 parts of ethanol to obtain a mixed conductive ink of single-walled carbon nanotubes and graphene; using an impregnation device to dip-coat the mixed conductive ink of single-walled carbon nanotubes and graphene on a glass fiber cloth coated with a conductive layer 1, and then sequentially performing post-treatment steps including extrusion, drying and cooling to obtain a glass fiber cloth coated with a conductive layer 1 and a conductive layer 2;
[0014] S4. Evenly mix a modified aqueous polyurethane emulsion containing 1-3 parts of modified polyurethane, 0.08-0.2 parts of aziridine crosslinking agent and a nano-silicon dioxide dispersion containing 0.1-0.5 parts of nano-silicon dioxide in a mixed solvent consisting of 70-80 parts of water and 10-20 parts of ethanol to obtain a packaging ink; use an impregnation device to dip-coat the packaging ink on the glass fiber cloth coated with the conductive layer 1 and the conductive layer 2, and then perform post-treatment steps including extrusion, drying and cooling in sequence to form a packaging layer to obtain an ultra-thin conductive glass fiber cloth.
[0015] Preferably, in step S2, step S3 and step S4, the immersion time of the immersion coating is 2-10 seconds, and the immersion speed is 1-5 m / min.
[0016] Preferably, in step S2, step S3 and step S4, the drying method is infrared heating drying, the drying temperature is 80-140° C., and the drying time is 4-20 seconds.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The ultra-thin conductive glass fiber cloth of the present invention adopts a structure in which a low-resistance conductive layer and a high-resistance conductive layer cooperate with each other:
[0019] The low-resistance conductive layer 1 uses thick silver nanowires as the conductive component. Compared with thin silver nanowires (diameter 10-50nm), the thick silver nanowires of the present invention have better conductivity, and a low square resistance can be achieved on the glass fiber cloth by one dip coating. The conductive ink with thick silver nanowires as the conductive component alone has excellent stability, uniform dip coating, and good adhesion. Among them, polyvinyl pyrrolidone increases the steric hindrance of the silver nanowires and reduces the agglomeration and sedimentation of the silver nanowires. Polyethylene glycol octylphenyl ether reduces the surface tension of the ink, improves the wetting and leveling properties on the surface of the glass fiber cloth, and makes the dip coating liquid film uniform. Hydroxypropyl methylcellulose wraps the silver nanowire network during the drying process, which not only increases the adhesion to the substrate, but also plays a certain protective role on the silver nanowires.
[0020] The high-resistance conductive layer 2 uses long carbon nanotubes and flaky graphene as conductive components, and utilizes the chemical and structural characteristics of the two to increase the overlap sites on the conductive layer 1 through dip coating, thereby forming an efficient electron transmission network that penetrates and overlaps each other, while improving the uniformity of square resistance, and combining the synergistic effect of the connecting resin material to improve the interface bonding force between the carbon nanotubes, graphene, silver nanowires and glass fiber bundles, so that the conductive layer has good adhesion and conductivity on the glass fiber cloth, and realizes the preparation of low-resistance conductive glass fiber cloth. In addition, the conductive layer 2 also takes into account the function of the encapsulation layer, and reduces the direct contact of the silver nanowires with the external environment and oxidation through the interlacing and embedding of the silver nanowires. At the same time, the two conductive inks will also adhere to the inner wall of the fiber cloth mesh to connect the upper and lower four conductive layers.
[0021] 2. The design of the encapsulation layer of the present invention further improves the adhesion strength of the coating on the glass fiber cloth, while ensuring that the carbon nanotubes, graphene and silver nanowires are not directly in contact with the outside, and the formed encapsulation layer has excellent temperature resistance and stability, which can significantly increase the stiffness of the glass fiber cloth, enhance the ability to resist deformation due to external forces, make the electronic transmission network more stable, and improve the storage and application stability of the conductive layer. At the same time, combined with the encapsulation effect of the conductive layer 2 on the conductive layer 1, only a thin layer is required to meet the application performance requirements.
[0022] 3. The present invention is suitable for ultra-thin conductive glass fiber cloth, and uses low-viscosity silver nanowire conductive ink and mixed conductive ink of single-walled carbon nanotubes and graphene to evenly coat the mesh-shaped ultra-thin conductive glass fiber cloth through a dip coating process, so that the square resistance uniformity is high and the coating thickness is thin. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is an optical magnifying glass photograph of the conductive glass fiber cloth in Example 1 of the present invention.
[0024] Figure 2 This is a real photo of the conductive glass fiber cloth in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] The present invention is described in detail below in conjunction with embodiments. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0026] The silver nanowires used in the following examples have a diameter of 100-120 nm, a length of 10-30 μm, and a model number of XFJ06, and the single-walled carbon nanotubes used have a diameter of 1-2 nm, a length of 10-30 μm, and a model number of XFS16-1, all of which were provided by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.
[0027] The graphene sheets used in the following examples have a diameter of ≤6 μm, a number of layers of 6-10, model WJ-GP550, and are produced by Hefei Microcrystalline Material Technology Co., Ltd.
[0028] The modified waterborne polyurethane emulsion used in the following examples was purchased from Yierfu Chemical (Shanghai) Co., Ltd., model PU-6155, with a solid content of 40%.
[0029] The nano-silicon dioxide dispersion used in the following examples is model VK-S01N, with a solid content of 25%, and was purchased from Xuancheng Jingrui New Materials Co., Ltd.
[0030] Hydroxypropyl methylcellulose, polyvinyl pyrrolidone, polyethylene glycol octylphenyl ether, sodium dodecyl sulfate, and aziridine crosslinking agent used in the following examples were all purchased from Sinopharm Chemical Reagent Co., Ltd.
[0031] Example 1
[0032] The present invention provides an ultra-thin conductive glass fiber cloth, comprising an ultra-thin glass fiber base cloth, a conductive layer 1 formed on the ultra-thin glass fiber base cloth, a conductive layer 2 formed on the conductive layer 1, and an encapsulation layer formed on the conductive layer 2. The preparation steps are as follows:
[0033] S1, ultra-thin glass fiber base cloth (weight per unit area 25g / m 2 , thickness 0.03mm) was washed with acetone and deionized water in turn, and then dried to obtain a clean ultra-thin glass fiber base cloth.
[0034] S2. Mix 4 parts of silver nanowire dispersion containing silver nanowires, 1 part of hydroxypropyl methylcellulose, 0.5 parts of polyvinyl pyrrolidone and 0.02 parts of polyethylene glycol octyl phenyl ether in a mixed solvent consisting of 90 parts of water and 10 parts of ethanol to obtain silver nanowire conductive ink. Use an impregnation device to dip-coat the silver nanowire conductive ink on the clean silver nanowire conductive ink, and then perform post-treatment steps including extrusion, drying and cooling in sequence to obtain a glass fiber cloth coated with a conductive layer 1. The dry weight of the conductive layer 1 is 0.8g / m 2 , thickness is 1.0μm.
[0035] S3. Evenly mix a carbon nanotube dispersion containing 3 parts of single-walled carbon nanotubes, a graphene dispersion containing 1 part of graphene, 0.2 parts of sodium dodecyl sulfate and a modified polyurethane emulsion containing 5 parts of modified polyurethane in a mixed solvent consisting of 80 parts of water and 20 parts of ethanol to obtain a mixed conductive ink of single-walled carbon nanotubes and graphene. The mixed conductive ink of single-walled carbon nanotubes and graphene is dip-coated on a glass fiber cloth coated with a conductive layer 1 by using an impregnation device, and then post-treatment steps including extrusion, drying and cooling are sequentially performed to obtain a glass fiber cloth coated with a conductive layer 1 and a conductive layer 2. The dry weight of the conductive layer 2 coating is 1.4 g / m 2 , thickness is 1.8μm.
[0036] S4. Mix a modified aqueous polyurethane emulsion containing 1.5 parts of modified polyurethane, 0.12 parts of aziridine crosslinking agent and a nano-silicon dioxide dispersion containing 0.5 parts of nano-silicon dioxide in a mixed solvent consisting of 80 parts of water and 10 parts of ethanol to obtain a packaging ink. Use an impregnation device to dip-coat the packaging ink on the glass fiber cloth coated with the conductive layer 1 and the conductive layer 2, and then perform post-treatment steps including extrusion, drying and cooling in sequence to form a packaging layer to obtain an ultra-thin conductive glass fiber cloth. The coating dry weight of the packaging layer is 0.8g / m 2 , thickness is 0.6μm.
[0037] In step S2, step S3 and step S4: the immersion time of the immersion coating is 5 seconds, and the immersion speed is 2 m / min; the drying method is infrared heating drying, the drying temperature is 120° C., and the drying time is 10 seconds.
[0038] Example 2
[0039] The present invention provides an ultra-thin conductive glass fiber cloth, comprising an ultra-thin glass fiber base cloth, a conductive layer 1 formed on the ultra-thin glass fiber base cloth, a conductive layer 2 formed on the conductive layer 1, and an encapsulation layer formed on the conductive layer 2. The preparation steps are as follows:
[0040] S1, ultra-thin glass fiber base cloth (weight per unit area 48g / m 2 , thickness 0.1mm) was washed with acetone and deionized water in turn, and then dried to obtain a clean ultra-thin glass fiber base cloth.
[0041] S2. Mix 5 parts of silver nanowire dispersion containing silver nanowires, 2 parts of hydroxypropyl methylcellulose, 0.5 parts of polyvinyl pyrrolidone and 0.02 parts of polyethylene glycol octylphenyl ether in a mixed solvent consisting of 85 parts of water and 15 parts of ethanol to obtain silver nanowire conductive ink. Use an impregnation device to dip-coat the silver nanowire conductive ink on a clean ultra-thin glass fiber base cloth, and then perform post-treatment steps including extrusion, drying and cooling in sequence to obtain a glass fiber cloth coated with a conductive layer 1. The dry weight of the conductive layer 1 is 1.8 g / m 2 , thickness is 2μm.
[0042] S3. Evenly mix a carbon nanotube dispersion containing 2 parts of single-walled carbon nanotubes, a graphene dispersion containing 2 parts of graphene, 0.2 parts of sodium dodecyl sulfate and a modified polyurethane emulsion containing 4 parts of modified polyurethane in a mixed solvent consisting of 90 parts of water and 10 parts of ethanol to obtain a mixed conductive ink of single-walled carbon nanotubes and graphene. The mixed conductive ink of single-walled carbon nanotubes and graphene is dip-coated on a glass fiber cloth coated with a conductive layer 1 using an impregnation device, and then post-treatment steps including extrusion, drying and cooling are sequentially performed to obtain a glass fiber cloth coated with a conductive layer 1 and a conductive layer 2. The dry weight of the conductive layer 2 coating is 1.1 g / m 2 , thickness is 1.5μm.
[0043] S4. Mix a modified aqueous polyurethane emulsion containing 3 parts of modified polyurethane, 0.2 parts of aziridine crosslinking agent and a nano-silicon dioxide dispersion containing 0.3 parts of nano-silicon dioxide in a mixed solvent consisting of 70 parts of water and 20 parts of ethanol to obtain a packaging ink. Use an impregnation device to dip-coat the packaging ink on the glass fiber cloth coated with the conductive layer 1 and the conductive layer 2, and then perform post-treatment steps including extrusion, drying and cooling in sequence to form a packaging layer to obtain an ultra-thin conductive glass fiber cloth. The coating dry weight of the packaging layer is 1.1g / m 2 , thickness is 1μm.
[0044] In step S2, step S3 and step S4: the immersion time of the immersion coating is 10 seconds, and the immersion speed is 1 m / min; the drying method is infrared heating drying, the drying temperature is 80° C., and the drying time is 20 seconds.
[0045] Example 3
[0046] The present invention provides an ultra-thin conductive glass fiber cloth, comprising an ultra-thin glass fiber base cloth, a conductive layer 1 formed on the ultra-thin glass fiber base cloth, a conductive layer 2 formed on the conductive layer 1, and an encapsulation layer formed on the conductive layer 2. The preparation steps are as follows:
[0047] S1, ultra-thin glass fiber base cloth (weight per unit area 20g / m 2, thickness 0.02mm) was washed with acetone and deionized water in turn, and then dried to obtain a clean ultra-thin glass fiber base cloth.
[0048] S2. Mix 2 parts of silver nanowire dispersion containing silver nanowires, 0.3 parts of hydroxypropyl methylcellulose, 0.25 parts of polyvinyl pyrrolidone and 0.01 parts of polyethylene glycol octylphenyl ether in a mixed solvent consisting of 95 parts of water and 5 parts of ethanol to obtain silver nanowire conductive ink. Use an impregnation device to dip-coat the silver nanowire conductive ink on a clean ultra-thin glass fiber base cloth, and then perform post-treatment steps including extrusion, drying and cooling in sequence to obtain a glass fiber cloth coated with a conductive layer 1. The dry weight of the conductive layer 1 is 0.8g / m 2 , thickness is 0.9μm.
[0049] S3. Evenly mix a carbon nanotube dispersion containing 1 part of single-walled carbon nanotubes, a graphene dispersion containing 3 parts of graphene, 0.1 part of sodium dodecyl sulfate and a modified polyurethane emulsion containing 1 part of modified polyurethane in a mixed solvent consisting of 80 parts of water and 20 parts of ethanol to obtain a mixed conductive ink of single-walled carbon nanotubes and graphene. The mixed conductive ink of single-walled carbon nanotubes and graphene is dip-coated on a glass fiber cloth coated with a conductive layer 1 by using an impregnation device, and then post-treatment steps including extrusion, drying and cooling are sequentially performed to obtain a glass fiber cloth coated with a conductive layer 1 and a conductive layer 2. The dry weight of the conductive layer 2 coating is 0.6 g / m 2 , thickness is 0.5μm.
[0050] S4. Evenly mix a modified aqueous polyurethane emulsion containing 1 part of modified polyurethane, 0.08 parts of aziridine crosslinking agent and a nano-silicon dioxide dispersion containing 0.1 parts of nano-silicon dioxide in a mixed solvent consisting of 80 parts of water and 10 parts of ethanol to obtain a packaging ink. The packaging ink is dip-coated on the glass fiber cloth coated with the conductive layer 1 and the conductive layer 2 using an impregnation device, and then post-processing steps including extrusion, drying and cooling are sequentially performed to form a packaging layer to obtain an ultra-thin conductive glass fiber cloth. The coating dry weight of the packaging layer is 0.6 g / m 2 , thickness is 0.5μm.
[0051] In step S2, step S3 and step S4: the immersion time of the immersion coating is 2 seconds, and the immersion speed is 5 m / min; the drying method is infrared heating drying, the drying temperature is 140° C., and the drying time is 4 seconds.
[0052] Comparative Example 1
[0053] In this comparative example, conductive glass fiber cloth is prepared in the same manner as in Example 1, with the only difference being that step S2 is not performed when preparing the conductive glass fiber cloth, and in step S3, a mixed conductive ink of single-walled carbon nanotubes and graphene is directly dip-coated on the ultra-thin glass fiber base cloth cleaned in step S1 to form a conductive glass fiber cloth having only a conductive layer 2.
[0054] Comparative Example 2
[0055] In this comparative example, the conductive glass fiber cloth is prepared in the same manner as in Example 1, with the only difference being that when preparing the conductive glass fiber cloth, step S3 is not performed, and in step S4, the encapsulation ink is directly dip-coated on the glass fiber cloth coated with the conductive layer 1 in step S2 to form a conductive glass fiber cloth having only the conductive layer 1.
[0056] Comparative Example 3
[0057] In this comparative example, the conductive glass fiber cloth was prepared in the same manner as in Example 1, except that step S4 was not performed during the preparation of the conductive glass fiber cloth.
[0058] Comparative Example 4
[0059] In this comparative example, the conductive glass fiber cloth was prepared in the same manner as in Example 1, except that step S3 and step S4 were not performed during the preparation of the conductive glass fiber cloth.
[0060] Comparative Example 5
[0061] In this comparative example, the conductive glass fiber cloth was prepared in the same manner as in Example 1, except that: when preparing the conductive glass fiber cloth, the two conductive inks in step S2 and step S3 were mixed and coated together, and the dry weight of the coating of the mixed conductive layer formed was 2.0 g / m 2 , thickness is 1.9μm.
[0062] The properties of the conductive glass fiber cloths obtained in the above-mentioned embodiments and comparative examples were tested and compared according to the following testing methods. The results are shown in Table 1.
[0063] (1) Coating dry weight: The obtained conductive glass fiber cloth was cut into three square samples of 100 mm × 100 mm and weighed on an electronic balance with an accuracy of 0.0001 g. The arithmetic mean of the coating dry weight was calculated, and the gram weight of the final conductive glass fiber cloth and its gram weight increase compared with the original ultra-thin glass fiber base cloth were obtained.
[0064] (2) Thickness: The thickness of the conductive glass fiber cloth obtained was measured at 8 different positions using a thickness meter, and the arithmetic mean was calculated. The thickness increase compared with the original ultra-thin glass fiber base cloth was also calculated.
[0065] (3) Square resistance and coefficient of variation: The obtained conductive glass fiber cloth was cut into test samples with a length of 250 mm and a width of 200 mm. The A side and the B side were marked and each was evenly divided into 20 test areas. The square resistance of each area was tested using a four-probe tester, and the arithmetic mean and coefficient of variation were calculated.
[0066] (4) Adhesion fastness: The obtained conductive glass fiber cloth was subjected to the 3M tape test method to evaluate the coating adhesion fastness.
[0067] (5) Heating temperature: The obtained conductive glass fiber cloth was cut into square samples of 100 mm × 100 mm, and conductive silver paste was coated on the opposite sides in the length direction. After drying and cooling, the cloth was connected to an AC voltage regulating power supply. At the same time, an infrared imager was used to detect the heating temperature of the conductive glass fiber cloth. After power was turned on, the output working voltage was slowly increased and adjusted to a heating target temperature of 120°C.
[0068] (6) Heating time: The rated working voltage is applied to the sample to be tested, and the heating temperature of the conductive glass fiber cloth is detected by an infrared imager. The heating curve from room temperature to the stable state of the target temperature is recorded. The time required to rise from room temperature to 90% (108°C) of the target temperature is taken as the heating time.
[0069] (7) Resistance change rate after repeated heating: Apply the rated working voltage to the sample to be tested, power it on continuously for 16 hours, then turn it off and cool it down for 8 hours. After repeatedly powering it on and off 25 times, use a multimeter to measure the resistance at both ends of the electrode and calculate the resistance change rate.
[0070] The test results of the above embodiments and comparative examples are shown in Table 1.
[0071] Table 1
[0072] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 <![CDATA[Grammage (g / m 2 )]]> 28.1 51.8 22.2 27.4 26.4 27.3 25.9 27.1 Weight increase (%) 12.0% 8.4% 9.9% 9.2% 5.2% 8.8% 3.2% 8.0% Thickness(μm) 33.4 104.5 21.9 31.9 31.4 32.8 31 31.9 Thickness increase (%) 11.3% 4.5% 9.5% 6.3% 4.7% 9.3% 3.3% 6.3% Average square resistance of A surface (Ω / sq) 15.9 8.7 22.6 14930 23.6 14.2 28.7 2048 A surface square resistance variation coefficient (%) 7.12 8.3 7.89 6.27 18.58 12.0 16.36 10.62 Average square resistance of B surface (Ω / sq) 12.7 8.4 23.4 16470 28.7 18.2 27.3 2293 Coefficient of variation of surface resistance of B surface (%) 6.47 6.3 7.23 7.98 17.69 13.7 18.24 11.57 Adhesion fastness No shedding No shedding No shedding No shedding - No shedding - No shedding Heating temperature (120℃) Stablize Stablize Stablize - Stablize Stablize Stablize Stablize Heating time(s) 59 55 68 - 48 56 46 72 Repeated heating resistance change rate (%) 2.5% 2.3% 2.7% - 61.9% 23.2% 235.5% 8.0%
[0073] It can be seen from Table 1 that:
[0074] (1) The results of Examples 1-3 show that the conductive glass fiber cloth of the present invention has the characteristics of small increase in gram weight and thickness, low square resistance, excellent coating adhesion, etc., can heat up quickly, and has high repeated heating stability.
[0075] (2) The results of comparative example 1 show that when carbon nanotubes and graphene are impregnated alone as conductive materials, their resistance value is large due to the influence of wetting dispersants, film-forming resins and other substances, and a higher output voltage is required to generate heat at 120°C.
[0076] (3) The sample in Comparative Example 2 was not impregnated with the mixed conductive ink of single-walled carbon nanotubes and graphene, and its square resistance variation coefficient was large, the uniformity was insufficient, and the resistance change rate after repeated heating was large.
[0077] (4) In comparative example 3, the samples were not immersed in encapsulation ink, and the adhesion strength of the conductive ink coating met the requirements. However, after being prepared into a heating element and powered on for heating, the resistance increased to a certain extent. This also shows that the conductive layer 2 also plays the role of an encapsulation layer.
[0078] (5) When silver nanowires were immersed alone in comparative example 4, their uniformity of square resistance was relatively poor, and their resistance increased more seriously after being energized and heated. At the same time, the experiment also found that although the square resistance data of the glass fiber cloth surface was low, its stability was poor. The resistance data of the same position increased sharply to the megohm level after repeated measurement. This was because the silver nanowires broke after being compressed, causing the conductive network to fail.
[0079] (6) In Comparative Example 5, the two conductive inks were mixed and then dipped and coated together, which could achieve the conductive function of the glass fiber cloth. However, its resistance was relatively large and the resistance change rate after repeated heating was relatively large. Even after multiple dips, its resistance had a lower limit and could not achieve the goal of low resistance. In addition, the stability of the mixed ink system was relatively poor, and there was agglomeration and precipitation.
[0080] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An ultra-thin conductive glass fiber cloth, characterized in that: It comprises an ultra-thin glass fiber base cloth, a conductive layer 1 formed on the ultra-thin glass fiber base cloth, a conductive layer 2 formed on the conductive layer 1, and a packaging layer formed on the conductive layer 2; The conductive component in the conductive layer 1 is silver nanowires, and the conductive component in the conductive layer 2 is single-walled carbon nanotubes and graphene.
2. The ultra-thin conductive glass fiber cloth according to claim 1, characterized in that: The ultra-thin glass fiber base fabric has a unit area weight of 20-48 g / m 2 , thickness is 0.02-0.1mm.
3. The ultra-thin conductive glass fiber cloth according to claim 1, characterized in that: The dry weight of the conductive layer 1 is 0.5-2 g / m 2 , with a thickness of 0.8-2 μm; the components of the conductive layer 1 are composed by weight: 2-5 parts of silver nanowires, 0.3-2 parts of hydroxypropyl methylcellulose, 0.2-0.5 parts of polyvinyl pyrrolidone and 0.01-0.02 parts of polyethylene glycol octylphenyl ether.
4. The ultra-thin conductive glass fiber cloth according to claim 3, characterized in that: The silver nanowire has a diameter of 50-150 nm and a length of 10-30 μm.
5. The ultra-thin conductive glass fiber cloth according to claim 1, characterized in that: The dry weight of the conductive layer 2 is 0.5-1.5 g / m 2 , with a thickness of 0.5-2 μm; the components of the conductive layer 2 are composed by weight: 1-3 parts of single-walled carbon nanotubes, 1-3 parts of graphene, 0.1-0.2 parts of sodium dodecyl sulfate and 1-5 parts of modified polyurethane.
6. The ultra-thin conductive glass fiber cloth according to claim 5, characterized in that: The single-walled carbon nanotube has a diameter of 1-2 nm and a length of 10-30 μm; the graphene sheet has a diameter of ≤6 μm and has 6-10 layers.
7. The ultra-thin conductive glass fiber cloth according to claim 1, characterized in that: The coating dry weight of the encapsulation layer is 0.5-1.5 g / m 2 , with a thickness of 0.5-1 μm; the components of the encapsulation layer are composed of: 1-3 parts of modified polyurethane, 0.08-0.2 parts of aziridine crosslinking agent, and 0.1-0.5 parts of nano-silicon dioxide in parts by weight.
8. A method for preparing the ultra-thin conductive glass fiber cloth according to any one of claims 1 to 7, characterized in that: The steps include: S1, cleaning and drying the ultra-thin glass fiber base cloth to obtain a clean ultra-thin glass fiber base cloth; S2, mixing a silver nanowire dispersion containing 2-5 parts of silver nanowires, 0.3-2 parts of hydroxypropyl methylcellulose, 0.2-0.5 parts of polyvinyl pyrrolidone and 0.01-0.02 parts of polyethylene glycol octylphenyl ether in a mixed solvent consisting of 85-95 parts of water and 5-15 parts of ethanol to obtain a silver nanowire conductive ink; dip-coating the silver nanowire conductive ink on a clean ultra-thin glass fiber base cloth, and then sequentially performing post-treatment steps including extrusion, drying and cooling to obtain a glass fiber cloth coated with a conductive layer 1; S3, uniformly mixing a carbon nanotube dispersion containing 1-3 parts of single-walled carbon nanotubes, a graphene dispersion containing 1-3 parts of graphene, 0.1-0.2 parts of sodium dodecyl sulfate and a modified aqueous polyurethane emulsion containing 1-5 parts of modified polyurethane in a mixed solvent consisting of 80-90 parts of water and 10-20 parts of ethanol to obtain a mixed conductive ink of single-walled carbon nanotubes and graphene; dip-coating the mixed conductive ink of single-walled carbon nanotubes and graphene on a glass fiber cloth coated with a conductive layer 1, and then sequentially performing post-treatment steps including extrusion, drying and cooling to obtain a glass fiber cloth coated with a conductive layer 1 and a conductive layer 2; S4. Evenly mix a modified aqueous polyurethane emulsion containing 1-3 parts of modified polyurethane, 0.08-0.2 parts of aziridine crosslinking agent and a nano-silicon dioxide dispersion containing 0.1-0.5 parts of nano-silicon dioxide in a mixed solvent consisting of 70-80 parts of water and 10-20 parts of ethanol to obtain a packaging ink; dip-coat the packaging ink on a glass fiber cloth coated with a conductive layer 1 and a conductive layer 2, and then sequentially perform post-treatment steps including extrusion, drying and cooling to form a packaging layer to obtain an ultra-thin conductive glass fiber cloth.
9. The preparation method according to claim 8, characterized in that: In step S2, step S3 and step S4, the immersion time of the immersion coating is 2-10 seconds, and the immersion speed is 1-5 m / min.
10. The preparation method according to claim 8, characterized in that: In step S2, step S3 and step S4, the drying method is infrared heating drying, the drying temperature is 80-140° C., and the drying time is 4-20 seconds.
Citation Information
Cited By
Conductive heating graphene glass fiber cloth and preparation method thereof
CN120989903A