Non-woven fabric for acid and alkali resistant reverse osmosis nanofiltration membrane and preparation method of non-woven fabric

The synergistic effect of polyolefin composite fibers, polypropylene fibers and aramid fibers is solved by the composite melt spinning method, and the problems of poor acid and alkali resistance of polyester fibers in acid and alkali environments and insufficient strength of polyolefin fibers are solved. The reverse osmosis nanofiltration membrane non-woven fabric is achieved with excellent acid and alkali resistance and good mechanical properties, which simplifies the preparation process and reduces the thickness.

CN119021036AActive Publication Date: 2024-11-26ANHUI QINGLAN NEW MATERIAL TECH CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411268968.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-26
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing polyester fiber non-woven fabrics have poor acid and alkali resistance in acid-base corrosive environments, and the non-woven fabrics prepared by polyolefin fibers are insufficient in strength and unstable in form, which limits the application of reverse osmosis nanofiltration membranes. The existing double-layer The structure preparation process is complex and has a large thickness, which affects the application effect of the film.

Method used

The composite melt spinning method is used to prepare polyolefin composite fibers with a skin core structure, combined with polypropylene fibers and aramid fibers, and the fiber ratio and temperature are adjusted through web formation, drying and hot pressing treatment to form acid-base-resistant reverse osmosis. Non-woven fabric for nanofiltration membrane.

Benefits of technology

Non-woven fabric for reverse osmosis nanofiltration membrane with excellent acid and alkali resistance, good mechanical properties, smooth surface and high stability were obtained to meet actual production and application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005038092130000071
    Figure BDA0005038092130000071
  • Figure BDA0005038092130000081
    Figure BDA0005038092130000081
  • Figure BDA0005038092130000082
    Figure BDA0005038092130000082
Patent Text Reader

Abstract

The invention provides non-woven fabric for an acid and alkali resistant reverse osmosis nanofiltration membrane and a preparation method of the non-woven fabric, and relates to the technical field of non-woven fabric for a separation membrane. Polyethylene master batch is used as a skin layer material, polypropylene master batch is used as a core layer material, and a polyolefin composite fiber with a skin-core structure is prepared by adopting a composite melt spinning method; then fully dispersing the polypropylene fiber, the aramid fiber and the polyolefin composite fiber in water according to a preset proportion, and carrying out papermaking and netting, drying and hot-pressing treatment to obtain the non-woven fabric which simultaneously contains the polypropylene fiber, the aramid fiber and the polyolefin composite fiber and is used for the acid and alkali resistant reverse osmosis nanofiltration membrane. Through the mode, the aramid fibers and the polypropylene fibers can be tightly connected through the polyolefin composite fibers by utilizing the synergistic effect of the fibers, so that the non-woven fabric for the reverse osmosis nanofiltration membrane, which is excellent in acid and alkali resistance, good in mechanical property, smooth in surface and good in air permeability, is prepared in a simple, convenient and efficient mode; and the requirements of actual production and application are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-woven fabrics for separation membranes, and in particular to a non-woven fabric for acid-base resistant reverse osmosis nanofiltration membrane and a preparation method thereof. Background Art

[0002] Polyester fiber nonwoven fabric has certain heat resistance and high mechanical properties, and is currently the most commonly used nonwoven fabric for reverse osmosis nanofiltration membrane. However, due to the poor acid and alkali resistance of polyester fiber nonwoven fabric, it is difficult to be used in special environments with strong acid and alkali corrosion, which greatly limits the application of reverse osmosis nanofiltration membrane using polyester fiber nonwoven fabric as the supporting layer substrate.

[0003] Compared with polyester fibers, polyolefin fibers have excellent chemical resistance and good mechanical properties, and are inexpensive and easy to process. If they are used in the preparation of non-woven fabrics for reverse osmosis nanofiltration membranes, they are beneficial to improving the acid and alkali resistance of reverse osmosis nanofiltration membranes. However, when non-woven fabrics made from polyolefin fibers are used as the support layer substrate of reverse osmosis nanofiltration membranes, they still have problems such as insufficient strength, unstable shape, and easy bending. In addition, they are prone to inward shrinkage during hot pressing, which affects the coating of the subsequent filtration layer.

[0004] In the prior art, the patent with publication number CN106582313A provides a double-layer alkali-resistant separation membrane support material and a preparation method thereof. The patent designs the separation membrane support material as a double-layer structure, including a coating layer and a support layer. Among them, the coating layer is made of fine-diameter polypropylene fiber and hot-melt fiber as raw materials, and the support layer is made of coarse-diameter polypropylene fiber and a certain amount of hot-melt fiber as raw materials. After pulping, pulping and other process steps, different pulp supply systems are respectively transported to the double-layer molding wet process equipment to make a net, and then water spunlace and hot rolling calendaring are formed to prepare a double-layer separation membrane support material with excellent alkali resistance, good interlayer bonding, excellent mechanical properties, stable morphological structure and moderate rigidity and flexibility. However, this method not only has a complicated preparation process, but also requires a two-layer structure to ensure the mechanical properties of the support material. The obtained support material is relatively thick, which affects the application of reverse osmosis nanofiltration membranes.

[0005] In view of this, it is necessary to design an improved acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane and a preparation method thereof to solve the above problems. Summary of the invention

[0006] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide an acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane and a preparation method thereof, and to prepare a non-woven fabric for reverse osmosis nanofiltration membrane with excellent acid and alkali resistance, good mechanical properties, smooth surface and high stability in a simple and efficient manner by synergistically improving the fiber composition and preparation process of the non-woven fabric.

[0007] To achieve the above object, the present invention provides a method for preparing an acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane, comprising the following steps:

[0008] S1. Using polyethylene masterbatch as the skin material and polypropylene masterbatch as the core material, a polyolefin composite fiber with a skin-core structure was prepared by a composite melt spinning method;

[0009] S2. The polypropylene fiber, the aramid fiber and the polyolefin composite fiber obtained in step S1 are fully dispersed in water according to a predetermined ratio to obtain a fiber slurry;

[0010] S3. Sheeting the fiber slurry obtained in step S2 into a fiber web, and drying the fiber web;

[0011] S4. The fiber web after drying is subjected to heat pressing treatment to obtain an acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane.

[0012] As a further improvement of the present invention, in step S2, in the fiber slurry, the mass ratio of the polypropylene fiber, the polyolefin composite fiber and the aramid fiber is 40% to 60%: 20% to 40%: 10% to 20%.

[0013] As a further improvement of the present invention, in step S2, the length of the polypropylene fiber is 3 to 6 mm, the length of the aramid fiber is 3 to 5 mm, and the length of the polyolefin composite fiber is 3 to 4 mm.

[0014] As a further improvement of the present invention, in step S1, the mass ratio of the skin layer material to the core layer material is 45% to 50%: 50% to 55%.

[0015] As a further improvement of the present invention, in step S1, the melting point of the skin layer material is 125-135°C, and the melting point of the core layer material is 165-170°C.

[0016] As a further improvement of the present invention, in step S3, the temperature of the drying process is 120-130°C.

[0017] As a further improvement of the present invention, in step S4, the hot pressing treatment includes hard calendering treatment and soft calendering treatment performed sequentially; the hot pressing temperature of the hard calendering treatment is 130-160°C, and the temperature of the soft calendering treatment is 145-155°C.

[0018] As a further improvement of the present invention, in step S2, the total mass concentration of each fiber in the fiber slurry is 0.5% to 1%.

[0019] As a further improvement of the present invention, in step S2, a dispersant and a defoaming agent are also added to the fiber slurry.

[0020] To achieve the above objectives, the present invention also provides an acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane, which is prepared according to any of the above technical solutions and includes polypropylene fibers, aramid fibers and polyolefin composite fibers.

[0021] The beneficial effects of the present invention are:

[0022] The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane provided by the present invention comprises preparing a polyolefin composite fiber with a skin-core structure, blending the polyolefin composite fiber with polypropylene fiber and aramid fiber, and then forming a web, drying, and hot pressing to obtain the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane containing polypropylene fiber, aramid fiber and polyolefin composite fiber. During the preparation process, the present invention further regulates the length and proportion of each fiber, and at the same time adjusts the temperature of the drying and hot pressing process, so that the polyolefin composite fiber evenly distributed between the polypropylene fiber and the aramid fiber can have a better bonding effect, and uses aramid fiber to fix the polypropylene fiber to prevent the nonwoven fabric from shrinking, thereby improving the structural stability, air permeability and mechanical properties of the nonwoven fabric. The acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane prepared by the method provided by the present invention has the advantages of excellent acid and alkali resistance, good mechanical properties, smooth surface, good air permeability, etc., and can meet the needs of actual production and application. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below in conjunction with specific embodiments.

[0024] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0025] The present invention provides a method for preparing a non-woven fabric for an acid- and alkali-resistant reverse osmosis nanofiltration membrane, comprising the following steps:

[0026] S1. Using polyethylene masterbatch as the skin material and polypropylene masterbatch as the core material, a polyolefin composite fiber with a skin-core structure was prepared by a composite melt spinning method;

[0027] S2. The polypropylene fiber, the aramid fiber and the polyolefin composite fiber obtained in step S1 are fully dispersed in water according to a predetermined ratio to obtain a fiber slurry;

[0028] S3. Sheeting the fiber slurry obtained in step S2 into a fiber web, and drying the fiber web;

[0029] S4. The fiber web after drying is subjected to heat pressing treatment to obtain an acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane.

[0030] Through the above method, the synergistic effect between polypropylene fiber, aramid fiber and polyolefin composite fiber can be utilized, so that the prepared non-woven fabric for reverse osmosis nanofiltration membrane has the advantages of excellent acid and alkali resistance, good mechanical properties, smooth surface, high stability, etc.

[0031] Specifically, in step S1, polyethylene masterbatch with a melting point of 125-135°C is preferably used as the skin material, and polypropylene masterbatch with a melting point of 165-170°C is preferably used as the core material; the mass ratio of the skin material to the core material is preferably 45%-50%:50%-55%. In this way, the skin material in the polyolefin composite fiber can play a bonding role by adjusting the temperature of the hot pressing process.

[0032] In step S2, the length of the polypropylene fiber used is preferably 3-6 mm, and the diameter is preferably 5-15 μm; the length of the aramid fiber is preferably 3-5 mm, and the diameter is preferably 10-25 μm; the length of the polyolefin composite fiber is preferably 3-4 mm, and the diameter is preferably 10-20 μm. This arrangement facilitates the full dispersion of the polyolefin composite fiber between the polypropylene fiber and the aramid fiber, and effectively bonds them. In the fiber slurry, the mass ratio of the polypropylene fiber, the polyolefin composite fiber and the aramid fiber is 40%-60%: 20%-40%: 10%-20%, so as to more effectively exert the synergistic effect between the fibers.

[0033] In step S2, by adjusting the amount of water and each fiber, the total mass concentration of each fiber in the fiber slurry can be adjusted to 0.5% to 1% for more effective dispersion. In addition, when the polypropylene fiber, aramid fiber and polyolefin composite fiber are dispersed in water, a dispersant and a defoamer are added to further promote the dispersion of the fibers. Among them, the dispersant is preferably polyethylene oxide, and the amount is about 0.05% of the fiber slurry, and the defoamer is preferably a polyether defoamer, and the amount is preferably about 0.2% of the fiber slurry. In practical applications, the type and amount of the dispersant and defoamer can also be adjusted according to actual conditions.

[0034] In step S3, the temperature of the drying treatment is 120-130°C; in step S4, the hot pressing treatment includes hard calendering treatment and soft calendering treatment performed in sequence; the hot pressing temperature of the hard calendering treatment is 130-160°C, and the temperature of the soft calendering treatment is 145-155°C. In this way, the skin material of the polyolefin composite fiber can begin to soften during the drying process, which plays a preliminary bonding and shaping effect, and then the bonding effect is further improved through the hard calendering process, and the thermal shrinkage of the non-woven fabric is reduced by the interaction between the aramid fiber and the polypropylene fiber. On this basis, the soft calendering treatment is performed, which can further reduce the thermal shrinkage while improving the surface smoothness and air permeability of the non-woven fabric.

[0035] The acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane prepared based on the above method includes polypropylene fiber, aramid fiber and polyolefin composite fiber. It has the advantages of excellent acid and alkali resistance, good mechanical properties, smooth surface, high stability, etc., and can meet the needs of actual production and application.

[0036] The acid and alkali resistant nonwoven fabric for reverse osmosis nanofiltration membrane and the preparation method thereof provided by the present invention are described in detail below in conjunction with specific embodiments.

[0037] Example 1

[0038] This embodiment provides a method for preparing an acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane, comprising the following steps:

[0039] S1. A polyolefin composite fiber with a skin-core structure is prepared by a composite melt spinning method using polyethylene masterbatch with a melting point of about 130°C as a skin material and polypropylene masterbatch with a melting point of about 170°C as a core material. The mass ratio of the skin material to the core material is 45%:55%, and the average diameter of the prepared polyolefin composite fiber is about 5 μm.

[0040] S2. After the polyolefin composite fiber obtained in step S1 is cut to a fiber length of about 1 to 2 mm, it is mixed with a polypropylene fiber of about 3 to 6 mm in length and an average diameter of about 10 μm and an aramid fiber of about 3 to 5 mm in length and an average diameter of about 15 μm, and then dispersed in water, and a dispersant and a defoamer are added to prepare a fiber slurry with a total fiber mass fraction of about 0.5%. Among them, the mass ratio of polypropylene fiber, polyolefin composite fiber and aramid fiber is 40:40:20, the dispersant is polyethylene oxide, and the amount is 0.05% of the fiber slurry, and the defoamer is a polyether defoamer, and the amount is 0.2% of the fiber slurry.

[0041] S3. The fiber slurry obtained in step S2 is made into a fiber web through an inclined mesh headbox, which is then squeezed and dehydrated and then placed in a drying cylinder at 125°C for drying.

[0042] S4. First, a metal roller is used to perform hard calendering treatment on the fiber web after drying, and the hot pressing temperature of the hard calendering treatment is set to 135°C; then a rubber roller is used to perform soft calendering treatment, and the hot pressing temperature of the soft calendering treatment is set to 150°C. After treatment, an acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane is obtained.

[0043] The performance test data of the acid- and alkali-resistant nonwoven fabric for reverse osmosis nanofiltration membrane prepared in this embodiment are shown in Table 1.

[0044] Table 1 Performance parameters of the nonwoven fabric prepared in Example 1

[0045] Test items Test results Width(mm) 1100 Quantitative (g) 76 Thickness(μm) 99 Tensile strength (longitudinal / transverse KN / m) 6.2 / 3.5 Smoothness (front / back) 15 / 10 <![CDATA[Air permeability (cm 3 / cm 2 / s)]]> 2.2 Average pore size (μm) 9.2 Acid resistance (%) 0.2 Alkali resistance (%) 0.4

[0046] Among them, the method for measuring acid resistance is: placing the non-woven fabric in a hydrochloric acid solution with a pH of 3 and in water with a pH of 7, respectively, soaking them under the same external conditions for 24 hours, and testing their tensile strength respectively. The change rate of the tensile strength of the non-woven fabric soaked in the hydrochloric acid solution compared to the tensile strength of the non-woven fabric soaked in water is the acid resistance. Similarly, the method for measuring alkali resistance is: placing the non-woven fabric in a sodium hydroxide solution with a pH of 12 and in water with a pH of 7, respectively, soaking them under the same external conditions for 24 hours, and testing their tensile strength respectively. The change rate of the tensile strength of the non-woven fabric soaked in the sodium hydroxide solution compared to the tensile strength of the non-woven fabric soaked in water is the alkali resistance. The lower the measured values ​​of acid resistance and alkali resistance, the smaller the change in tensile strength after soaking in acid or alkali solution, and the better the acid resistance and alkali resistance.

[0047] It can be seen from the data in Table 1 that the acid- and alkali-resistant nonwoven fabric for reverse osmosis nanofiltration membrane prepared in Example 1 has the advantages of excellent acid and alkali resistance, good mechanical properties, smooth surface, good air permeability, etc.

[0048] Examples 2 to 4 and Comparative Examples 1 to 3

[0049] Examples 2 to 4 and comparative examples 1 to 3 respectively provide a method for preparing an acid- and alkali-resistant nonwoven fabric for reverse osmosis nanofiltration membrane. Compared with Example 1, the only difference is that the mass ratio of each fiber in step S2 is changed, and the remaining steps and parameters are consistent with Example 1, which will not be repeated here. The mass ratios corresponding to each embodiment and comparative example are shown in Table 2.

[0050] Table 2 Mass ratio of each fiber in Examples 2 to 4 and Comparative Examples 1 to 3

[0051] Example / Comparative Example Mass ratio of polypropylene fiber, polyolefin composite fiber and aramid fiber Example 2 50:30:20 Example 3 60:25:15 Example 4 50:40:10 Comparative Example 1 60:40:0 Comparative Example 2 60:35:5 Comparative Example 3 50:20:30

[0052] The properties of the nonwoven fabrics prepared in Examples 2 to 4 and Comparative Examples 1 to 3 were tested, and the results are shown in Table 3.

[0053] Table 3 Performance parameters of nonwoven fabrics prepared in Examples 2 to 4 and Comparative Examples 1 to 3

[0054]

[0055]

[0056] It can be seen from Table 3 that the change in the mass ratio of polypropylene fiber, polyolefin composite fiber and aramid fiber will have a great impact on the performance of non-woven fabrics. On the basis of polypropylene fiber as the main fiber, by introducing 20% ​​to 40% of polyolefin composite fiber, the non-woven fabric can have higher smoothness and air permeability; at the same time, by introducing 10% to 20% of aramid fiber, the non-woven fabric can have better acid and alkali resistance, but too little or too much aramid fiber will have an adverse effect on the performance of the non-woven fabric.

[0057] Examples 5 to 8 and Comparative Examples 4 to 5

[0058] Examples 5 to 8 and Comparative Examples 4 to 5 respectively provide a method for preparing an acid- and alkali-resistant nonwoven fabric for reverse osmosis nanofiltration membrane. Compared with Example 1, the only difference is that the average length and average diameter of each fiber in step S2 are changed, and the remaining steps are consistent with Example 1, which will not be repeated here. The average length and average diameter of the fibers corresponding to each embodiment and comparative example are shown in Table 4.

[0059] Table 4 Length and diameter of each fiber in Examples 5 to 8 and Comparative Examples 4 to 5

[0060]

[0061]

[0062] The properties of the nonwoven fabrics prepared in Examples 5 to 8 and Comparative Examples 4 to 5 were tested, and the results are shown in Table 5.

[0063] Table 5 Performance parameters of nonwoven fabrics prepared in Examples 5 to 8 and Comparative Examples 4 to 5

[0064]

[0065] It can be seen from Table 5 that the average length and average diameter of each fiber mainly affect the strength, smoothness, air permeability and pore size of the non-woven fabric. Among them, the fiber diameter has the greatest influence on the tensile strength of the non-woven fabric, and the fiber length has the second greatest influence on the tensile strength of the non-woven fabric. Within a certain range, the smaller the fiber diameter and the longer the fiber length, the higher the fiber bonding force and the greater the tensile strength.

[0066] Examples 9-10 and Comparative Examples 6-7

[0067] Examples 9-10 and Comparative Examples 6-7 respectively provide a method for preparing an acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane. Compared with Example 1, the only difference is that the drying temperature and hot pressing temperature in steps S3-S4 are changed, and the remaining steps are consistent with Example 1, which will not be repeated here. The temperature parameters corresponding to each embodiment and comparative example are shown in Table 6.

[0068] Table 6 Temperature parameters in Examples 9-10 and Comparative Examples 6-7

[0069]

[0070]

[0071] The properties of the nonwoven fabrics prepared in Examples 9-10 and Comparative Examples 6-7 were tested, and the results are shown in Table 7.

[0072] Table 7 Performance parameters of nonwoven fabrics prepared in Examples 9 to 10 and Comparative Examples 6 to 7

[0073]

[0074] It can be seen from Table 7 that the temperature of drying and hard calendering and soft calendering will affect the performance of non-woven fabrics, mainly affecting the strength, smoothness and air permeability of non-woven fabrics. Relatively high or relatively low temperatures will make the final non-woven fabric difficult to meet application requirements.

[0075] It can be seen from the implementation methods and product performance in the above embodiments and comparative examples that the present invention can make the polyolefin composite fibers evenly distributed between the polypropylene fibers and the aramid fibers have a better bonding effect by regulating the length and ratio of each fiber and adjusting the temperature of the drying and hot pressing process, and fix the polypropylene fibers with aramid fibers to prevent the non-woven fabric from shrinking, thereby improving the structural stability, air permeability and mechanical properties of the non-woven fabric. The acid- and alkali-resistant reverse osmosis nanofiltration membrane non-woven fabric prepared by the method provided by the present invention has the advantages of excellent acid- and alkali resistance, good mechanical properties, smooth surface, good air permeability, etc., and can meet the needs of actual production and application.

[0076] In summary, the present invention provides an acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane and a preparation method thereof, and relates to the technical field of non-woven fabrics for separation membranes. The present invention uses polyethylene masterbatch as the skin layer material and polypropylene masterbatch as the core layer material, and adopts a composite melt spinning method to prepare a polyolefin composite fiber with a skin-core structure; then the polypropylene fiber, aramid fiber and polyolefin composite fiber are fully dispersed in water according to a predetermined ratio, and after being made into a net, dried and hot-pressed, an acid- and alkali-resistant non-woven fabric for reverse osmosis nanofiltration membrane containing polypropylene fiber, aramid fiber and polyolefin composite fiber can be obtained. Through the above method, the present invention can utilize the synergistic effect between the fibers to tightly connect the aramid fiber and the polypropylene fiber through the polyolefin composite fiber, thereby preparing a non-woven fabric for reverse osmosis nanofiltration membrane with excellent acid and alkali resistance, good mechanical properties, smooth surface and good air permeability in a simple and efficient manner to meet the needs of actual production and application.

[0077] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a non-woven fabric for acid- and alkali-resistant reverse osmosis nanofiltration membrane, It is characterized in that The steps include: S1. Using polyethylene masterbatch as the skin material and polypropylene masterbatch as the core material, a polyolefin composite fiber with a skin-core structure was prepared by a composite melt spinning method; S2. The polypropylene fiber, the aramid fiber and the polyolefin composite fiber obtained in step S1 are fully dispersed in water according to a predetermined ratio to obtain a fiber slurry; S3. Sheeting the fiber slurry obtained in step S2 into a fiber web, and drying the fiber web; S4. The fiber web after drying is subjected to heat pressing treatment to obtain an acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane.

2. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S2, in the fiber slurry, the mass ratio of polypropylene fiber, polyolefin composite fiber and aramid fiber is 40% to 60%: 20% to 40%: 10% to 20%.

3. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S2, the length of the polypropylene fiber is 3-6 mm, the length of the aramid fiber is 3-5 mm, and the length of the polyolefin composite fiber is 3-4 mm.

4. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S1, the mass ratio of the skin layer material to the core layer material is 45% to 50%: 50% to 55%.

5. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S1, the melting point of the skin layer material is 125-135°C, and the melting point of the core layer material is 165-170°C.

6. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S3, the temperature of the drying process is 120-130°C.

7. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S4, the hot pressing treatment includes hard calendering treatment and soft calendering treatment performed sequentially; the hot pressing temperature of the hard calendering treatment is 130-160°C, and the temperature of the soft calendering treatment is 145-155°C.

8. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S2, the total mass concentration of each fiber in the fiber slurry is 0.5% to 1%.

9. The method for preparing the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane according to claim 1, Features: In step S2, a dispersant and a defoaming agent are also added to the fiber slurry.

10. A non-woven fabric for acid and alkali resistant reverse osmosis nanofiltration membrane, Features: The acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane is prepared by the preparation method described in any one of claims 1 to 9; the acid-base resistant nonwoven fabric for reverse osmosis nanofiltration membrane comprises polypropylene fiber, aramid fiber and polyolefin composite fiber.

Citation Information

Patent Citations

  • Nonwoven cloth composite nanofiltration membrane and preparation method and application thereof

    CN105498550A

  • Multi-purpose sheath-core composite monofilament as well as production method and application thereof

    CN106048777A

  • Reverse osmosis membrane support for seawater desalination and preparation method

    CN106823838A

  • Polyolefin type eccentric composite fiber and preparation apparatus therefor

    JP1983180614A

  • Pulp formed body and method for producing the same

    JP2005139582A