Packing cup with framework for infinite-grade soluble spears and preparation method of packing cup

By introducing skeletons and multi-stage heating treatment methods into the leather bowl, the existing rubber leather bowls have been solved, and the leather bowl design with higher strength and easy treatment has been achieved, suitable for oil and gas exploration high voltage environment.

CN119021627APending Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310592413.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing rubber bowls have weak pressure bearing capacity and are prone to surface scorching and flow marks, which are difficult to meet the needs of medium and high-pressure environments for oil and natural gas exploration and development.

Method used

采用带骨架的皮碗设计,骨架由可溶镁合金制成,外部包裹橡胶层,骨架设置有底座和承压齿,通过喷砂处理和多阶段加热处理提高结构强度,并在皮碗制备中使用环氧树脂粘结剂和模具加压成型,确保橡胶均匀包裹。

Benefits of technology

It significantly improves the structural strength and pressure bearing capacity of the leather bowl, can withstand pressure difference up to 70MPa, avoids surface scorching and flow mark defects, and facilitates damage or removal of the leather bowl in water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119021627A_ABST
    Figure CN119021627A_ABST
Patent Text Reader

Abstract

The invention discloses a leather cup with a framework for an infinite-grade soluble spear and a preparation method of the leather cup, and belongs to the technical field of oil well operation tools. The leather cup with the framework for the infinite-grade soluble spear comprises the framework and a rubber layer, the rubber layer wraps the framework; the framework is provided with a base; the outer edge of the upper surface of the base extends upwards to form a plurality of pressure-bearing teeth; the included angle between the plane where the pressure-bearing teeth are located and the upper surface of the base is 40-50 degrees. According to the leather cup with the framework, the metal framework is embedded, and the metal framework has a special structural design, so that the structural strength of the leather cup is effectively improved, and the leather cup is suitable for a pressure-bearing environment with higher strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil well operation tools, and in particular relates to a leather cup with a skeleton for an infinite-level soluble dart and a preparation method thereof. Background Art

[0002] The javelin is a tool for opening the sliding sleeve, which is recorded in the literature such as "Application of secondary plugging valve in completion test" and "Technology research and optimization application of ultra-deep high-pressure coiled tubing unblocking in Tarim Oilfield". It is a common tool in the oil field. Figure 4 The structure shown in Mark 3.

[0003] Infinite-stage soluble dart refers to a dart used in an infinite-stage cementing sleeve, which is not limited by the number of stages and is soluble. Infinite-stage cementing sleeves are described in the references "Shi, L., Zhong, XJ, Wu, J., et al., 2014, Research on the Technology of RFID Sliding Sleeve, Applied Mechanics and Materials, 496-500 1552-1555" and "Liu Hailong et al., Field Practice and Applicability Analysis of Infinite-stage Cementing Sleeve Pressure Dividing Technology".

[0004] At present, in devices such as infinite-level soluble darts, a leather cup structure is usually used to meet the pressure requirements.

[0005] A simple rubber cup has low strength and poor pressure resistance. It can generally only withstand a one-way pressure of less than 5 MPa. Moreover, since it is made entirely of rubber and has a soft texture, it will deform during normal storage and transportation. Therefore, the packaging method also needs to have higher requirements.

[0006] At the same time, the existing method for preparing rubber cups usually adopts a vulcanization molding process under a single temperature condition, which will cause defects such as scorching and flow marks on the product surface. Figure 2 shown.

[0007] Therefore, there is an urgent need in this field to develop a leather cup with a new structure that has a stronger pressure-bearing capacity and no scorch or flow marks on the surface. Summary of the invention

[0008] In order to solve the problems of weak pressure bearing capacity, surface scorching and flow marks of conventional leather cups in the prior art in the field, the present invention provides a leather cup with a skeleton for infinite-stage soluble darts and a preparation method thereof. The leather cup part can be used on full-diameter infinite-stage soluble darts for casing cementing and sliding sleeve staged fracturing in oil and gas exploration and development, and has higher structural strength and pressure bearing capacity. The preparation method of the leather cup proposed in the present invention can improve the structural strength of the leather cup under pressure, can withstand higher pressure requirements, increase the scope of use, and facilitate operation when the leather cup needs to be removed or destroyed.

[0009] The technical solution of the present invention is as follows:

[0010] A leather cup with a frame for infinite-level soluble darts, characterized in that it comprises: a frame and a rubber layer; the rubber layer is wrapped around the outside of the frame; the frame is provided with a base; a plurality of pressure-bearing teeth extend upward from the outer edge of the upper surface of the base; the angle between the plane where the pressure-bearing teeth are located and the upper surface of the base is 40°-50°.

[0011] The plane where the pressure-bearing teeth of the leather cup with skeleton are located in the pressure-bearing state is at an angle of 45°-50° with the upper surface of the base;

[0012] Preferably, the plane where the pressure-bearing teeth of the leather cup with skeleton are located in the non-pressure-bearing state forms an angle of 40°-44° with the upper surface of the base, preferably 42°.

[0013] The angle at which the extended lines of two adjacent side edges of two adjacent pressure-bearing teeth intersect is 15°-25°.

[0014] The shape and size of the inner wall of the rubber layer are matched with the shape and size of the outer wall of the frame.

[0015] The skeleton is made of soluble magnesium alloy.

[0016] In some specific embodiments, the soluble magnesium alloy is purchased from Chongqing Yuhua New Material Technology Co., Ltd., with product grade 008 and specification diameter of 100*1000.

[0017] A method for preparing a leather cup with a skeleton for an infinite-level soluble dart, characterized by comprising:

[0018] S1: Make the skeleton;

[0019] S2: frame surface sandblasting;

[0020] S3: Apply adhesive and heat treat at 120°C for 30 min, 150°C for 30 min, and 180°C for 120 min in sequence;

[0021] S4: After the rubber softens, it wraps the surface of the frame and is pressed into shape by a mold so that the leather cup with the frame has a rubber layer;

[0022] The frame is provided with a base; a plurality of pressure-bearing teeth extend upward from the outer edge of the upper surface of the base; the angle between the plane where the pressure-bearing teeth are located and the upper surface of the base is 40°-50°.

[0023] The plane where the pressure-bearing teeth of the leather cup with skeleton are located in the pressure-bearing state is 40-50 degrees with the upper surface of the base;

[0024] Preferably, the plane where the pressure-bearing teeth of the leather cup with skeleton are located in the non-pressure-bearing state is at an angle of 40° to 50° with the upper surface of the base;

[0025] Preferably, the angle at which the extended lines of two adjacent side edges of two adjacent pressure-bearing teeth intersect is 15°-25°;

[0026] Preferably, the shape and size of the inner wall of the rubber layer match the shape and size of the outer wall of the frame;

[0027] Preferably, the skeleton is made of a soluble magnesium alloy.

[0028] During the pressing process, the mold was heated to 120°C for 60 min and 180°C for 120 min; then cooled to below 90°C and heated again to 150°C for 30 min.

[0029] The heating treatment refers to baking;

[0030] Preferably, the rubber softening means: cutting the rubber into strips and baking at 70° C. for 30 minutes;

[0031] Preferably, the strip size is 50 cm, 3-5 mm wide and 2 mm thick.

[0032] The mold was demoulded after cooling to below 60°C.

[0033] On one hand, the present invention provides a leather cup with a skeleton for an infinite-level soluble dart, comprising an internal skeleton and an external rubber wrapping layer.

[0034] The internal skeleton is made of hollow metal hardware.

[0035] Another aspect of the present invention provides a method for preparing a leather cup with a skeleton for infinite-level soluble darts, which is characterized by comprising the steps of:

[0036] The cup product of the present invention is a product used in the process of oil and gas development. The product is assembled on an infinite-level soluble dart and is used to withstand pressure. It can withstand a maximum pressure difference of 70MPa (such as Figure 3As shown), this is the key to unlimited levels (not limited by the number of levels). The leather cup is composed of an internal skeleton and an external rubber wrapping layer. The skeleton is a hollow metal fixture. After the metal fixture is processed, all surfaces of the metal fixture are treated, and rubber is prepared. The rubber strip is taken out of the oven and evenly wrapped on the surface of the skeleton. It is required to be completely wrapped without leakage. The release agent is evenly applied inside the mold, and the rubber-wrapped fixture is placed in the mold. The mold is closed, pressurized to 40 tons, and the mold is heated to 120℃*60min+180℃*120min. The mold is cooled to below 90℃ and heated again to 150℃*30min. Cool the mold to below 60℃ and take out the leather cup.

[0037] Processing metal hardware;

[0038] After the metal fixtures are processed, all surfaces of the metal fixtures are sandblasted (sand grains 40-80 mesh), and then a high-temperature resistant (above 180°C) epoxy resin adhesive is evenly applied on the surface of the frame. The fixtures are then placed in an oven and baked at 120°C for 30 minutes + 150°C for 30 minutes + 180°C for 120 minutes. The oven heating system is then turned off, and the oven door remains closed. The frame is naturally cooled down to below 60°C along with the oven (usually takes 2-3 hours. The purpose of this process is to prevent the adhesive on the surface of the frame from cracking due to a sudden drop in temperature). The fixtures are then removed (do not touch the frame directly with your hands during the removal process. Clean rubber gloves must be used to avoid contaminating the surface of the fixtures).

[0039] Cut the rubber into strips of 50cm in length, 3-5mm in width and 2mm in thickness, and bake them in an oven at 70℃ for 30min (this step softens the rubber to facilitate the later wrapping of the firmware);

[0040] Take the rubber strip out of the oven and wrap it evenly around the surface of the frame, making sure it is completely wrapped without any leaks;

[0041] Apply release agent evenly inside the mold, put the rubber-wrapped hardware into the mold, close the mold, pressurize it to 40 tons, and heat the mold to 120℃*60min+180℃*120min;

[0042] The mold is cooled to below 90°C and then heated again to 150°C*30min;

[0043] Cool the mold to below 60℃ and take out the leather cup.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The leather cup with a frame provided by the present invention has metal fasteners embedded in the rubber, and the frame formed by the metal fasteners has a special structural setting, thereby improving the structural strength of the leather cup and facilitating its application in a higher-intensity pressure-bearing environment.

[0046] (2) In the present invention, metal fasteners are embedded in the rubber, and the metal skeleton is a magnesium alloy that can be dissolved in water. After the work of the leather cup is completed, when the leather cup needs to be destroyed or removed, the leather cup can be placed in water, and the internal metal skeleton will dissolve in the water, forming a hollow state inside the leather cup, and the overall strength of the leather cup will disappear, making it easy to destroy or remove. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. The drawings described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Figure 1 Schematic diagram of the structure of the skeleton and rubber layer of the skeleton leather cup provided for some embodiments of the present invention; the left figure is a schematic diagram of the skeleton structure of the skeleton leather cup, and the right figure is a schematic diagram of the rubber layer structure of the skeleton leather cup.

[0049] Figure 2 A picture of surface scorch and flow marks on a conventional rubber cup provided as background technology for the present invention.

[0050] Figure 3 A diagram showing the pressure difference test results of a leather cup with a skeleton provided in some embodiments of the present invention.

[0051] Figure 4 Schematic diagram of the internal and external structure of the infinite-stage cementing sleeve including the infinite-stage soluble darts.

[0052] The markings in the figure are listed as follows: 1-oil pipe joint, 2-sliding sleeve, 3-dart, 4-leather cup with skeleton, 41-skeleton, 411-base, 412-pressure-bearing tooth, 42-rubber layer. DETAILED DESCRIPTION

[0053] The hydraulic compound hand release device of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0054] The term "spear" herein has the conventional technical meaning known to ordinary technicians in the petroleum field. Figure 4 The structure shown in Mark 3.

[0055] The term "unlimited stage" in this article means that the number of stages of staged fracturing is not limited. The concept of unlimited stage is recorded in the references "Shi, L., Zhong, XJ, Wu, J., et al., 2014, Research on the Technology of RFID Sliding Sleeve, Applied Mechanics and Materials, 496-500 1552-1555" and "Liu Hailong et al., Field Practice and Applicability Analysis of Unlimited Stage Cementing Sliding Sleeve Pressure Dividing Technology". The term unlimited stage has the conventional technical meaning familiar to ordinary technicians in the petroleum field.

[0056] The "infinite-stage soluble dart" in this article refers to a dart used in an infinite-stage cementing sleeve, which is not limited by the number of stages and is soluble. References "Shi, L., Zhong, XJ, Wu, J., et al., 2014, Research on the Technology of RFID Sliding Sleeve, Applied Mechanics and Materials, 496-5001552-1555" and "Liu Hailong et al., Field Practice and Applicability Analysis of Infinite-stage Cementing Sleeve Pressure Dividing Technology" have records about infinite-stage cementing sleeves.

[0057] The "soluble" in "unlimited soluble darts" means that the darts are soluble, and the dissolution principle is that the material of the darts is a soluble magnesium alloy. The soluble magnesium alloy is a commercially available product purchased from Chongqing Yuhua New Materials Technology Co., Ltd., product brand 008, specification diameter 100*1000.

[0058] The first group of embodiments, the present invention with a skeleton leather cup

[0059] This group of embodiments provides a framed leather cup for infinite-level soluble darts. All embodiments of this group have the following common features: Figure 1 As shown, the leather cup 4 with a skeleton includes: a skeleton 41 and a rubber layer 42; the rubber layer 42 is wrapped around the outside of the skeleton 41; the skeleton 41 is provided with a base 411; a plurality of pressure-bearing teeth 412 extend upward from the outer edge of the upper surface of the base 411; the angle between the plane where the pressure-bearing teeth 412 are located and the upper surface of the base 411 is 40°-50°.

[0060] In a specific embodiment, the plane where the pressure-bearing teeth 412 of the leather cup with skeleton 4 are located in the pressure-bearing state is 45-50 degrees with the upper surface of the base 411;

[0061] Preferably, the plane where the pressure-bearing teeth of the leather cup with skeleton are located in the non-pressure-bearing state forms an angle of 40°-44° with the upper surface of the base, preferably 42°.

[0062] In a specific embodiment, the angle at which the extended lines of two adjacent side edges of two adjacent pressure-bearing teeth intersect is 15°-25°.

[0063] In some embodiments, the shape and size of the inner wall of the rubber layer match the shape and size of the outer wall of the frame.

[0064] In a preferred embodiment, the skeleton is made of soluble magnesium alloy.

[0065] In some specific embodiments, the soluble magnesium alloy is purchased from Chongqing Yuhua New Material Technology Co., Ltd., with product grade 008 and specification diameter of 100*1000.

[0066] In a preferred embodiment, the leather cup 4 with a skeleton is a bowl-shaped structure, and the size and shape of the inner space of the bowl-shaped structure are compatible with the shape and size of the outer structure of the infinite-stage soluble dart.

[0067] The second group of embodiments, the preparation method of the leather cup with skeleton of the present invention

[0068] This group of embodiments provides a method for preparing a leather cup with a skeleton for infinite-level soluble darts. All embodiments in this group have the following common features: the method for preparing the leather cup with a skeleton comprises:

[0069] S1: Make the skeleton;

[0070] S2: frame surface sandblasting;

[0071] S3: Apply adhesive and heat treat at 120°C for 30 min, 150°C for 30 min, and 180°C for 120 min in sequence;

[0072] S4: After the rubber softens, it wraps the surface of the frame and is pressed into shape by a mold so that the leather cup with the frame has a rubber layer;

[0073] The frame is provided with a base; a plurality of pressure-bearing teeth extend upward from the outer edge of the upper surface of the base; and the angle between the plane where the pressure-bearing teeth are located and the upper surface of the base is 40°-50°.

[0074] In some embodiments, the plane where the pressure-bearing teeth of the leather cup with skeleton are located in the pressure-bearing state is 45°-50° with the upper surface of the base;

[0075] Preferably, the plane where the pressure-bearing teeth of the leather cup with skeleton are located in the non-pressure-bearing state forms an angle of 40-42° with the upper surface of the base, preferably 42°;

[0076] Preferably, the angle at which the extended lines of the two adjacent side edges of the two adjacent pressure-bearing teeth intersect is 15°-25°;

[0077] Preferably, the shape and size of the inner wall of the rubber layer match the shape and size of the outer wall of the frame;

[0078] Preferably, the skeleton is made of a soluble magnesium alloy.

[0079] In other embodiments, during the compression molding process, the mold is heated to 120°C for 60 min and 180°C for 120 min; then cooled to below 90°C and heated again to 150°C for 30 min.

[0080] In a specific embodiment, the heating treatment refers to baking;

[0081] Preferably, the rubber softening means: cutting the rubber into strips and baking at 70° C. for 30 minutes;

[0082] Preferably, the strip size is 50 cm, 3-5 mm wide and 2 mm thick.

[0083] In a preferred embodiment, the mold is demoulded after cooling to below 60°C.

[0084] The cup consists of an inner frame and an outer rubber wrapping layer.

[0085] In the most specific embodiment of the present invention, a metal skeleton is embedded in the rubber layer, and the metal skeleton is a magnesium alloy that can be dissolved in water. After the work of the leather cup is completed, when the leather cup needs to be destroyed or removed, the leather cup can be placed in water, and the internal metal skeleton will dissolve in the water, and the interior of the leather cup will form a hollow state, and the overall strength of the leather cup will disappear, which is convenient for destruction or removal.

[0086] Experimental example, preparation process and performance test of the leather cup with skeleton of the present invention

[0087] After the metal fixtures are processed, all surfaces of the metal fixtures are sandblasted (sand particles 5-15 mesh), and then a high temperature resistant (above 180°C) epoxy resin adhesive is evenly applied on the surface of the frame, and then the fixtures are placed in an oven and baked at 120°C for 30min + 150°C for 30min + 180°C for 120min. The 120°C, 150°C, and 180°C segmented baking of the present invention can significantly improve the performance of the leather cup, as shown in Table 1 below:

[0088] Table 1

[0089] Baking process 130℃×45min 120℃×30min→150℃×30min→180℃×120min Adhesive strength / MPa 16.82 21.42 Bonding surface description The adhesive layer is torn, and no metal surface is exposed The adhesive layer is torn, and no metal surface is exposed

[0090] Then turn off the oven heating system, keep the oven door closed, and allow the frame to cool naturally along with the oven to below 60°C (usually takes 2-3 hours. The purpose of this process is to prevent the adhesive on the surface of the frame from cracking due to sudden cooling). Remove the fixed parts (do not touch the frame directly with your hands during the removal process. Use clean rubber gloves to avoid contaminating the surface of the fixed parts).

[0091] Cut the rubber into strips of 50cm in length, 3-5mm in width and 2mm in thickness, and put them into an oven and bake at 70℃ for 30min (this step softens the rubber to facilitate the later wrapping of the firmware).

[0092] Take the rubber strip out of the oven and evenly wrap it around the surface of the frame, ensuring that it is completely wrapped without any leaks.

[0093] Apply release agent evenly inside the mold, put the rubber-wrapped hardware into the mold, close the mold, pressurize it to 40 tons, and heat the mold to 120℃*60min+180℃*120min.

[0094] The mold is cooled to below 90°C and then heated again to 150°C*30min.

[0095] Cool the mold to below 60℃ and take out the leather cup.

[0096] Scorch marks, sulfur marks, and splicing marks are two types of defects that occur in the vulcanization process of rubber products, such as Figure 2 As shown. The leather cup made by the present invention will not Figure 2 The surface scorch and sulfur marks are shown in the figure. At the same time, the pressure difference tester tests the pressure difference of the leather cup. Figure 3 shown.

Claims

1. A leather cup with a skeleton for infinite-level soluble darts, characterized in that: include: Skeleton and rubber layer; The rubber layer is wrapped around the outside of the frame; the frame is provided with a base; a plurality of pressure-bearing teeth extend upward from the outer edge of the upper surface of the base; the angle between the plane where the pressure-bearing teeth are located and the upper surface of the base is 40°-50°.

2. A leather cup with a skeleton for infinite-level soluble darts according to claim 1, characterized in that: The plane where the pressure-bearing teeth of the leather cup with skeleton are located in the pressure-bearing state forms an angle of 45°-50° with the upper surface of the base.

3. A leather cup with a skeleton for infinite-level soluble darts according to claim 1 or 2, characterized in that: The angle at which the extended lines of two adjacent side edges of two adjacent pressure-bearing teeth intersect is 15°-25°.

4. A leather cup with a skeleton for infinite-level soluble darts according to claim 1, characterized in that: The shape and size of the inner wall of the rubber layer match the shape and size of the outer wall of the frame.

5. A leather cup with a skeleton for infinite-level soluble darts according to claim 1 or 4, characterized in that: The skeleton is made of soluble magnesium alloy.

6. A method for preparing a leather cup with a skeleton for infinite-level soluble darts, characterized in that: include: S1: Make the skeleton; S2: frame surface sandblasting; S3: Apply adhesive and perform heating treatment at 120°C for 30 min, 150°C for 30 min, and 180°C for 120 min in sequence; S4: After the rubber softens, it wraps the surface of the frame and is pressed into shape by a mold so that the leather cup with the frame has a rubber layer; The frame is provided with a base; a plurality of pressure-bearing teeth extend upward from the outer edge of the upper surface of the base; the angle between the plane where the pressure-bearing teeth are located and the upper surface of the base is 40°-50°.

7. The method for preparing a leather cup with a skeleton for infinite-level soluble darts according to claim 6, characterized in that: The plane where the pressure-bearing teeth of the leather cup with skeleton are located in the pressure-bearing state is 40-50 degrees with the upper surface of the base; and / or, the plane where the pressure-bearing teeth of the leather cup with skeleton are located in the non-pressure-bearing state is at an angle of 40° to 50° with the upper surface of the base; and / or, the angle at which the extended lines of two adjacent side edges of two adjacent pressure-bearing teeth intersect is 15°-25°; and / or, the shape and size of the inner wall of the rubber layer match the shape and size of the outer wall of the frame; And / or, the skeleton is made of a soluble magnesium alloy.

8. The method for preparing a leather cup with a skeleton for infinite-level soluble darts according to claim 6, characterized in that: During the pressing process, the mold was heated to 120°C for 60 min and 180°C for 120 min; then cooled to below 90°C and heated again to 150°C for 30 min.

9. The method for preparing a leather cup with a skeleton for infinite-level soluble darts according to claim 6, characterized in that: The heating treatment refers to baking; And / or, the rubber softening refers to: cutting the rubber into strips and baking at 70° C. for 30 min; And / or, the strip size is 50 cm, 3-5 mm wide and 2 mm thick.

10. A method for preparing a leather cup with a skeleton for infinite-level soluble darts according to claim 6 or 8, characterized in that: The mold was demoulded after cooling to below 60°C.